High-gloss low-warpage polyphthalamide material and preparation method thereof
By coating rutile titanium dioxide with cerium oxide, aluminum oxide and polyol, the problems of yellowing, fading and powdering of polyphthalamide materials under UV irradiation are solved, and the weather resistance and durability of the material are improved. Mechanical properties extend service life.
Patent Information
- Application Number
- CN202411082848.3
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-08-08
- Publication Date
- 2024-10-29
- Estimated Expiration
- Not applicable · inactive patent
AI Technical Summary
Existing high-gloss polyphthalamide materials are prone to yellowing, fading, and powdering under UV irradiation, which affects their service life.
Cerium oxide, alumina and polyol are used to collaboratively coat rutile titanium dioxide to form a modified coated titanium dioxide mixed with polyphthalamide to improve the mechanical properties of the material and reduce yellowing, fading and powdering. Phenomenon.
It effectively improves the weather resistance and mechanical properties of polyphthalamide materials, reduces the occurrence of yellowing, fading, and powdering, and improves the gloss and service life of the material.
Smart Images

Figure BDA0004984278210000201
Abstract
Description
Technical Field
[0001] The invention relates to the technical field of semi-aromatic nylon, in particular to a high-gloss and low-warping polyphthalamide material and a preparation method thereof. Background Art
[0002] Polyphthalamide (PPA) is a semi-aromatic polyamide and a high-temperature nylon. It uses isophthalic acid or terephthalic acid as the main synthetic raw material and is a semi-crystalline thermoplastic functional material. PPA is currently the most commercially valuable semi-aromatic polyamide. The successful production of high-temperature resistant PPA supplements the original differences between engineering plastics and special polymers in terms of cost performance and function. Compared with some fully aromatic polyamides, the process of PPA is relatively simple, and it is easier to blow mold, injection mold and extrusion mold. In addition, the mechanical properties, thermal conductivity, heat resistance and chemical corrosion resistance of PPA are superior to those of aliphatic polyamides, and it has good performance in heat, electricity, physics and chemical resistance. This makes PPA composite materials have broad application prospects in the fields of electronics, electrical engineering, mechanical engineering, etc.
[0003] In order to obtain high-gloss PPA materials in the prior art, PPA is usually mixed with titanium dioxide. Titanium dioxide has a very high refractive index, which means it can scatter and reflect light more effectively, thereby improving the whiteness and gloss of the material. However, titanium dioxide monomer is composed of two TiO 2 Unit composition, its surface has lattice defects. Under 375nm ultraviolet light, the electrons on the surface of titanium dioxide will jump, causing the oxygen atoms on its lattice to lose two electrons, forming new ecological oxygen. New ecological oxygen has strong oxidizing properties, causing the organic matter around titanium dioxide to be oxidized, causing physical and chemical changes in organic coatings, such as yellowing, fading, and powdering, which affects the service life of PPA materials. Summary of the invention
[0004] The object of the present invention is to provide a high-gloss, low-warping polyphthalamide material and a preparation method thereof. The present invention obtains a modified coated titanium dioxide by sequentially coating rutile titanium dioxide with cerium oxide, aluminum oxide and polyol. After mixing with polyphthalamide, the modified coated titanium dioxide not only improves the mechanical properties of the polyphthalamide, but also effectively reduces the occurrence of yellowing, fading, powdering and the like.
[0005] In order to achieve the above object, the present invention adopts the following technical solutions:
[0006] The present invention provides a high-gloss, low-warping polyphthalamide material, which comprises the following components by mass percentage:
[0007] Polyphthalamide 40-66%, modified coated titanium dioxide 30-56%, compatibilizer 0.1-2%, antioxidant 0.2-0.6%, lubricant 0.2-0.4% and nucleating agent 0.3-1%.
[0008] Further, on the basis of the above technical solution of the present invention, the modified coated titanium dioxide is rutile titanium dioxide synergistically coated with cerium oxide, aluminum oxide and polyol;
[0009] And / or, the particle size of the modified coated titanium dioxide is 50-70 mesh.
[0010] Further, based on the above technical solution of the present invention, the preparation method of the modified coated titanium dioxide comprises the following steps:
[0011] S1: ultrasonically dispersing the rutile titanium dioxide slurry and sodium hexametaphosphate to obtain a dispersion;
[0012] S2: heating the dispersion, adding cerium nitrate solution and sodium hydroxide solution to the dispersion, and after the titration, performing a first aging to obtain a cerium oxide coated rutile titanium dioxide slurry;
[0013] S3: adding a sodium aluminate solution dropwise to the rutile titanium dioxide slurry coated with cerium oxide, and performing a second aging after the titration is completed to obtain a rutile titanium dioxide slurry coated with cerium oxide and aluminum oxide;
[0014] S4: adding a polyol solution and a dilute sulfuric acid solution to the rutile titanium dioxide slurry coated with cerium oxide and aluminum oxide, and performing a third aging after the titration is completed to obtain a rutile titanium dioxide slurry coated with cerium oxide, aluminum oxide and a polyol;
[0015] S5: filtering the cerium oxide, aluminum oxide and polyol coated rutile titanium dioxide slurry for multiple times, and then drying and grinding the obtained filter cake to obtain modified coated titanium dioxide.
[0016] Further, based on the above technical solution of the present invention, in step S1, the concentration of the rutile titanium dioxide slurry is 280-320 g / L, preferably 300 g / L;
[0017] And / or, the mass ratio of the rutile titanium dioxide slurry to the sodium hexametaphosphate is (10-15):1;
[0018] And / or, the ultrasonic dispersion time is 30-45 min.
[0019] Further, based on the above technical solution of the present invention, in step S2, the heating conditions include:
[0020] Heat in a water bath to 50-90°C;
[0021] and / or, the concentration of the cerium nitrate solution is 90-110 g / L, preferably 100 g / L;
[0022] Preferably, the volume of the cerium nitrate solution added dropwise is 20-40 mL, preferably 30 mL;
[0023] And / or, the concentration of the sodium hydroxide solution is 250-300 g / L, preferably 280 g / L;
[0024] Preferably, the purpose of adding the sodium hydroxide solution is to maintain the pH value of the dispersion at 9-10;
[0025] And / or, the titration speed is 4-5 mL / min;
[0026] And / or, the conditions of the first aging include:
[0027] The temperature is 50-90°C, the pH is 9-10, and the time is 1.5-2h.
[0028] Further, based on the above technical solution of the present invention, in step S3, the concentration of the sodium aluminate solution is 90-110 g / L, preferably 100 g / L;
[0029] Preferably, the volume of the sodium aluminate solution added dropwise is 20-40 mL, preferably 30 mL;
[0030] And / or, the titration speed is 4-5 mL / min;
[0031] And / or, the conditions for the second aging include:
[0032] The temperature is 50-90°C, the pH is 9-10, and the time is 1.5-2h.
[0033] Further, based on the above technical solution of the present invention, in step S4, the concentration of the polyol solution is 90-110 g / L, preferably 100 g / L;
[0034] Preferably, the volume of the polyol solution added dropwise is 20-40 mL, preferably 30 mL;
[0035] Preferably, the polyol includes one or more of neopentyl glycol, trimethylolpropane or trimethylolethane;
[0036] and / or, the concentration of the dilute sulfuric acid solution is 150-200 g / L, preferably 190 g / L;
[0037] Preferably, the purpose of adding the dilute sulfuric acid solution is to maintain the pH value during the third aging process at 4-6;
[0038] And / or, the conditions for the third aging include:
[0039] The temperature is 50-90°C, the pH is 4-6, and the time is 1.5-2h;
[0040] And / or, the titration speed is 4-5 mL / min.
[0041] Further, on the basis of the above technical solution of the present invention, in step S5, the filtration comprises: using 50-60° C. water to filter the cerium oxide, aluminum oxide and polyol-coated rutile titanium dioxide slurry for multiple times until no sulfate is found in the filtrate using a 10% BaCl2 solution to obtain a filter cake;
[0042] And / or, the drying comprises:
[0043] The filter cake was placed in a drying oven at 100-130° C. for 10-12 h.
[0044] Further, on the basis of the above technical solution of the present invention, the compatibilizer is a polymer containing maleic anhydride grafts;
[0045] Preferably, the polymer containing maleic anhydride grafts includes one or more of maleic anhydride grafted polyolefins, maleic anhydride grafted polyesters, maleic anhydride grafted polyethers, and maleic anhydride grafted polyamides;
[0046] And / or, the antioxidant is a composite antioxidant;
[0047] Preferably, the composite antioxidant includes one or more of KBG779 and H3373;
[0048] And / or, the lubricant is one or more of paraffin wax, polyethylene wax, polypropylene wax, polysiloxane, and silicone powder;
[0049] And / or, the nucleating agent includes one or more of sodium laurate, sodium stearate, sodium oleate, and sodium myristic acid.
[0050] The present invention also provides a method for preparing the above-mentioned high-gloss and low-warping polyphthalamide material, comprising the following steps:
[0051] (1) drying the raw materials;
[0052] (2) placing the dried raw materials in a blender and mixing them evenly;
[0053] (3) melt-blending the uniformly mixed materials in a twin-screw extruder and extruding them into granules;
[0054] Among them, the setting conditions of the twin-screw extruder are: zone 1 temperature 250-270°C, zone 2 temperature 260-280°C, zone 3 temperature 270-290°C, zone 4 temperature 280-300°C, zone 5 temperature 290-310°C, and head temperature 300-320°C; the screw speed is controlled at 220-350r / min, the mixed material conveying time in the screw is 3-5min, and the pressure is 12-20Pa.
[0055] The present invention provides a high-gloss, low-warping polyphthalamide material and a preparation method thereof, and the beneficial effects are as follows:
[0056] 1. The present invention first uses cerium oxide to coat rutile titanium dioxide because cerium oxide has good ultraviolet shielding ability and will not affect the refractive index of rutile titanium dioxide. It can also serve as a base coating film to block and cover the lattice defects of rutile titanium dioxide. Furthermore, the different electron hybrid orbits of transition metal cerium can form new unsaturated electron orbits on the surface of rutile titanium dioxide, which can capture free active electrons. The free active electrons can combine with the holes of rutile titanium dioxide to block the generation of active free radicals, thereby effectively improving the weather resistance of rutile titanium dioxide and effectively reducing the occurrence of yellowing, fading, powdering and the like.
[0057] 2. The present invention uses aluminum oxide to perform a second coating on the cerium oxide-coated rutile titanium dioxide because the reflection wavelength range of aluminum oxide is wider than that of titanium dioxide, which can effectively improve the light refractive index of titanium dioxide, reflect more ultraviolet rays, and improve the weather resistance of titanium dioxide. During the coating process, aluminum oxide covers the surface of the titanium dioxide particles to form a continuous coating layer. The coating layer significantly increases the hydroxyl content on the surface of the titanium dioxide particles. The increase in hydroxyl groups increases the hydrophilicity and surface activity of the titanium dioxide particles, which is beneficial to chemical bonds such as hydrogen bonds. The hydroxyl groups can also interact with the polyphthalamide molecular chain by physical adsorption and entanglement, thereby forming a strong interface interaction with the PPA material, thereby improving the bonding strength between the titanium dioxide and the PPA material, thereby improving the mechanical strength of the PPA material and reducing the warping of the PPA material.
[0058] 3. The present invention adopts polyol to coat the rutile titanium dioxide coated with cerium oxide and aluminum oxide for the third time. The polyol molecules form hydrogen bonds or van der Waals forces with the hydroxyl groups on the surface of the rutile titanium dioxide through their hydrophilic hydroxyl groups, thereby being adsorbed on the particle surface; and in a weakly acidic environment, some hydroxyl groups of the polyol molecules lose protons to form negatively charged oxygen atoms, which are more likely to undergo condensation reactions with the hydroxyl groups on the surface of the rutile titanium dioxide to form organic functional groups, thereby preventing the rutile titanium dioxide from agglomerating.
[0059] 4. The present invention adopts a composite antioxidant containing hindered phenols and phosphites. This structure can terminate free radicals and inhibit the decomposition of hydroperoxides, effectively prevent the thermal oxidation reaction of polyphthalamide at high temperature, and effectively improve the heat resistance, light resistance and oxygen resistance of polyphthalamide, thereby preventing aging and yellowing of the composite material during processing and use.
[0060] 5. The high-gloss, low-warping polyphthalamide material provided by the present invention has a tensile strength of 130-160 MPa, a flexural strength of 242-280 MPa, a warping degree of 2.8-3.0%, a blue-white luminosity of 94.22-97.20, and a YI value of 9.46-10.03. DETAILED DESCRIPTION
[0061] In order to make the purpose, technical scheme and advantages of the present invention clearer, the technical scheme in the embodiment of the present invention will be clearly and completely described below in conjunction with the embodiments of the present invention. It should be understood by those skilled in the art that the embodiments are only to help understand the present invention and should not be regarded as specific limitations of the present invention. Based on the embodiments in the present invention, all other embodiments obtained by ordinary technicians in the field without making creative work are within the scope of protection of the present invention. The process parameters of the following embodiments that do not specify specific conditions are usually based on conventional conditions.
[0062] The endpoints and any values of the ranges disclosed in the present invention are not limited to the precise ranges or values, and these ranges or values should be understood to include values close to these ranges or values. For numerical ranges, the endpoint values of each range, the endpoint values of each range and the individual point values, and the individual point values can be combined with each other to obtain one or more new numerical ranges, which should be regarded as specifically disclosed in the present invention.
[0063] According to a first aspect of the present invention, there is provided a high-gloss, low-warpage polyphthalamide material, comprising the following components by mass percentage:
[0064] Polyphthalamide 40-66% (such as 45%, 50%, 55%, 60%, etc.), modified coated titanium dioxide 30-56% (such as 35%, 40%, 45%, 50%, etc.), compatibilizer 0.1-2%, antioxidant 0.2-0.6%, lubricant 0.2-0.4% and nucleating agent 0.3-1%.
[0065] As an optional embodiment of the present invention, the modified coated titanium dioxide is rutile titanium dioxide synergistically coated with cerium oxide, aluminum oxide and polyol;
[0066] And / or, the particle size of the modified coated titanium dioxide after grinding is 50-70 mesh (such as 55 mesh, 60 mesh, 65 mesh, etc.).
[0067] As an optional embodiment of the present invention, the method for preparing the modified coated titanium dioxide comprises the following steps:
[0068] S1: ultrasonically dispersing the rutile titanium dioxide slurry and sodium hexametaphosphate to obtain a dispersion;
[0069] S2: heating the dispersion, adding cerium nitrate solution and sodium hydroxide solution to the dispersion, and after the titration, performing a first aging to obtain a cerium oxide coated rutile titanium dioxide slurry;
[0070] S3: adding a sodium aluminate solution dropwise to the rutile titanium dioxide slurry coated with cerium oxide, and performing a second aging after the titration is completed to obtain a rutile titanium dioxide slurry coated with cerium oxide and aluminum oxide;
[0071] S4: adding a polyol solution and a dilute sulfuric acid solution to the rutile titanium dioxide slurry coated with cerium oxide and aluminum oxide, and performing a third aging after the titration is completed to obtain a rutile titanium dioxide slurry coated with cerium oxide, aluminum oxide and a polyol;
[0072] S5: filtering the cerium oxide, aluminum oxide and polyol coated rutile titanium dioxide slurry for multiple times, and then drying and grinding the obtained filter cake to obtain modified coated titanium dioxide.
[0073] Specifically, the present invention first uses cerium oxide to coat rutile titanium dioxide because cerium oxide has good ultraviolet shielding ability and will not affect the refractive index of rutile titanium dioxide. It can also serve as a base coating film to block and cover the lattice defects of rutile titanium dioxide. Furthermore, the different electron hybrid orbits of transition metal cerium can form new unsaturated electron orbits on the surface of rutile titanium dioxide, which can capture free active electrons. The free active electrons can combine with the holes of rutile titanium dioxide to block the generation of active free radicals, thereby effectively improving the weather resistance of rutile titanium dioxide and effectively reducing the occurrence of yellowing, fading, powdering and the like.
[0074] Furthermore, the present invention uses aluminum oxide to perform a second coating on the cerium oxide-coated rutile titanium dioxide because the reflection wavelength range of aluminum oxide is wider than that of titanium dioxide, which can effectively increase the light refractive index of titanium dioxide, reflect more ultraviolet rays, and improve the weather resistance of titanium dioxide; during the coating process, aluminum oxide is covered on the surface of titanium dioxide particles in a fibrous or flocculent form to form a continuous coating layer, and the coating layer significantly increases the hydroxyl content on the surface of the titanium dioxide particles. The increase in hydroxyl groups increases the hydrophilicity and surface activity of the titanium dioxide particles, which is beneficial to chemical bonds such as hydrogen bonds. Hydroxyl groups can also interact with polyphthalamide molecular chains through physical adsorption and entanglement, thereby forming a strong interface interaction with the PPA material, thereby increasing the bonding strength between titanium dioxide and the PPA material, thereby increasing the mechanical strength of the PPA material and reducing the warping of the PPA material.
[0075] Since the particle size of rutile titanium dioxide is small and the surface free energy is high, the particles are prone to agglomeration. Therefore, the present invention uses polyols to perform a third coating on the rutile titanium dioxide coated with cerium oxide and aluminum oxide. The polyol molecules form hydrogen bonds or van der Waals forces with the hydroxyl groups on the surface of the rutile titanium dioxide through their hydrophilic hydroxyl groups, thereby being adsorbed on the particle surface; and in a weakly acidic environment, some hydroxyl groups of the polyol molecules lose protons to form negatively charged oxygen atoms, thereby making it easier to undergo condensation reactions with the hydroxyl groups on the surface of the rutile titanium dioxide to form organic functional groups, thereby preventing the rutile titanium dioxide from agglomerating.
[0076] As an optional embodiment of the present invention, in step S1, the concentration of the rutile titanium dioxide slurry is 280-320 g / L (such as 285 g / L, 290 g / L, 295 g / L, 300 g / L, 305 g / L, 310 g / L, 315 g / L), preferably 300 g / L;
[0077] Specifically, the present invention limits the concentration of rutile titanium dioxide slurry to 280-320 g / L. This is because when the concentration of the slurry is 280-320 g / L, the cerium ions and the rutile titanium dioxide particles are evenly distributed in the slurry, and the tetravalent cerium ions react with the hydroxide ions in the solution and immediately collide with the rutile titanium dioxide particles, forming cerium oxygen titanium bonds on the surface of the rutile titanium dioxide particles to form coated core points, and the continuous collision of the tetravalent cerium ions with the rutile titanium dioxide particles causes continuous accumulation around the core points to form a dense film layer;
[0078] When the concentration of the slurry is too high or too low, it will lead to uneven distribution of tetravalent cerium ions in the slurry, causing the rutile titanium dioxide particles and tetravalent cerium ions to agglomerate separately. The tetravalent cerium ions quickly react with the hydroxide ions and nucleate themselves in a short time, making it difficult to form nuclei on the surface of the rutile titanium dioxide particles. Even if nuclei are formed, it is difficult to continue to grow on the nuclei to form a continuous, uniform and dense film layer.
[0079] And / or, the mass ratio of the rutile titanium dioxide slurry to the sodium hexametaphosphate is (10-15):1 (such as 10:1, 11:1, 12:1, 13:1, 14:1, etc.);
[0080] And / or, the ultrasonic dispersion time is 30-45 min.
[0081] As an optional embodiment of the present invention, in step S2, the heating conditions include:
[0082] Heat in a water bath to 50-90°C (e.g. 60°C, 70°C, 80°C, etc.);
[0083] and / or, the concentration of the cerium nitrate solution is 90-110 g / L (such as 95 g / L, 100 g / L, 105 g / L, etc.), preferably 100 g / L;
[0084] Preferably, the volume of the cerium nitrate solution added dropwise is 20-40 mL (such as 25 mL, 30 mL, 35 mL, etc.), preferably 30 mL;
[0085] And / or, the concentration of the sodium hydroxide solution is 250-300 g / L (such as 260 g / L, 270 g / L, 280 g / L, 290 g / L, etc.), preferably 280 g / L;
[0086] Preferably, the purpose of adding the sodium hydroxide solution is to maintain the pH value of the dispersion at 9-10;
[0087] And / or, the titration speed is 4-5 mL / min;
[0088] And / or, the conditions of the first aging include:
[0089] The temperature is 50-90°C, the pH is 9-10, and the time is 1.5-2h.
[0090] Specifically, during the first aging process, the pH value is maintained at 9-10 because the alkaline environment can promote the hydrolysis and precipitation of cerium ions to generate cerium hydroxide precipitates. These precipitates can form a uniform cerium oxide film on the surface of titanium dioxide particles, thereby further enhancing the weather resistance of titanium dioxide.
[0091] As an optional embodiment of the present invention, in step S3, the concentration of the sodium aluminate solution is 90-110 g / L (such as 95 g / L, 100 g / L, 105 g / L, etc.), preferably 100 g / L;
[0092] Preferably, the volume of the sodium aluminate solution added dropwise is 20-40 mL (e.g., 25 mL, 30 mL, 35 mL, etc.), preferably 30 mL;
[0093] And / or, the titration speed is 4-5 mL / min;
[0094] And / or, the conditions for the second aging include:
[0095] The temperature is 50-90°C (such as 60°C, 70°C, 80°C, etc.), the pH is 9-10, and the time is 1.5-2h.
[0096] Specifically, during the second aging process, the pH is maintained at 9-10 because under alkaline conditions, sodium aluminate will hydrolyze in water to form aluminum hydroxide, allowing the aluminum oxide film to better adhere to the surface of the titanium dioxide particles of the cerium oxide film to obtain a better coating effect.
[0097] As an optional embodiment of the present invention, in step S4, the concentration of the polyol solution is 90-110 g / L (such as 95 g / L, 100 g / L, 105 g / L, etc.), preferably 100 g / L;
[0098] Preferably, the volume of the polyol solution added dropwise is 20-40 mL (such as 25 mL, 30 mL, 35 mL, etc.), preferably 30 mL;
[0099] Preferably, the polyol comprises one or more of neopentyl glycol (NPG), trimethylolpropane (TMP) or trimethylolethane (TME);
[0100] Specifically, the polyols defined in the present invention are short carbon chain polyols with a neopentyl structure. These alcohols contain planar symmetrical primary hydroxyl groups, and due to the geminal dimethyl structure, there are no hydrogen atoms at the β-position, which makes them highly chemically stable and thermally stable. They can form a uniform organic coating layer on the surface of titanium dioxide particles, eliminate or weaken the polar adsorption between titanium dioxide particles, and prevent the occurrence of agglomeration.
[0101] And / or, the concentration of the dilute sulfuric acid solution is 150-200 g / L (such as 160 g / L, 170 g / L, 180 g / L, 190 g / L, etc.), preferably 190 g / L;
[0102] Preferably, the purpose of adding the dilute sulfuric acid solution is to maintain the pH value during the third aging process at 4-6 (such as 4.5, 5, 5.5, etc.);
[0103] And / or, the conditions for the third aging include:
[0104] The temperature is 50-90°C, the pH is 4-6, and the time is 1.5-2h;
[0105] And / or, the titration speed is 4-5 mL / min.
[0106] Specifically, during the third aging process, the pH is maintained at 4-6 because in a weakly acidic environment, some hydroxyl groups of the polyol molecules lose protons to form negatively charged oxygen atoms, which are easier to condense with the hydroxyl groups on the surface of rutile titanium dioxide to form organic functional groups, thereby preventing rutile titanium dioxide from agglomerating.
[0107] As an optional embodiment of the present invention, in step S5, the filtration includes: using 50-60°C water to filter the cerium oxide, aluminum oxide and polyol-coated rutile titanium dioxide slurry for multiple times until the concentration of BaCl 2 The solution was determined to have no sulfate in the filtrate, and a filter cake was obtained;
[0108] And / or, the drying comprises:
[0109] The filter cake was placed in a drying oven at 100-130° C. for 10-12 h.
[0110] As an optional embodiment of the present invention, the compatibilizer is a polymer containing maleic anhydride grafts;
[0111] Preferably, the polymer containing maleic anhydride grafts includes one or more of maleic anhydride grafted polyolefins, maleic anhydride grafted polyesters, maleic anhydride grafted polyethers, and maleic anhydride grafted polyamides.
[0112] Specifically, the present invention adopts a polymer containing maleic anhydride grafts as a compatibilizer. The polymer containing maleic anhydride grafts is usually composed of a main chain and multiple side chains. This structure enables the grafted polymer to act as a bridge between different polymers, improve the interfacial compatibility between two or more polymers, and reduce phase separation at the interface; and the polymer containing maleic anhydride grafts contains polar functional groups, which enables it to form hydrogen bonds or other interactions with polar polymers (such as nylon, polyester, epoxy resin, etc.), thereby improving the adhesion and compatibility of the material.
[0113] And / or, the antioxidant is a composite antioxidant;
[0114] Preferably, the composite antioxidant includes one or more of KBG779 and H3373.
[0115] Specifically, the yellowing of polyphthalamide is caused by the thermal oxidation of polyphthalamide at high temperature to generate chromophores such as carboxyl, aldehyde or ketone, while the composite antioxidants KBG779 and H3373 are both highly efficient antioxidant additives, containing a complex of hindered phenols and phosphite antioxidants. This structure can terminate free radicals and inhibit the decomposition of hydroperoxides, which can effectively prevent the thermal oxidation reaction of polyphthalamide at high temperature, and effectively improve the heat resistance, light resistance and oxygen resistance of polyphthalamide, thereby preventing aging and yellowing of the composite materials during processing and use.
[0116] And / or, the lubricant is one or more of paraffin wax, polyethylene wax, polypropylene wax, polysiloxane, and silicone powder;
[0117] And / or, the nucleating agent includes one or more of sodium laurate, sodium stearate, sodium oleate, and sodium myristic acid.
[0118] According to a second aspect of the present invention, there is provided a method for preparing the above-mentioned high-gloss, low-warpage polyphthalamide material, comprising the following steps:
[0119] (1) drying the raw materials;
[0120] (2) placing the dried raw materials in a blender and mixing them evenly;
[0121] (3) The uniformly mixed materials are melt-blended in a twin-screw extruder and extruded into granules.
[0122] As an optional embodiment of the present invention, in step (1), the drying condition is drying at 100-120° C. (such as 105° C., 110° C., 115° C., etc.) for 4-6 h (such as 4.5 h, 5 h, 5.5 h, etc.);
[0123] And / or, in step (2), the stirring time is 10-20 min (e.g., 12 min, 14 min, 16 min, 18 min, etc.).
[0124] And / or, in step (3), the setting conditions of the twin-screw extruder are: the temperature of zone 1 is 250-270°C (for example, 255°C, 260°C, 265°C, etc.), the temperature of zone 2 is 260-280°C (for example, 265°C, 270°C, 275°C, etc.), the temperature of zone 3 is 270-290°C (for example, 275°C, 280°C, 285°C, etc.), the temperature of zone 4 is 280-300°C (for example, 285°C, 290°C, 295°C, etc.), the temperature of zone 5 is 290-310°C (for example, 295°C, 300°C, 305°C, etc.) ), the head temperature is 300-320℃ (such as 305℃, 310℃, 315℃, etc.); the screw speed is controlled at 220-350r / min (such as 240r / min, 260r / min, 280r / min, 300r / min, 320r / min, 340r / min, etc.), the mixture is conveyed in the screw for 3-5min (such as 3.5min, 4min, 4.5min, etc.), and the pressure is 12-20Pa (such as 14Pa, 16Pa, 18Pa, etc.).
[0125] The present invention will be further described in detail below with reference to specific embodiments and comparative examples.
[0126] The polyphthalamide used was semi-aromatic nylon (PPAHTN 51G50, DuPont (China) Co., Ltd., USA);
[0127] The remaining raw materials are commercially available.
[0128] Example 1
[0129] Preparation of modified coated titanium dioxide:
[0130] S1: ultrasonically disperse rutile titanium dioxide slurry (300 g / L, 1 L) and sodium hexametaphosphate (30 g) for 30 min to obtain a dispersion;
[0131] S2: The dispersion is heated in a water bath to 70° C., a cerium nitrate solution (100 g / L, 30 mL) and a sodium hydroxide solution (280 g / L) are added dropwise to the dispersion, the pH value of the dispersion is maintained at 10, and titration is performed at a rate of 4 mL / min. After the titration is completed, the first aging is performed at a temperature of 70° C. and a pH of 10 for 2 h to obtain a cerium oxide-coated rutile titanium dioxide slurry;
[0132] S3: adding sodium aluminate solution (100 g / L, 30 mL) to the rutile titanium dioxide slurry coated with cerium oxide, maintaining the pH value of the solution at 10, and titrating at a rate of 4 mL / min. After the titration is completed, aging for a second time at a temperature of 70° C. and a pH of 10 for 2 h to obtain a rutile titanium dioxide slurry coated with cerium oxide and aluminum oxide;
[0133] S4: adding a polyol solution (100 g / L, 20-40 mL) and a dilute sulfuric acid solution (190 g / L) to the rutile titanium dioxide slurry coated with cerium oxide and aluminum oxide, maintaining the pH value at 4, and titrating at a rate of 4 mL / min. After the titration is completed, aging for a third time at a temperature of 70° C. and a pH of 4 for 2 h to obtain a rutile titanium dioxide slurry coated with cerium oxide, aluminum oxide and a polyol;
[0134] S5: The cerium oxide, aluminum oxide and polyol coated rutile titanium dioxide slurry is filtered several times with deionized water at 60°C until the slurry is diluted with 10% BaCl 2 The solution was determined to contain no sulfate in the filtrate, and a filter cake was obtained; the filter cake was then placed in a drying oven, dried at 130° C. for 10 hours, and finally placed in a grinder for grinding to obtain a modified coated titanium dioxide with a particle size of 70 meshes.
[0135] Preparation of high gloss and low warpage polyphthalamide materials:
[0136] (1) 65 g of polyphthalamide, 50 g of modified coated titanium dioxide, g of maleic anhydride grafted polyolefin, 0.2 g of KBG779, 0.4 g of polysiloxane and 0.3 g of sodium stearate were placed in an electric heated blast drying oven at 120° C. and dried for 6 h;
[0137] (2) Place the dried raw materials in a high-speed stirrer and stir to mix evenly for 20 minutes;
[0138] (3) The uniformly mixed materials are melt-blended in a twin-screw extruder. The setting conditions of the twin-screw extruder are as follows: the temperature of zone 1 is 250°C, the temperature of zone 2 is 260°C, the temperature of zone 3 is 270°C, the temperature of zone 4 is 280°C, the temperature of zone 5 is 290°C, and the head temperature is 300°C; the screw speed is controlled at 220r / min, the conveying time of the mixed material in the screw is 5min, and the pressure is 12Pa; after melt-blending extrusion, water cooling, air drying, pelletizing, and drying, a high-gloss and low-warpage polyphthalamide material is obtained.
[0139] The performance data of the high-gloss, low-warpage polyphthalamide material prepared in this embodiment are shown in Table 1.
[0140] Example 2
[0141] Preparation of modified coated titanium dioxide:
[0142] S1: ultrasonically disperse rutile titanium dioxide slurry (310 g / L, 1 L) and sodium hexametaphosphate (25 g) for 45 min to obtain a dispersion;
[0143] S2: The dispersion is heated in a water bath to 60° C., and a cerium nitrate solution (90 g / L, 40 mL) and a sodium hydroxide solution (280 g / L) are added dropwise to the dispersion, and the pH value of the dispersion is maintained at 9, and titration is performed at a rate of 5 mL / min. After the titration is completed, the first aging is performed at a temperature of 60° C. and a pH of 9 for 2 h to obtain a cerium oxide-coated rutile titanium dioxide slurry;
[0144] S3: adding sodium aluminate solution (90 g / L, 40 mL) to the rutile titanium dioxide slurry coated with cerium oxide, maintaining the pH value of the solution at 9, and titrating at a rate of 5 mL / min. After the titration is completed, aging for a second time at a temperature of 60° C. and a pH of 9 for 2 h to obtain a rutile titanium dioxide slurry coated with cerium oxide and aluminum oxide;
[0145] S4: adding a polyol solution (900 g / L, 40 mL) and a dilute sulfuric acid solution (190 g / L) to the rutile titanium dioxide slurry coated with cerium oxide and aluminum oxide, maintaining the pH value at 6, and titrating at a rate of 5 mL / min. After the titration is completed, aging for a third time at a temperature of 60° C. and a pH of 6 for 2 h to obtain a rutile titanium dioxide slurry coated with cerium oxide, aluminum oxide and a polyol;
[0146] S5: The cerium oxide, aluminum oxide and polyol coated rutile titanium dioxide slurry is filtered several times with deionized water at 60°C until the slurry is diluted with 10% BaCl 2 The solution was determined to contain no sulfate in the filtrate, and a filter cake was obtained; the filter cake was then placed in a drying oven, dried at 120° C. for 11 hours, and finally placed in a grinder for grinding to obtain a modified coated titanium dioxide with a particle size of 60 meshes.
[0147] Preparation of high gloss and low warpage polyphthalamide materials:
[0148] (1) 55 g of polyphthalamide, 45 g of modified coated titanium dioxide, 0.1 g of maleic anhydride grafted polyamide, 0.6 g of H3373, 0.2 g of paraffin wax, and 0.5 g of sodium laurate were placed in an electric heated blast drying oven at 100° C. and dried for 4 h;
[0149] (2) Place the dried raw materials in a high-speed stirrer and stir to mix evenly for 10 minutes;
[0150] (3) The uniformly mixed materials are melt-blended in a twin-screw extruder. The setting conditions of the twin-screw extruder are as follows: the temperature of zone 1 is 270°C, the temperature of zone 2 is 280°C, the temperature of zone 3 is 290°C, the temperature of zone 4 is 300°C, the temperature of zone 5 is 310°C, and the head temperature is 320°C; the screw speed is controlled at 350r / min, the conveying time of the mixed material in the screw is 3min, and the pressure is 20Pa; after melt-blending extrusion, water cooling, air drying, pelletizing, and drying, a high-gloss and low-warpage polyphthalamide material is obtained.
[0151] The performance data of the high-gloss, low-warpage polyphthalamide material prepared in this embodiment are shown in Table 1.
[0152] Example 3
[0153] Preparation of modified coated titanium dioxide:
[0154] S1: ultrasonically disperse rutile titanium dioxide slurry (280 g / L, 1 L) and sodium hexametaphosphate (18 g) for 40 min to obtain a dispersion;
[0155] S2: The dispersion is heated to 90° C. in a water bath, and a cerium nitrate solution (110 g / L, 20 mL) and a sodium hydroxide solution (280 g / L) are added dropwise to the dispersion, the pH value of the dispersion is maintained at 10, and titration is performed at a rate of 5 mL / min. After the titration is completed, the first aging is performed at a temperature of 90° C. and a pH of 10 for 1.5 h to obtain a cerium oxide-coated rutile titanium dioxide slurry;
[0156] S3: adding sodium aluminate solution (110 g / L, 40 mL) to the rutile titanium dioxide slurry coated with cerium oxide, maintaining the pH value of the solution at 10, and titrating at a rate of 5 mL / min. After the titration is completed, a second aging is performed at a temperature of 90° C. and a pH of 10 for 1.5 h to obtain a rutile titanium dioxide slurry coated with cerium oxide and aluminum oxide;
[0157] S4: adding a polyol solution (110 g / L, 40 mL) and a dilute sulfuric acid solution (190 g / L) to the rutile titanium dioxide slurry coated with cerium oxide and aluminum oxide, maintaining the pH value at 5, and titrating at a rate of 5 mL / min. After the titration is completed, aging for a third time at a temperature of 90° C. and a pH of 5 for 1.5 h to obtain a rutile titanium dioxide slurry coated with cerium oxide, aluminum oxide and a polyol;
[0158] S5: The cerium oxide, aluminum oxide and polyol coated rutile titanium dioxide slurry is filtered several times with deionized water at 50°C until the slurry is filtered with a concentration of 10% BaCl 2The solution was determined to contain no sulfate in the filtrate, and a filter cake was obtained; the filter cake was then placed in a drying oven, dried at 100° C. for 12 hours, and finally placed in a grinder for grinding to obtain a modified coated titanium dioxide with a particle size of 50 meshes.
[0159] Preparation of high gloss and low warpage polyphthalamide materials:
[0160] (1) 48 g of polyphthalamide, 45 g of modified coated titanium dioxide, 1 g of maleic anhydride grafted polyether, 0.4 g of KBG779, 0.3 g of polyethylene wax and polypropylene wax, and 0.4 g of sodium laurate and sodium stearate were placed in an electric heated blast drying oven at 110° C. and dried for 5 h;
[0161] (2) Place the dried raw materials in a high-speed stirrer and stir to mix evenly for 15 minutes;
[0162] (3) The uniformly mixed materials are melt-blended in a twin-screw extruder. The setting conditions of the twin-screw extruder are as follows: the temperature of zone 1 is 260°C, the temperature of zone 2 is 270°C, the temperature of zone 3 is 280°C, the temperature of zone 4 is 290°C, the temperature of zone 5 is 300°C, and the head temperature is 310°C; the screw speed is controlled at 300 r / min, the conveying time of the mixed material in the screw is 4 min, and the pressure is 15 Pa; after melt-blending extrusion, water cooling, air drying, pelletizing, and drying, a high-gloss and low-warpage polyphthalamide material is obtained.
[0163] The performance data of the high-gloss, low-warpage polyphthalamide material prepared in this embodiment are shown in Table 1.
[0164] Example 4
[0165] Preparation of modified coated titanium dioxide:
[0166] S1: ultrasonically disperse rutile titanium dioxide slurry (300 g / L, 1 L) and sodium hexametaphosphate (30 g) for 45 min to obtain a dispersion;
[0167] S2: The dispersion is heated to 50° C. in a water bath, and a cerium nitrate solution (100 g / L, 30 mL) and a sodium hydroxide solution (280 g / L) are added dropwise to the dispersion, the pH value of the dispersion is maintained at 10, and titration is performed at a rate of 45 mL / min. After the titration is completed, the first aging is performed at a temperature of 50° C. and a pH of 10 for 2 h to obtain a cerium oxide-coated rutile titanium dioxide slurry;
[0168] S3: adding sodium aluminate solution (100 g / L, 30 mL) to the rutile titanium dioxide slurry coated with cerium oxide, maintaining the pH value of the solution at 10, and titrating at a rate of 5 mL / min. After the titration is completed, aging for a second time at a temperature of 50° C. and a pH of 10 for 2 h to obtain a rutile titanium dioxide slurry coated with cerium oxide and aluminum oxide;
[0169] S4: adding a polyol solution (100 g / L, 30 mL) and a dilute sulfuric acid solution (190 g / L) to the rutile titanium dioxide slurry coated with cerium oxide and aluminum oxide, maintaining the pH value at 4, and titrating at a rate of 5 mL / min. After the titration is completed, aging for a third time at a temperature of 50° C. and a pH of 4 for 2 h to obtain a rutile titanium dioxide slurry coated with cerium oxide, aluminum oxide and a polyol;
[0170] S5: The cerium oxide, aluminum oxide and polyol coated rutile titanium dioxide slurry is filtered several times with deionized water at 50°C until the slurry is filtered with a concentration of 10% BaCl 2 The solution was determined to contain no sulfate in the filtrate, and a filter cake was obtained; the obtained filter cake was then placed in a drying oven, dried at 100° C. for 12 hours, and finally placed in a grinder for grinding to obtain a modified coated titanium dioxide with a particle size of 65 meshes.
[0171] Preparation of high gloss and low warpage polyphthalamide materials:
[0172] (1) 60 g of polyphthalamide, 45 g of modified coated titanium dioxide, 2 g of maleic anhydride grafted polyolefin and maleic anhydride grafted polyester, 0.6 g of KBG779 and H3373, 0.4 g of polysiloxane and silicone powder, and 0.5 g of sodium myristate were placed in an electric heated forced air drying oven at 120° C. and dried for 6 h;
[0173] (2) Place the dried raw materials in a high-speed stirrer and stir to mix evenly for 20 minutes;
[0174] (3) The uniformly mixed materials are melt-blended in a twin-screw extruder. The setting conditions of the twin-screw extruder are as follows: the temperature of zone 1 is 250°C, the temperature of zone 2 is 260°C, the temperature of zone 3 is 270°C, the temperature of zone 4 is 280°C, the temperature of zone 5 is 290°C, and the head temperature is 300°C; the screw speed is controlled at 220r / min, the conveying time of the mixed material in the screw is 5min, and the pressure is 12Pa; after melt-blending extrusion, water cooling, air drying, pelletizing, and drying, a high-gloss and low-warpage polyphthalamide material is obtained.
[0175] The performance data of the high-gloss, low-warpage polyphthalamide material prepared in this embodiment are shown in Table 1.
[0176] Comparative Example 1
[0177] The difference between this comparative example and Example 1 is that only cerium oxide and polyol are used to encapsulate rutile titanium dioxide, and the remaining steps and technical parameters are the same as those in Example 1.
[0178] The performance data of the high-gloss, low-warpage polyphthalamide material prepared in this comparative example are shown in Table 1.
[0179] Comparative Example 2
[0180] The difference between this comparative example and Example 1 is that only aluminum oxide and polyol are used to coat the rutile titanium dioxide, and the remaining steps and technical parameters are the same as those in Example 1.
[0181] The performance data of the high-gloss, low-warpage polyphthalamide material prepared in this comparative example are shown in Table 1.
[0182] Comparative Example 3
[0183] The difference between this comparative example and Example 1 is that only cerium oxide and aluminum oxide are used to coat the rutile titanium dioxide, and the remaining steps and technical parameters are the same as those in Example 1.
[0184] The performance data of the high-gloss, low-warpage polyphthalamide material prepared in this comparative example are shown in Table 1.
[0185] Comparative Example 4
[0186] The difference between this comparative example and Example 1 is that in step S1, the concentration of the rutile titanium dioxide slurry is 350 g / L, and the remaining steps and technical parameters are the same as those in Example 1.
[0187] The performance data of the high-gloss, low-warpage polyphthalamide material prepared in this comparative example are shown in Table 1.
[0188] Performance Comparison
[0189] The performance testing method adopted by the present invention is as follows:
[0190] Tensile strength: tested according to GB / T 1040 standard; the specimen type is type I, the specimen size (mm): 170 (length) × (20 ± 0.2) (end width) × (4 ± 0.2) (thickness), the tensile speed is 50 mm / min;
[0191] Bending strength: Tested according to GB / T9341 standard; sample type: sample size (mm): (80±2)×(10±0.2)×(4±0.2), bending speed: 20mm / min;
[0192] Warpage: The prepared polyphthalamide material was injection molded into a disc with a diameter of D = 100 mm and a thickness of 2.0 = mm using an injection molding machine. After being placed for 48 hours, the maximum height H of the disc after warping was measured. H and D were used to characterize the degree of warping of the material. Warpage = H / D.
[0193] Blue-white photometry: The whiteness of a substance is usually measured with magnesium oxide as the standard whiteness of 100%. The whiteness of the sample is expressed as the percentage of the reflectivity of the surface of the standard plate illuminated by blue light to magnesium oxide. The measurement is performed using a fully automatic whiteness meter (WD-5).
[0194] YI: refers to the degree to which colorless, transparent, translucent or nearly white plastics that do not contain fluorescent substances deviate from white. YI is a parameter that is very sensitive to aging. Sometimes, even when the structural changes have not yet been reflected in its infrared spectrum, the changes in YI can be detected. According to ASTM D1925-1970 (1977) standard, the calculation formula of YI is:
[0195] YI = 100 (1.28X - 1.06Z) / Y;
[0196] Where: X, Y, Z are the three stimulus values of the material color measured under the standard light source.
[0197] The larger the positive value of YI is, the yellower the material is, and the negative value indicates that the material is bluish.
[0198] The high gloss and low warpage polyphthalamide materials prepared in Examples 1-4 and Comparative Examples 1-4 were injection molded on an injection molding machine to prepare samples and perform performance tests, as shown in Table 1:
[0199] Table 1
[0200]
[0201] As shown in Table 1, compared with Example 1 of the present invention, since only cerium oxide and polyol are used to encapsulate rutile titanium dioxide in Comparative Example 1, and no aluminum oxide is added, the interfacial interaction between the titanium dioxide particles and the PPA material is reduced, thereby affecting the mechanical properties of the PPA material. In addition, the refractive index of titanium dioxide is reduced to a certain extent, so the blue-white luminosity of Comparative Example 1 decreases and the YI value increases.
[0202] As shown in Table 1, compared with Example 1 of the present invention, since Comparative Example 2 only uses aluminum oxide and polyol to encapsulate rutile titanium dioxide without adding cerium oxide, not only does it lead to a decrease in the blue-white luminosity of the PPA material, but it also fails to cover the lattice defects of rutile titanium dioxide, thereby causing a significant increase in the YI value.
[0203] As shown in Table 1, compared with Example 1 of the present invention, in Comparative Example 3, since only cerium oxide and aluminum oxide are used to encapsulate the rutile titanium dioxide in Comparative Example 3, and no polyol is added, the rutile titanium dioxide agglomerates, which affects the uniformity of bonding with the PPA material and causes a decrease in mechanical properties.
[0204] As shown in Table 1, compared with Example 1 of the present invention, in step S1 of Comparative Example 4, the concentration of the rutile titanium dioxide slurry is 350 g / L, which causes uneven distribution of tetravalent cerium ions in the slurry, resulting in agglomeration of rutile titanium dioxide particles and tetravalent cerium ions, making it difficult to form nuclei and a uniform film layer on the surface of the rutile titanium dioxide particles, resulting in a decrease in the mechanical properties and blue-white luminosity of the prepared PPA material, and an increase in the YI value.
[0205] Finally, it should be noted that the above embodiments are only used to illustrate the technical solutions of the present invention, rather than to limit it. Although the present invention has been described in detail with reference to the aforementioned embodiments, those skilled in the art should understand that they can still modify the technical solutions described in the aforementioned embodiments, or replace some or all of the technical features therein with equivalents. However, these modifications or replacements do not cause the essence of the corresponding technical solutions to deviate from the scope of the technical solutions of the embodiments of the present invention.
Claims
1. A high gloss, low warpage polyphthalamide material, characterized in that: In terms of mass percentage, it includes the following components: Polyphthalamide 40-66%, modified coated titanium dioxide 30-56%, compatibilizer 0.1-2%, antioxidant 0.2-0.6%, lubricant 0.2-0.4% and nucleating agent 0.3-1%.
2. The high-gloss, low-warping polyphthalamide material according to claim 1, characterized in that: The modified coated titanium dioxide is rutile titanium dioxide synergistically coated with cerium oxide, aluminum oxide and polyol; And / or, the particle size of the modified coated titanium dioxide is 50-70 mesh.
3. The high gloss, low warpage polyphthalamide material according to claim 1, characterized in that: The preparation method of the modified coated titanium dioxide comprises the following steps: S1: ultrasonically dispersing the rutile titanium dioxide slurry and sodium hexametaphosphate to obtain a dispersion; S2: heating the dispersion, adding cerium nitrate solution and sodium hydroxide solution to the dispersion, and after the titration, performing a first aging to obtain a cerium oxide coated rutile titanium dioxide slurry; S3: adding a sodium aluminate solution dropwise to the rutile titanium dioxide slurry coated with cerium oxide, and performing a second aging after the titration is completed to obtain a rutile titanium dioxide slurry coated with cerium oxide and aluminum oxide; S4: adding a polyol solution and a dilute sulfuric acid solution to the rutile titanium dioxide slurry coated with cerium oxide and aluminum oxide, and performing a third aging after the titration is completed to obtain a rutile titanium dioxide slurry coated with cerium oxide, aluminum oxide and a polyol; S5: filtering the cerium oxide, aluminum oxide and polyol coated rutile titanium dioxide slurry for multiple times, and then drying and grinding the obtained filter cake to obtain modified coated titanium dioxide.
4. The high-gloss, low-warping polyphthalamide material according to claim 3, characterized in that: In step S1, the concentration of the rutile titanium dioxide slurry is 280-320 g / L, preferably 300 g / L; And / or, the mass ratio of the rutile titanium dioxide slurry to the sodium hexametaphosphate is (10-15):1; And / or, the ultrasonic dispersion time is 30-45 min.
5. The high-gloss, low-warpage polyphthalamide material according to claim 3, characterized in that: In step S2, the heating conditions include: Heat in a water bath to 50-90°C; and / or, the concentration of the cerium nitrate solution is 90-110 g / L, preferably 100 g / L; Preferably, the volume of the cerium nitrate solution added dropwise is 20-40 mL, preferably 30 mL; And / or, the concentration of the sodium hydroxide solution is 250-300 g / L, preferably 280 g / L; Preferably, the purpose of adding the sodium hydroxide solution is to maintain the pH value of the dispersion at 9-10; And / or, the titration speed is 4-5 mL / min; And / or, the conditions of the first aging include: The temperature is 50-90°C, the pH is 9-10, and the time is 1.5-2h.
6. The high-gloss, low-warpage polyphthalamide material according to claim 3, characterized in that: In step S3, the concentration of the sodium aluminate solution is 90-110 g / L, preferably 100 g / L; Preferably, the volume of the sodium aluminate solution added dropwise is 20-40 mL, preferably 30 mL; And / or, the titration speed is 4-5 mL / min; And / or, the conditions for the second aging include: The temperature is 50-90°C, the pH is 9-10, and the time is 1.5-2h.
7. The high-gloss, low-warpage polyphthalamide material according to claim 3, characterized in that: In step S4, the concentration of the polyol solution is 90-110 g / L, preferably 100 g / L; Preferably, the volume of the polyol solution added dropwise is 20-40 mL, preferably 30 mL; Preferably, the polyol includes one or more of neopentyl glycol, trimethylolpropane or trimethylolethane; and / or, the concentration of the dilute sulfuric acid solution is 150-200 g / L, preferably 190 g / L; Preferably, the purpose of adding the dilute sulfuric acid solution is to maintain the pH value during the third aging process at 4-6; And / or, the conditions for the third aging include: The temperature is 50-90°C, the pH is 4-6, and the time is 1.5-2h; And / or, the titration speed is 4-5 mL / min.
8. The high-gloss, low-warpage polyphthalamide material according to claim 3, characterized in that: In step S5, the filtration includes: using 50-60° C. water to filter the cerium oxide, aluminum oxide and polyol-coated rutile titanium dioxide slurry for multiple times until no sulfate is found in the filtrate using a 10% BaCl2 solution to obtain a filter cake; And / or, the drying comprises: The filter cake was placed in a drying oven at 100-130° C. for 10-12 h.
9. The high-gloss, low-warpage polyphthalamide material according to claim 3, characterized in that: The compatibilizer is a polymer containing maleic anhydride grafts; Preferably, the polymer containing maleic anhydride grafts includes one or more of maleic anhydride grafted polyolefins, maleic anhydride grafted polyesters, maleic anhydride grafted polyethers, and maleic anhydride grafted polyamides; And / or, the antioxidant is a composite antioxidant; Preferably, the composite antioxidant includes one or more of KBG779 and H3373; And / or, the lubricant is one or more of paraffin wax, polyethylene wax, polypropylene wax, polysiloxane, and silicone powder; And / or, the nucleating agent includes one or more of sodium laurate, sodium stearate, sodium oleate, and sodium myristic acid.
10. A method for preparing a high-gloss, low-warpage polyphthalamide material as claimed in any one of claims 1 to 9, characterized in that: The steps include: (1) drying the raw materials; (2) placing the dried raw materials in a blender and mixing them evenly; (3) melt-blending the uniformly mixed materials in a twin-screw extruder and extruding them into granules; Among them, the setting conditions of the twin-screw extruder are: zone 1 temperature 250-270°C, zone 2 temperature 260-280°C, zone 3 temperature 270-290°C, zone 4 temperature 280-300°C, zone 5 temperature 290-310°C, and head temperature 300-320°C; the screw speed is controlled at 220-350r / min, the mixed material conveying time in the screw is 3-5min, and the pressure is 12-20Pa.