A yellow jarosite composite material and its preparation method and application in thallium-containing wastewater
By combining chloropotassium iron and sodium alginate-loaded nano zero-valent iron, the problems of low efficiency and high cost in the prior art are solved, and efficient and rapid adsorption and reduction of thallium ion is achieved, which is suitable for A variety of thallium-containing wastewater treatments have strong anti-interference ability.
Patent Information
- Application Number
- CN202411324324.0
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2024-09-23
- Publication Date
- 2024-11-29
- Estimated Expiration
- 2044-09-23
AI Technical Summary
The prior art has low efficiency and high cost in treating industrial heavy metal wastewater. It is not treated with low concentration thallium-containing wastewater, and is easily disturbed by other ions, resulting in thallium ion residues.
Using chloropotassium iron-fenaceous composite material, this material uses electron transfer mechanism and porous structure to achieve efficient adsorption and reduction of thallium ions, enhancing anti-interference ability, and is suitable for A variety of thallium-containing wastewater treatment.
It realizes efficient, rapid and deep removal of thallium ions in thallium-containing wastewater, reduces treatment costs, has a wide range of applications, and maintains a stable removal effect under complex water quality conditions.
Smart Images

Figure SMS_1 
Figure SMS_2
Abstract
Description
Technical Field
[0001] The invention relates to a jarosite composite material and application thereof in treating thallium-containing wastewater, belonging to the technical field of wastewater treatment. Background Art
[0002] Industrial heavy metal wastewater originates from industries such as metal processing, chemical industry, mining, electroplating, battery manufacturing, and semiconductor production, and contains heavy metals such as lead, cadmium, mercury, chromium, arsenic, copper, zinc, nickel, and thallium. Although these elements are widely present in nature, industrial activities have significantly increased their environmental concentrations, posing a major threat to ecosystems and human health. The discharge of heavy metal wastewater can lead to water quality deterioration, the death of aquatic organisms, and the destruction of ecological balance. Long-term exposure to heavy metal-contaminated water will not only accumulate through the food chain, affecting the growth and reproduction of organisms, but may also cause diseases of the human nervous system, kidneys, bones, and blood systems. For example, the toxicity of thallium is second only to methylmercury, and its toxicity to mammals is far greater than other heavy metal inorganic salt compounds such as lead, mercury, cadmium, and antimony. Its main industrial sources include smelters, thermal power plants, and the manufacturing process of thallium-containing materials and pharmaceuticals. Therefore, it is an urgent need to ensure public health and environmental protection to effectively control and treat industrial heavy metal wastewater and adopt advanced treatment technologies such as chemical precipitation, membrane separation, and biological adsorption to reduce heavy metal concentrations to a safe level.
[0003] At present, the content of thallium in industrial heavy metal wastewater is lower than that of other heavy metals, but due to its strong bioaccumulation and toxicity, it poses a serious threat to the environment and human health. At present, the treatment of industrial heavy metal wastewater is to first neutralize the wastewater and precipitate and separate it, and then carry out the thallium removal process. The treatment steps are relatively cumbersome and thallium cannot be removed at the same time. The technical means for treating thallium-containing industrial wastewater mainly focus on chemical precipitation, adsorption, ion exchange and membrane separation. These technologies achieve thallium removal through different mechanisms, including changing the chemical form of thallium, adsorbing thallium by the affinity of adsorbents, selectively capturing thallium ions through ion exchange resins, and blocking thallium ions by membrane technology. These methods have their own characteristics and are suitable for the treatment of thallium-containing wastewater of different concentrations and types. However, they all have a series of common disadvantages, such as large dosage of reagents, high cost, and the generation of a large amount of thallium-containing waste residues. In addition, the treatment depth of low-concentration thallium-containing wastewater is not enough, and it is easy to be interfered by other ions and fail to meet the treatment standards, resulting in residual thallium ions.
[0004] For example, patent CN108793378A discloses a method for removing thallium from wastewater containing thallium tailings. The method removes thallium from wastewater containing thallium tailings by adding ferrous sulfate to the wastewater. + Restore to T1 + Then add reduced iron powder as a reducing agent to reduce the T1 in the wastewater +Sponge thallium reduced to solid can effectively remove thallium from wastewater. Although thallium ions in wastewater can be effectively removed, other wastewater ions that are easily reduced, such as chromium ions, copper ions and mercury ions, exist in wastewater, and thallium ions in wastewater cannot be accurately removed. Another example is patent CN105921763A, a preparation method of sodium alginate / inorganic mineral-co-loaded nano zero-valent iron. This material has high aqueous solution stability, overcomes the shortcomings of nano zero-valent iron and inorganic mineral-co-loaded nano zero-valent iron that are difficult to separate from water, improves the reuse rate of materials, and has a good removal effect on heavy metals in water environments. However, the sodium alginate / inorganic mineral-co-loaded nano zero-valent iron is easily biodegraded in complex wastewater and is unstable, which affects the removal efficiency of heavy metals in wastewater. Summary of the invention
[0005] In view of the defects of thallium removal agents in the prior art, the first object of the present invention is to provide a jarosite composite material. The composite material combines jarosite with sodium alginate-loaded nano zero-valent iron, utilizing the synergistic effect of the two in structure and chemical composition. The composite material can effectively and quickly treat thallium-containing wastewater, has a large adsorption capacity for thallium in thallium-containing wastewater, a fast adsorption rate, and a strong anti-interference ability, and is adaptable to a variety of thallium-containing wastewater.
[0006] The second object of the present invention is to provide a method for preparing a jarosite composite material, which has mild preparation conditions, is easy to operate, is easy to mass produce, and each component is easy to control, thereby ensuring the high-efficiency adsorption performance and stability of the composite material.
[0007] The third object of the present invention is to provide an application of a jarosite composite material, which is used as a thallium removal treatment agent in the treatment of thallium-containing industrial wastewater. The composite material can quickly and efficiently deeply treat thallium in thallium-containing wastewater, has low treatment cost, strong anti-interference ability, and is suitable for the treatment of a variety of thallium-containing wastewater.
[0008] In order to achieve the above technical purpose, the present invention provides a jarosite composite material, which is composed of the following components by weight percentage: 23-55% jarosite, 23-45% sodium alginate-loaded nano zero-valent iron, 15-28% stabilizer, 3-8% binder and 0.5-5% thickener; the sodium alginate-loaded nano zero-valent iron is obtained by adding nano zero-valent iron to a sodium alginate aqueous solution and dispersing it evenly to obtain a mixed solution, and then dripping the mixed solution into a calcium chloride solution for cross-linking reaction, and the loading amount of nano zero-valent iron in the sodium alginate-loaded nano zero-valent iron is 10-20%.
[0009] The jarosite composite material of the present invention is composed of jarosite, sodium alginate loaded nano zero-valent iron, a stabilizer, a binder and a thickener, and its uniqueness lies in the synergistic effect between the components. Jarosite and nano zero-valent iron work synergistically through an electron transfer mechanism, the former provides a large number of adsorption sites, and the latter accelerates the reduction and precipitation of heavy metal ions through its strong reducibility, significantly improving the adsorption efficiency and selectivity of the composite material for thallium ions. Sodium alginate, as a carrier, not only gives the composite material good biocompatibility and stability, but also promotes the uniform dispersion of nano zero-valent iron, and enhances the adsorption capacity and regeneration performance of the material. The addition of a stabilizer further optimizes the chemical stability of the composite material and ensures its efficient adsorption performance under different pH conditions. The binder is a cellulose derivative that can disintegrate in water, which can not only provide bonding performance, but also can quickly disintegrate the effective ingredients in water during wastewater treatment, thereby adsorbing, reducing and precipitating harmful heavy metal ions to improve the removal rate of the composite material.
[0010] As a preferred solution, the calcium chloride solution is a 2-5% calcium chloride saturated boric acid aqueous solution.
[0011] As a preferred solution, the conditions of the cross-linking reaction are: temperature of 25-55° C. and time of 6-24 h.
[0012] As a preferred solution, the binder is one of hydroxypropyl cellulose, sodium carboxymethyl cellulose, cross-linked sodium carboxymethyl cellulose and microcrystalline cellulose. The binder selected in the present invention can enhance the binding force between the jarosite particles and the sodium alginate-loaded nano zero-valent iron, ensuring that the composite material will not be dispersed or lost due to mechanical stirring or water flow during the water treatment process. In addition, the binder selected in the present invention can also be used as a disintegrant, which increases the contact area with the thallium-containing wastewater by promoting the disintegration of the composite material, thereby improving the thallium removal efficiency.
[0013] As a preferred solution, the stabilizer is at least one of potassium salt, calcium salt and magnesium salt; the potassium salt is one of potassium chloride, potassium sulfate and potassium carbonate; the calcium salt is one of calcium chloride, calcium sulfate, calcium nitrate and calcium carbonate; the magnesium salt is one of magnesium chloride, magnesium sulfate, magnesium nitrate and magnesium carbonate.
[0014] As a preferred solution, the thickener is one of polyvinyl alcohol, sodium polyacrylate and polyacrylamide.
[0015] As a preferred solution, the mass ratio of sodium alginate to nano zero-valent iron is 4-9:1.
[0016] The present invention also provides a method for preparing a jarosite composite material, which comprises dispersing sodium alginate loaded nano zero-valent iron into a binder aqueous solution, then sequentially adding ground jarosite and a stabilizer mixture, and finally adding a thickener for spray drying and granulation.
[0017] As a preferred solution, the particle size of the ground jarosite and stabilizer mixture is 2-10 μm. The control of the particle size of the present invention can improve its contact efficiency with pollutants, thereby enhancing adsorption and catalytic performance.
[0018] The invention also provides an application of the jarosite composite material, which is used as a thallium removal treatment agent for the treatment of thallium-containing industrial wastewater.
[0019] As a preferred solution, the parameters of the jarosite composite material for treating thallium-containing industrial wastewater are: time is 10-30 minutes; addition amount is 5-50 mg / L. The present invention uses the jarosite composite material as a thallium removal agent to efficiently treat thallium-containing industrial wastewater, with short treatment time, fast response, high treatment efficiency, and small addition amount, which can ensure high removal rate while reflecting both economic and environmental benefits.
[0020] Compared with the prior art, the technical solution of the present invention brings about the following innovative and beneficial technical effects:
[0021] 1) The composite material provided by the present invention, based on its unique structural and chemical properties, constructs an efficient heavy metal capture mechanism. The structure of jarosite is rich in Fe 3+ / Fe 2+The valence conversion site can accelerate the reduction and precipitation of heavy metal ions through the electron transfer process; and the high activity and high specific surface area of nano zero-valent iron provide a large number of reaction sites, which enhances the adsorption and reduction ability of heavy metals. As a carrier with good biocompatibility, sodium alginate not only provides a stable microenvironment for nano zero-valent iron through the cross-linking of its polysaccharide chain, avoiding the agglomeration of nanoparticles, but also forms hydrogen bonds and coordination bonds with jarosite through its abundant carboxyl and hydroxyl functional groups, thus enhancing the overall stability of the composite material. This synergistic effect enables jarosite to more effectively reduce heavy metal ions to a lower valence state, promoting its precipitation and adsorption on the surface of nano zero-valent iron. At the same time, the porous structure of sodium alginate further increases the specific surface area of the composite material and improves the contact efficiency with heavy metal ions. This synergistic effect in structure and chemical composition characteristics provides a strong scientific basis for the application of composite materials in heavy metal wastewater treatment, and demonstrates its great potential in the field of industrial wastewater treatment. Compared with existing thallium removal materials, the jarosite composite material provided by the present invention has a larger adsorption capacity and can more effectively capture and fix high-concentration thallium ions in wastewater; the adsorption rate is significantly accelerated, shortening the wastewater treatment cycle and improving the treatment efficiency; the material exhibits stronger anti-interference ability and can maintain a stable removal effect even under complex water quality conditions; the active sites are rich, which enhances the material's affinity for heavy metal ions and ensures efficient removal performance.
[0022] 2) The present invention adds a water-soluble adhesive to the composite material, which can disintegrate in time when used, effectively release the active ingredients, accelerate the contact and adsorption process with heavy metal ions, especially thallium ions, and significantly improve the treatment efficiency.
[0023] 3) The preparation process of the present invention is simple and easy to operate, which not only reduces the difficulty of production, but also greatly reduces energy consumption, which is conducive to large-scale industrial production; by precisely controlling the reaction conditions and component ratios, the uniformity and stability of the material are effectively improved, ensuring the reliability and consistency of product performance; the selected disintegrable adhesive is easy to mix evenly during the preparation process, and can be naturally decomposed in the later stage of use to release the active ingredients, without the need for complex post-processing, thereby simplifying the entire wastewater treatment process.
[0024] 4) The composite material provided by the present invention is used for the treatment of thallium-containing industrial wastewater, and can efficiently and accurately capture trace or even trace amounts of thallium ions in the wastewater, ensuring that the effluent quality is far below the emission standards and meeting strict environmental protection requirements; the material has strong anti-interference ability and can maintain stable thallium removal performance even in complex wastewater containing multiple coexisting ions, ensuring that the treatment effect is not affected, and can treat a variety of industrial wastewaters, with a wide range of applications. DETAILED DESCRIPTION
[0025] The technical solution of the present invention will be further described below in conjunction with specific embodiments of the present invention. It should be noted that the described embodiments are only part of the embodiments of the present invention, rather than all of the embodiments; these embodiments are only for a better understanding of the present invention, rather than limiting the scope of protection of the present invention.
[0026] Unless otherwise specified, all reagents and raw materials used in the present invention are commercially available products or products that can be prepared by known methods.
[0027] Embodiment 1:
[0028] The invention discloses a jarosite composite material, which is composed of the following components by weight percentage: 41.32% jarosite, 33.06% sodium alginate loaded nano zero-valent iron, 18.60% potassium chloride, 6.20% hydroxypropyl cellulose and 0.82% polyvinyl alcohol.
[0029] The preparation method of the jarosite composite material of the present invention is as follows:
[0030] Preparation of sodium alginate loaded nano zero-valent iron: Add 24 g of sodium alginate to 1000 ml of deionized water, stir at room temperature with a magnetic stirrer until completely dissolved, add 4 g of nano zero-valent iron powder, and continue stirring for 1 hour to ensure that the iron powder is evenly dispersed in the solution. The sodium alginate solution containing nano zero-valent iron is added dropwise to 1000 ml of saturated boric acid solution containing 2% calcium chloride, and stand at 35°C in the dark for 12 hours to promote the formation and solidification of the gel. The solidified gel is separated by centrifugation and washed several times with anhydrous ethanol. Then, under nitrogen protection, the gel is placed in a vacuum dryer and dried at 40°C for 24 hours to remove moisture and maintain the activity of zero-valent iron, to obtain sodium alginate loaded nano zero-valent iron with a loading of 12%.
[0031] Preparation of yellow potassium iron alum composite material: 15 grams of hydroxypropyl cellulose was added to 1500 milliliters of deionized water, heated to 80 ° C on a magnetic stirrer, and stirred for 30 minutes to form a viscous aqueous solution. Subsequently, 80 grams of sodium alginate loaded nano zero-valent iron powder was slowly added to the hydroxypropyl cellulose aqueous solution at a speed of 1000 rpm using a high-speed stirrer, and continued to stir for 10 minutes to ensure that the nanoparticles were evenly dispersed to form a stable suspension. Next, 100 grams of yellow potassium iron alum powder and 45 grams of potassium chloride were ground and mixed evenly using a grinder in advance to make the average particle size of 8 μm, added to the above suspension, and stirred at a speed of 800 rpm using a high-speed stirrer for 5 minutes to ensure that the mixture was evenly dispersed. After that, 2 grams of polyvinyl alcohol was added to the mixture, and the high-speed stirrer was used to continue stirring at a speed of 500 rpm for 20 minutes to improve the rheological properties of the mixture. The above mixture was transferred to a spray dryer, and the appropriate drying temperature and feed rate were set, and spray drying was performed to obtain 80 mesh uniform composite material particles. After spray drying is completed, the composite material particles are collected using a collecting device, placed in a vacuum desiccator to cool to room temperature, and then sealed for storage.
[0032] Embodiment 2:
[0033] Compared with Example 1, the only difference is the composition and formula of the jarosite composite material, and the other conditions and steps are the same. It is composed of the following components by weight percentage: 49.59% jarosite, 26.86% sodium alginate loaded nano zero-valent iron, 16.53% magnesium chloride, 6.20% hydroxypropyl cellulose, and 0.82% polyvinyl alcohol.
[0034] Embodiment 3:
[0035] Compared with Example 2, the only difference is that the mass ratio of sodium alginate to nano zero-valent iron is 4:1, and the other conditions and steps are the same.
[0036] Comparative Example 1
[0037] Compared with Example 1, the only difference is the formula. This comparative example does not add sodium alginate to load nano zero-valent iron, and the other conditions and steps are the same. The materials of this comparative example are composed of the following components by weight percentage: 74.38% jarosite, 18.60% potassium chloride, 6.20% hydroxypropyl cellulose, and 0.82% polyvinyl alcohol.
[0038] Comparative Example 2
[0039] Compared with Example 1, the only difference is the formula, and the other conditions and steps are the same. The material of this comparative example is composed of the following components by weight percentage: 20.66% jarosite, 53.72% sodium alginate loaded nano zero-valent iron, 18.60% potassium chloride, 6.20% hydroxypropyl cellulose, and 0.82% polyvinyl alcohol.
[0040] Comparative Example 3
[0041] Compared with Example 1, the only difference is that sodium alginate does not load nano zero-valent iron, and physical blending is adopted, and the other conditions and steps are the same. The material of this comparative example is composed of the following components by weight percentage: 41.32% jarosite, 28.51% sodium alginate, 4.55% nano zero-valent iron, 18.60% potassium chloride, 6.20% hydroxypropyl cellulose, and 0.82% polyvinyl alcohol.
[0042] The following thallium removal performance test was performed on the thallium removal agents prepared in Examples 1 to 3 and Comparative Examples 1 to 3. The specific operation was as follows: Under sufficient stirring conditions, 6 mg of jarosite composite material was added to 1000 mL of thallium-containing industrial wastewater with a thallium content of 541 μg / L. After treatment for 20 minutes, the thallium ion concentration in the wastewater was determined by an inductively coupled plasma mass spectrometer. The results are shown in Table 1.
[0043] Table 1 Thallium removal rate test results of thallium removal agents prepared in Examples 1 to 3 and Comparative Examples 1 to 3
[0044]
[0045] As shown in Table 1, the thallium removal agent prepared in Examples 1 to 3 can reach a thallium removal rate of more than 96% in high-concentration thallium-containing wastewater after only 20 minutes of treatment, with significant thallium removal effect and fast thallium removal efficiency. Comparative Example 1 does not add sodium alginate loaded nano zero-valent iron and only uses jarosite to remove thallium. It can be seen that the final liquid wastewater still contains a large amount of thallium ions. Comparative Example 2 reduces the content of jarosite in the thallium removal agent and increases the content of sodium alginate loaded nano zero-valent iron. The thallium removal rate is still low. Comparative Example 3 does not load nano zero-valent iron in sodium alginate, but simply blends. It can be seen from the table that the thallium removal rate is still worse than that of the embodiment. It can be seen from the above that the composite material of the present invention has excellent thallium removal performance in thallium-containing wastewater in terms of component ratio and synergistic effect. The possible reason is that the combination of jarosite and sodium alginate loaded nano zero-valent iron realizes the dual effects of physical adsorption and chemical reduction, and improves the thallium removal efficiency.
[0046] The following thallium removal agents prepared in Examples 1 to 3 and Comparative Examples 1 to 3 were used for the treatment of acidic washing liquid wastewater from a non-ferrous smelter, and the removal rates of various heavy metals and the anti-interference properties were tested. Specifically, 1000 mL of acidic washing liquid wastewater from a non-ferrous smelter was taken, and the contents of lead, chromium, arsenic and thallium ions were measured to be 17.21 mg / L, 2.31 mg / L, 1.35 mg / L, and 0.66 mg / L, respectively. 20 mg of thallium removal agent was directly added, and the mixture was stirred for 30 minutes without stopping, and the solid-liquid was separated. Finally, the concentration of each heavy metal in the final liquid was tested again, and the removal rate of each heavy metal was calculated. The results are shown in Table 2.
[0047] Table 2 Test results of heavy metal removal rate of thallium removal agents prepared in Examples 1 to 3 and Comparative Examples 1 to 3
[0048]
[0049] As can be seen from Table 2, the jarosite composite materials prepared in Examples 1 to 3 can still maintain a very high thallium removal efficiency even in the presence of interference from heavy metal ions such as lead, chromium, and arsenic. This indicates that the jarosite composite material has excellent anti-interference ability when treating wastewater containing multiple heavy metal ions, and the removal of thallium is not significantly affected by other heavy metal ions, while it also has a certain adsorption and removal ability for other heavy metal ions.
[0050] In summary, the jarosite composite material of the present invention realizes the chemical and structural synergy of various raw materials through carefully designed components and preparation processes, which not only improves the adsorption efficiency and selectivity of thallium ions, but also enhances the overall performance of the material, providing a more efficient and environmentally friendly solution for the treatment of thallium-containing industrial wastewater.
[0051] The above embodiments are only for better explanation of the principles and practical applications of the present invention, so that those skilled in the relevant technical field can better understand and utilize the present invention, but they are not intended to limit the patent scope of the present invention. All equivalent changes made using the contents of the present invention are within the patent protection scope of the present invention.
Claims
1. A jarosite composite material, characterized in that: The invention is composed of the following components by weight percentage: 23-55% jarosite, 23-45% sodium alginate loaded nano zero-valent iron, 15-28% stabilizer, 3-8% binder and 0.5-5% thickener; the sodium alginate loaded nano zero-valent iron is prepared by adding nano zero-valent iron into a sodium alginate aqueous solution and dispersing the nano zero-valent iron uniformly to obtain a mixed solution, and then dropping the mixed solution into a calcium chloride solution for cross-linking reaction, wherein the loading amount of nano zero-valent iron in the sodium alginate loaded nano zero-valent iron is 10-20%.
2. The jarosite composite material according to claim 1, characterized in that: The binder is one of hydroxypropyl cellulose, sodium carboxymethyl cellulose, cross-linked sodium carboxymethyl cellulose and microcrystalline cellulose.
3. The jarosite composite material according to claim 2, characterized in that: The stabilizer is at least one of potassium salt, calcium salt and magnesium salt; the potassium salt is one of potassium chloride, potassium sulfate and potassium carbonate; the calcium salt is one of calcium chloride, calcium sulfate, calcium nitrate and calcium carbonate; the magnesium salt is one of magnesium chloride, magnesium sulfate, magnesium nitrate and magnesium carbonate.
4. The jarosite composite material according to claim 1, characterized in that: The thickener is one of polyvinyl alcohol, sodium polyacrylate and polyacrylamide.
5. The jarosite composite material according to claim 1, characterized in that: The mass ratio of the sodium alginate to the nano zero-valent iron is 4-9:
1.
6. The method for preparing a jarosite composite material according to any one of claims 1 to 5, characterized in that: The sodium alginate loaded nano zero-valent iron is dispersed in a binder aqueous solution, and then ground jarosite and a stabilizer mixture are added in sequence, and finally a thickener is added to perform spray drying and granulation to obtain the product.
7. The method for preparing a jarosite composite material according to claim 6, characterized in that: The particle size of the ground jarosite and stabilizer mixture is 2-10 μm.
8. The use of a jarosite composite material according to any one of claims 1 to 5, characterized in that: It is used as a thallium removal agent in the treatment of thallium-containing industrial wastewater.
9. The use of a jarosite composite material according to claim 8, characterized in that: The parameters of the jarosite composite material when used for treating thallium-containing industrial wastewater are: time of 10-30 minutes; and addition amount of 5-50 mg / L.
Citation Information
Patent Citations
Preparation method of sodium alginate / inorganic mineral linked load type nanometer zero-valent iron
CN105921763A
Method for desorbing thallium from thallium-containing tailing pond wastewater
CN108793378A
Precipitating agent for removing thallium from industrial wastewater and method for deeply removing thallium from industrial wastewater
CN108658301A
Preparation and application of manganese carbide cross-linked sodium alginate modified charcoal loaded nZVI
CN113181885A
Modified nano zero-valent iron-bio-based composite functional material as well as preparation method and application thereof