Preparation method and application of uniform carbon-coated lithium iron phosphate

Through graded wet grinding, high-temperature coating machine and graded crushing technology, the deficiencies in rate performance of lithium iron phosphate materials have been solved, the material's efficient conductive network construction and particle grading have been achieved, and the rate and compaction of the material have been significantly improved. density, extending the charging and discharging platform.

CN118851135APending Publication Date: 2024-10-29银贮(阜阳)科技有限公司

Patent Information

Application Number
CN202411336862.1
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-09-25
Publication Date
2024-10-29

AI Technical Summary

Technical Problem

Lithium iron phosphate materials have shortcomings in high-rate performance, such as low lithium ion diffusion rate, low electronic conductivity, and low tap density. Existing technologies cannot fully solve these problems through element doping and carbon coating methods.

Method used

The graded wet grinding technology is used to nanonize the material particles, a high-temperature coating machine is used to achieve uniformity of carbon coating, and the particle gradation and compaction density are improved through graded crushing to form a good conductive network.

Benefits of technology

It significantly improves the rate performance and compaction density of lithium iron phosphate, improves the electronic and ionic conductivity of the material, extends the charge and discharge platform and improves cycle performance.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118851135A_ABST
    Figure CN118851135A_ABST
Patent Text Reader

Abstract

The invention relates to the technical field of lithium batteries, in particular to a preparation method and application of uniform carbon-coated lithium iron phosphate, and the preparation method comprises the following steps: S1, adding iron phosphate, a lithium source, an organic carbon source and a dopant into pure water for graded wet grinding to obtain a uniformly mixed suspension; s2, carrying out spray drying on the obtained suspension to obtain a precursor with uniform particle size; s3, calcining the obtained precursor in an inert gas atmosphere to obtain primary lithium iron phosphate with a uniform phase; and S4, carrying out mixed coating on the obtained primary lithium iron phosphate and a mixed carbon source, and carrying out graded crushing to obtain the uniformly-coated and grain-graded lithium iron phosphate material. According to the preparation method, firstly, a grading wet grinding technology is adopted, so that material particles are nanocrystallized, and the particle size distribution is uniform; secondly, a high-temperature coating machine (VCJ) is used, so that carbon coating is uniform, and the coating thickness is uniform; and finally, a graded crushing mode is adopted, so that the material particles are graded and are tightly stacked.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention relates to the technical field of lithium batteries, and in particular to a preparation method of uniformly carbon-coated lithium iron phosphate and applications thereof. Background Art

[0002] Lithium iron phosphate cathode material is recognized as the safest power battery material. It has become the most promising lithium battery cathode material due to its long charge and discharge platform, stable properties, low price, environmental friendliness and many other advantages. It is widely used in many fields such as portable electronic devices, power batteries and energy storage power stations. However, LFP has disadvantages such as low lithium ion diffusion rate, low electronic conductivity and low tap density, resulting in extremely poor high-rate performance.

[0003] In order to improve the low temperature and rate performance of lithium iron phosphate, the existing technology optimizes the electronic and ionic conductivity by means of element doping modification or carbon coating. For example, the patent with patent number CN 202211649263.6 uses one or more of zirconium, titanium, manganese, magnesium, vanadium and their compounds for doping, and forms crystal defects by doping to improve the ionic conductivity of the material body; the patent with patent number CN 117819509 A uses a porous carbon coating method to inhibit the growth of lithium iron phosphate grains, control the particle size of lithium iron phosphate, and shorten the diffusion path of lithium ions. The above methods only form a conductive network through carbon coating and form crystal defects through doping to improve the ionic and electronic conductivity of the material body, and the improvement of the compaction density and rate performance of the material is not yet ideal. Therefore, it is urgent to construct a new method to solve the above problems. Summary of the invention

[0004] In view of this, the purpose of the present invention is to propose a preparation method and application of uniform carbon-coated lithium iron phosphate. The present invention first adopts a graded wet grinding technology to make the material particles nano-sized and uniformly distributed in particle size, reduce the particle size, and shorten the Li + The diffusion distance is shortened, thereby significantly improving the rate performance of LFP; secondly, a high-temperature coating machine (VCJ) is used to ensure uniform carbon coating and uniform coating thickness, forming a good conductive network between the particles, thereby promoting the transfer rate of electrons; finally, a graded crushing method is adopted to ensure that the material particles are graded and tightly stacked, achieving close stacking of large and small particles, thereby significantly improving the compaction density of LFP.

[0005] Based on the above purpose, the present invention provides a method for preparing uniform carbon-coated lithium iron phosphate, comprising the following steps: S1, adding iron phosphate, lithium source, organic carbon source and dopant into pure water for graded wet grinding to obtain a uniformly mixed suspension; S2, spray drying the obtained suspension to obtain a precursor with uniform particle size; S3, calcining the obtained precursor under an inert gas atmosphere to obtain primary lithium iron phosphate with uniform phase; S4. The obtained primary lithium iron phosphate is mixed and coated with a mixed carbon source, and then graded and crushed to obtain a lithium iron phosphate material with uniform coating and particle size distribution.

[0006] The ratio of iron phosphate and lithium source in S1 is 1-1.05:1 according to the molar ratio of lithium to iron, the molar ratio of iron to phosphorus in iron phosphate is 0.96-1:1, the amount of organic carbon source added is 5-15% of the mass of iron phosphate, and the amount of dopant added is 0.1-0.5% of the mass of iron phosphate. Preferably, the ratio of iron phosphate and lithium source is 1.02-1.04:1 according to the molar ratio of lithium to iron, the molar ratio of iron to phosphorus in iron phosphate is 0.96-0.98:1, the amount of organic carbon source added is 8-12% of the mass of iron phosphate, and the amount of dopant added is 0.1-0.3% of the mass of iron phosphate.

[0007] The lithium source is one or more of lithium phosphate, lithium carbonate, lithium hydroxide, dilithium hydrogen phosphate, and lithium dihydrogen phosphate; the organic carbon source is one or more of ascorbic acid, polyethylene glycol, sucrose, glucose, citric acid, fructose, cellulose, and starch; and the dopant is one or more of titanium oxide, niobium oxide, vanadium oxide, and manganese oxide.

[0008] The graded wet grinding is first wet ball milling and then wet sand milling, wherein the solid content is 20-40%, the ball milling particle size D50 is 1-1.5 μm, and the sand milling particle size D50 is 100-500 nm. Preferably, the solid content is 30-35%, the ball milling particle size D50 is 1-1.2 μm, and the sand milling particle size D50 is 200-400 nm.

[0009] The spray drying in S2 adopts centrifugal or two-fluid spray drying, the inlet temperature of the spray drying is 190-210°C, the outlet temperature is 90-110°C, the feed rate is 20-50mL / min, and the particle size of the spray-dried precursor D50 is 5-20μm. Preferably, the particle size of the spray-dried precursor D50 is 8-15μm.

[0010] The calcination in S3 is carried out at high temperature, and the high temperature calcination procedure is pre-sintering temperature 300-600°C, holding time 2-5h; sintering temperature 600-750°C, holding time 10-15h, wherein the inert atmosphere is N2 or Ar, and the heating rate is 1-10°C / min. Preferably, the pre-sintering temperature is 350-550°C, and the holding time is 3-4h. Preferably, the sintering temperature is 650-750°C, the holding time is 10-15h, and the heating rate is preferably 5-8°C / min.

[0011] The mixed carbon source in S4 is a mixture of an organic carbon source and an inorganic carbon source, wherein the organic carbon source is one or more of glucose, sucrose, polyethylene glycol and citric acid, and the inorganic carbon source is one or more of graphite, carbon nanotubes, graphene and acetylene black, and the amount of the mixed carbon source added is 1-5% of the mass of the primary lithium iron phosphate, and the mixed mass ratio is organic carbon source: inorganic carbon source = 9-1: 1-9. Preferably, the amount of the mixed carbon source added is 3-4% of the mass of the primary lithium iron phosphate, and the mixed mass ratio is 8-2: 2-8 for the organic carbon source: inorganic carbon source.

[0012] In S4, the mixed coating is carried out by a high temperature coating machine, the mixing speed of the high temperature coating machine is 100-500 rpm / min, the heating temperature is 300-700°C, and the mixing time is 1-5h. Preferably, the mixing speed of the high temperature coating machine is 200-400 rpm / min, the heating temperature is 300-600°C, and the mixing time is 2-4h.

[0013] The device for graded pulverization in S4 is a mechanical ultrafine pulverizer or an air flow ultrafine pulverizer, wherein after graded pulverization, the particle size D50 of large-particle lithium iron phosphate is 500-1000 nm and the particle size D50 of small-particle lithium iron phosphate is 50-500 nm, and the mass ratio of large-particle lithium iron phosphate to small-particle lithium iron phosphate is 1-9:9-1. Preferably, the particle size D50 of the granular lithium iron phosphate is 600-800 nm, the particle size D50 of the small-particle lithium iron phosphate is 100-300 nm, and the mass ratio of large-particle lithium iron phosphate to small-particle lithium iron phosphate is preferably 4-6:6-4.

[0014] The present invention also provides a uniform carbon-coated lithium iron phosphate, which is prepared by adopting the preparation method of the uniform carbon-coated lithium iron phosphate.

[0015] The present invention also provides the use of lithium iron phosphate prepared by the preparation method of uniformly carbon-coated lithium iron phosphate in battery positive electrode materials.

[0016] Beneficial effects of the present invention: The present invention adopts graded wet grinding technology to make the slurry mixing more uniform, the particles are nanosized and the particle size distribution is more uniform, and the lithium ion diffusion distance is shortened and the electrolyte infiltration area is increased by reducing the particle size, thereby effectively improving the material's rate performance.

[0017] The present invention adopts a modification method of carbon coating and ion doping, forms a conductive network through carbon coating and forms crystal defects through doping, improves the ionic and electronic conductivity of the material body, and thus effectively improves the rate performance of the material.

[0018] The present invention adopts in-situ doping combining organic and inorganic carbon sources. The atomic-level carbon produced by the decomposition of the organic carbon source can be evenly coated on the surface of the material, inhibiting the growth of the primary particles of lithium iron phosphate. The particle morphology is fuller and the size is more uniform, which is beneficial to the improvement of the cycle performance. In addition, the doping of inorganic carbon source reduces the internal resistance of the material and also greatly improves the conductivity of the material.

[0019] The present invention adopts a graded pulverization method, so that LFP particles with different particle sizes are in close contact with each other, which can not only increase the compaction density of the material, but also improve the rate performance of the material.

[0020] The present invention uses a high-temperature coating machine (VCJ) to ensure uniform carbon coating and uniform coating thickness, forming a good conductive network between particles, thereby promoting the transfer rate of electrons. BRIEF DESCRIPTION OF THE DRAWINGS

[0021] In order to more clearly illustrate the technical solutions in the present invention or the prior art, the drawings required for use in the embodiments or the description of the prior art will be briefly introduced below. Obviously, the drawings in the following description are only for the present invention. For ordinary technicians in this field, other drawings can be obtained based on these drawings without paying creative work.

[0022] Figure 1 The XRD pattern of lithium iron phosphate prepared in Example 1; Figure 2 is the TEM spectrum of lithium iron phosphate prepared in Example 1; Figure 3 It is a comparison chart of the first charge and discharge curves of the lithium iron phosphate prepared in Example 1 and Comparative Example 1. DETAILED DESCRIPTION

[0023] In order to make the objectives, technical solutions and advantages of the present invention more clearly understood, the present invention is further described in detail below in conjunction with specific embodiments.

[0024] It should be noted that, unless otherwise defined, the technical terms or scientific terms used in the present invention should have the common meanings understood by persons having ordinary skills in the field to which the present invention belongs. Example 1

[0025] (1) After lithium carbonate and iron phosphate (iron:phosphorus molar ratio = 0.968:1) are mixed according to a lithium:iron molar ratio of 1.025:1, glucose and titanium dioxide are added at 10% and 0.15% of the mass of the iron phosphate, respectively; pure water is added at a solid content of 35% for graded grinding, first ball milling to a particle size of D50 = 1 μm, and then sand milling to a particle size of D50 = 350 nm to obtain a uniformly mixed suspension; (2) The mixed suspension was centrifugally spray dried, the feed inlet temperature was 200 °C, the discharge port temperature was 100 °C, the feed rate was 30 mL / min, and the dry particle size D50 was controlled to be 15 μm to obtain a precursor with uniform particle size; (3) The dried precursor was heated to 500°C at a rate of 5°C / min and kept at a constant temperature for 4 h in a N2 atmosphere, and then heated to 700°C at a rate of 5°C / min and kept at a constant temperature for 10 h to obtain a calcined gray-black powder, which was then crushed to obtain primary lithium iron phosphate with uniform phase; (4) After adding the primary lithium iron phosphate into the high temperature coating machine (VCJ), a mixed carbon source (glucose: carbon nanotubes = 8:2) was added at 3% of the mass of the primary lithium iron phosphate for mixed coating. The mixing speed was 350 rpm / min, the heating temperature was 500 °C, and the mixing time was 3 h. After the mixed coating was completed, it was subjected to graded crushing to control the large particle size to 600 nm and the small particle size to 200 nm. The mass ratio of large-particle lithium iron phosphate to small-particle lithium iron phosphate was 4:6, and lithium iron phosphate with uniform coating and particle grading was obtained. Example 2

[0026] (1) After lithium carbonate and iron phosphate (iron:phosphorus molar ratio = 0.965:1) are mixed according to a lithium:iron molar ratio of 1.03:1, sucrose and niobium pentoxide are added at 12% and 0.2% of the mass of the iron phosphate, respectively; pure water is added at a solid content of 30% for graded grinding, first ball milling to a particle size of D50 = 1.2 μm, and then sand milling to a particle size of D50 = 300 nm to obtain a mixed suspension; (2) The mixed suspension was centrifugally spray dried at a feed inlet temperature of 210 °C, a discharge outlet temperature of 100 °C, a feed rate of 35 mL / min, and a drying particle size of D50 = 14 μm to obtain a precursor with uniform particle size; (3) heating the dried precursor to 400°C for 6 h at a heating rate of 6°C / min in a N2 atmosphere, and then heating the precursor to 680°C for 12 h at a heating rate of 6°C / min to obtain a calcined gray-black powder, which was then crushed to obtain primary lithium iron phosphate with uniform phase; (4) After adding the primary lithium iron phosphate into the high temperature coating machine (VCJ), a mixed carbon source (sucrose: carbon nanotube = 6:4) was added at 4% of the mass of the primary lithium iron phosphate for mixed coating. The mixing speed was 400 rpm / min, the heating temperature was 600 °C, and the mixing time was 2 h. After the mixed coating was completed, it was subjected to graded crushing to control the large particle size to 500 nm and the small particle size to 300 nm. The mass ratio of large-particle lithium iron phosphate to small-particle lithium iron phosphate was 5:5, and lithium iron phosphate with uniform coating and particle grading was obtained. Example 3

[0027] (1) Lithium carbonate and iron phosphate (iron:phosphorus molar ratio = 0.971:1) were mixed according to a lithium:iron molar ratio of 1.025:1, and glucose and niobium pentoxide were added at 8% and 0.1% of the mass of the iron phosphate, respectively; pure water was added at a solid content of 32% for graded grinding, first ball milling to a particle size of D50 = 1 μm, and then sand milling to a particle size of D50 = 200 nm to obtain a uniformly mixed suspension; (2) The mixed suspension was centrifugally spray dried, the feed inlet temperature was 200 °C, the discharge port temperature was 100 °C, the feed rate was 40 mL / min, and the dry particle size D50 was controlled to be 12 μm to obtain a precursor with uniform particle size; (3) heating the dried precursor to 550°C at a rate of 6°C / min and maintaining the temperature for 2 h in a N2 atmosphere, and then heating the precursor to 720°C at a rate of 6°C / min and maintaining the temperature for 8 h to obtain a calcined gray-black powder, which was then crushed to obtain primary lithium iron phosphate with uniform phase; (4) After adding the primary lithium iron phosphate into the high temperature coating machine (VCJ), a mixed carbon source (glucose: graphite = 7:3) was added at 4% of the mass of the primary lithium iron phosphate for mixed coating. The mixing speed was 400 rpm / min, the heating temperature was 550 °C, and the mixing time was 3 h. After the mixed coating was completed, it was subjected to graded crushing to control the large particle size to 600 nm and the small particle size to 300 nm. The mass ratio of large-particle lithium iron phosphate to small-particle lithium iron phosphate was 6:4, and lithium iron phosphate with uniform coating and particle grading was obtained. Example 4

[0028] (1) After lithium carbonate and iron phosphate (iron:phosphorus molar ratio = 0.985:1) are mixed according to a lithium:iron molar ratio of 1.03:1, sucrose and titanium dioxide are added at 10% and 0.2% of the mass of the iron phosphate, respectively; pure water is added at a solid content of 35% for graded grinding, first ball milling to a particle size of D50 = 1.5 μm, and then sand milling to a particle size of D50 = 250 nm to obtain a mixed suspension; (2) The mixed suspension was centrifugally spray dried at a feed inlet temperature of 210 °C, a discharge outlet temperature of 110 °C, a feed rate of 25 mL / min, and a drying particle size of D50 of 15 μm to obtain a precursor with uniform particle size; (3) The dried precursor was heated to 500°C at a rate of 8°C / min and kept at a constant temperature for 5 h in a N2 atmosphere, and then heated to 700°C at a rate of 8°C / min and kept at a constant temperature for 12 h to obtain a calcined gray-black powder, which was then crushed to obtain primary lithium iron phosphate with uniform phase; (4) After adding the primary lithium iron phosphate into the high temperature coating machine (VCJ), a mixed carbon source (sucrose: graphite = 8:2) was added at 3.5% of the mass of the primary lithium iron phosphate for mixed coating. The mixing speed was 400 rpm / min, the heating temperature was 600 °C, and the mixing time was 4 h. After the mixed coating was completed, it was subjected to graded crushing to control the large particle size to 500 nm and the small particle size to 200 nm. The mass ratio of large-particle lithium iron phosphate to small-particle lithium iron phosphate was 9:2, and lithium iron phosphate with uniform coating and particle grading was obtained.

[0029] Comparative Example 1 (1), (2), and (3) are the same as in Example 1; (4) The 3% mixed carbon source (molar ratio of glucose: carbon nanotubes = 8:2) was replaced with 3% single carbon source glucose, while other conditions remained unchanged.

[0030] Comparative Example 2 (1), (2), and (3) are the same as in Example 1; (4) The 3% mixed carbon source (molar ratio of glucose: carbon nanotubes = 8:2) was replaced with 3% single carbon source carbon nanotubes, while other conditions remained unchanged.

[0031] Comparative Example 3 (1), (2), and (3) are the same as in Example 1; (4) Do not use a high temperature coating machine (VCJ) for mixed coating.

[0032] Figure 1 It is the XRD spectrum of the lithium iron phosphate prepared in Example 1. As can be seen from the figure, the XRD spectrum of Example 1 is consistent with the standard PDF card, indicating that the lithium iron phosphate prepared by the inventive method is pure phase and free of impurities; Figure 2 This is a TEM spectrum of the lithium iron phosphate prepared in Example 1. It can be seen from the figure that the lithium iron phosphate prepared in Example 1 has a uniform carbon coating with a moderate thickness; Figure 3 It is a comparison chart of the first charge and discharge curves of the lithium iron phosphate prepared in Example 1 and Comparative Example 1. It can be seen from the figure that Example 1 has a longer charge and discharge platform and a higher specific capacity than Comparative Example 1, indicating that the lithium iron phosphate prepared by the inventive method has the potential performance of high capacity and high rate.

[0033] The lithium iron phosphate positive electrode material prepared in Examples 1-4 and Comparative Examples 1-3 was dispersed in NMP with Super-P and PVDF in a mass ratio of 8:1:1. After uniform dispersion, it was coated on aluminum foil and vacuum dried to obtain a positive electrode plate. The electrolyte was 1 mol / L LiPF6, wherein the solvent volume ratio was EC:DMC:EMC=1:1:1 (volume ratio), the diaphragm was a polypropylene film, and the metal lithium sheet was the negative electrode, which were assembled together into a button half-cell. The test voltage range was 2.0 V to 3.75 V. It was charged to 3.75 V in a constant current and constant voltage charging mode, and discharged to 2.0 V in a constant current discharge mode. The charge and discharge current was 0.2C, 0.5C, and 1C for 3 cycles respectively; then the charge and discharge current was 3C, and the cycle was 500 cycles, and the cut-off voltage condition was the same as 0.2C. The test results are shown in Table 1 below:

[0034] From the data in the above table, it can be seen that the specific capacity of the lithium iron phosphate prepared by the method of the present invention is significantly higher than that of the lithium iron phosphate of the comparative example, and the rate performance is also significantly better than that of the comparative example. The 0.2C specific capacity of the lithium iron phosphate of the present invention can reach 159.6 mAh / g, and the capacity retention rate is as high as 98.7% after 500 cycles at 3C.

[0035] Those skilled in the art should understand that the discussion of any of the above embodiments is only exemplary and is not intended to imply that the scope of the present invention is limited to these examples; under the concept of the present invention, the technical features in the above embodiments or different embodiments can also be combined, the steps can be implemented in any order, and there are many other changes in different aspects of the present invention as described above, which are not provided in detail for the sake of simplicity. Any omissions, modifications, equivalent substitutions, improvements, etc. made within the spirit and principles of the present invention should be included in the scope of protection of the present invention.

Claims

1. A method for preparing uniform carbon-coated lithium iron phosphate, characterized in that: The steps include: S1, adding iron phosphate, lithium source, organic carbon source and dopant into pure water for graded wet grinding to obtain a uniformly mixed suspension; S2, spray drying the obtained suspension to obtain a precursor with uniform particle size; S3, calcining the obtained precursor under an inert gas atmosphere to obtain primary lithium iron phosphate with uniform phase; S4. The obtained primary lithium iron phosphate is mixed and coated with a mixed carbon source, and then graded and crushed to obtain a lithium iron phosphate material with uniform coating and particle size distribution.

2. The method for preparing uniform carbon-coated lithium iron phosphate according to claim 1, characterized in that: The ratio of iron phosphate and lithium source in S1 is 1-1.05:1 according to the molar ratio of lithium to iron, the molar ratio of iron to phosphorus in iron phosphate is 0.96-1:1, the added amount of organic carbon source is 5-15% of the mass of iron phosphate, and the added amount of dopant is 0.1-0.5% of the mass of iron phosphate.

3. The method for preparing uniform carbon-coated lithium iron phosphate according to claim 1, characterized in that: The lithium source is one or more of lithium phosphate, lithium carbonate, lithium hydroxide, dilithium hydrogen phosphate, and lithium dihydrogen phosphate; the organic carbon source is one or more of ascorbic acid, polyethylene glycol, sucrose, glucose, citric acid, fructose, cellulose, and starch; and the dopant is one or more of titanium oxide, niobium oxide, vanadium oxide, and manganese oxide.

4. The method for preparing uniform carbon-coated lithium iron phosphate according to claim 1, characterized in that: The graded wet grinding is first wet ball milling and then wet sand milling, wherein the solid content is 20-40%, the ball milling particle size D50 is 1-1.5 μm, and the sand milling particle size D50 is 100-500 nm.

5. The method for preparing uniform carbon-coated lithium iron phosphate according to claim 1, characterized in that: The spray drying in S2 adopts centrifugal or two-fluid spray drying, the inlet temperature of the spray drying is 190-210°C, the outlet temperature is 90-110°C, the feed rate is 20-50mL / min, and the particle size of the precursor in the spray drying is D50=5-20μm.

6. The method for preparing uniform carbon-coated lithium iron phosphate according to claim 1, characterized in that: The calcination in S3 is carried out at high temperature, and the high temperature calcination procedure is as follows: pre-sintering temperature 300-600°C, holding time 2-5h; sintering temperature 600-750°C, holding time 10-15h, wherein the inert atmosphere is N2 or Ar, and the heating rate is 1-10°C / min.

7. The method for preparing uniform carbon-coated lithium iron phosphate according to claim 1, characterized in that: The mixed carbon source in S4 is a mixture of an organic carbon source and an inorganic carbon source, wherein the organic carbon source is one or more of glucose, sucrose, polyethylene glycol and citric acid, and the inorganic carbon source is one or more of graphite, carbon nanotubes, graphene and acetylene black. The added amount of the mixed carbon source is 1-5% of the mass of the primary lithium iron phosphate, and the mixed mass ratio is organic carbon source: inorganic carbon source = 9-1:1-9.

8. The method for preparing uniform carbon-coated lithium iron phosphate according to claim 1, characterized in that: The mixed coating in S4 is carried out by a high temperature coating machine, the mixing speed of the high temperature coating machine is 100-500rpm / min, the heating temperature is 300-700℃, and the mixing time is 1-5h.

9. The method for preparing uniform carbon-coated lithium iron phosphate according to claim 1, characterized in that: The device for graded pulverization in S4 is a mechanical ultrafine pulverizer or an air flow ultrafine pulverizer, wherein after graded pulverization, the particle size of large-particle lithium iron phosphate is D50=500-1000nm and the particle size of small-particle lithium iron phosphate is D50=50-500 nm, and the mass ratio of large-particle lithium iron phosphate to small-particle lithium iron phosphate is 1-9:9-1.

10. Use of lithium iron phosphate prepared by the method for preparing uniformly carbon-coated lithium iron phosphate according to any one of claims 1 to 9 in battery positive electrode materials.

Citation Information

Patent Citations

  • Positive electrode material lithium iron phosphate and preparation method thereof

    CN109665508A

  • Preparation method of high-capacity lithium-ion battery cathode material lithium iron phosphate

    CN111313010A

  • Preparation method of all-carbon-layer-coated lithium iron phosphate

    CN113540461A

  • Preparation method of carbon and lithium phosphate dual-coated lithium manganese iron phosphate material

    CN116230932A

  • Preparation method of low-cost high-capacity spherical lithium iron phosphate

    CN116639673A

Cited By

  • Preparation method and application of modified carbon-coated lithium iron phosphate positive electrode material

    CN119059508A

  • Preparation method and application of modified carbon-coated lithium iron phosphate positive electrode material

    CN119059508B

  • Preparation method of low-temperature-resistant lithium ion energy storage battery and prepared battery

    CN119725761A

  • Preparation method of low-temperature-resistant lithium ion energy storage battery and battery prepared thereby

    CN119725761B

  • Method for preparing lithium iron phosphate positive electrode material based on secondary sintering

    CN120736502A