Modified calcium carbonate filler for non-intumescent fire retardant coating and preparation method of modified calcium carbonate filler

Through the preparation of modified calcium carbonate filler, the combination technology of nano-calcium carbonate and calcium carbonate suspension is used to solve the problem of poor dispersion of fillers in non-expanding fire retardant coatings, improve the bonding strength and fire resistance, and improve the coating's Fire protection effect.

CN118852891APending Publication Date: 2024-10-29HUBEI JINGJING CALCIUM IND CO LTD
View PDF 0 Cites 2 Cited by

Patent Information

Application Number
CN202410818288.7
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-06-24
Publication Date
2024-10-29

AI Technical Summary

Technical Problem

The poor dispersion of inorganic fillers in existing non-intumescent fire retardant coatings results in poor bonding strength and affects its fire retardant performance.

Method used

By preparing modified calcium carbonate filler, using the combined technology of nano-calcium carbonate and calcium carbonate suspension, and using methods such as ball milling and laser irradiation to improve the dispersion of nano-calcium carbonate, so that it can be better dispersed in the coating to form calcium carbonate. The structure of wrapped nano calcium carbonate.

Benefits of technology

Significantly improves the bonding strength and fire resistance of non-intumescent fire retardant coatings, improves the dispersion of fillers, and enhances the fire retardant properties of the coating.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118852891A_ABST
    Figure CN118852891A_ABST
Patent Text Reader

Abstract

The invention belongs to the technical field of inorganic fillers, and particularly relates to a modified calcium carbonate filler for a non-intumescent fire retardant coating and a preparation method of the modified calcium carbonate filler. The preparation method of the modified calcium carbonate filler for the non-intumescent fire retardant coating comprises the steps of preparation of nano calcium carbonate, preparation of a calcium carbonate suspension, preparation of the modified calcium carbonate filler and the like, the prepared modified calcium carbonate filler is applied to the fire retardant coating, and the dispersing performance of a fire retardant coating system can be improved; and the adhesive strength and fireproof performance of the coating and the base material are improved, and excellent practicability is achieved.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention belongs to the technical field of inorganic fillers, and in particular relates to a modified calcium carbonate filler for non-expanding fire retardant coatings and a preparation method thereof. Background Art

[0002] Inorganic fillers are one of the important components of fire retardant coatings. In addition to acting as a skeleton in the coating, making the coating full and thick and reducing the cost of coating production, they can also serve as functional additives to give the coating some physical or chemical properties, such as adjusting the rheology of the coating, improving the mechanical strength of the coating, and enhancing the fire resistance of the coating. Common inorganic fillers in fire retardant coatings can be roughly divided into five types: carbonates, silicates, silicon dioxide, barium sulfate, and aluminum hydroxide. Among them, carbonates are the most common minerals in the earth's crust. According to different chemical compositions and sedimentation factors, they can be divided into two categories: calcium carbonate and dolomite. Compared with dolomite, calcium carbonate has become one of the most widely used inorganic fillers in the field of fire retardant coatings due to its low price.

[0003] Fire retardant coating refers to a type of material that is coated on the surface of the protected substrate to reduce the flammability of the substrate and improve the fire resistance of the substrate. According to the combustion characteristics of fire retardant coatings, they can be divided into intumescent and non-intumescent fire retardant coatings. At present, the commonly used fire retardant coatings on the market are mainly intumescent fire retardant coatings. Intumescent fire retardant coatings are mainly composed of polymer resins, fillers, additives, etc. Since suitable polymer resins are selected as film-forming substrates, under high temperature conditions, the coating will rapidly expand and carbonize into a uniform and dense honeycomb or sponge-like structure, forming an expansion layer that is dozens of times thicker than the original coating, thereby achieving the effect of flame retardancy and heat insulation. However, since the main component of intumescent coatings is polymer resins, a large amount of toxic smoke will be generated during the combustion process, which is harmful to human health and affects the safety of people's lives.

[0004] Compared with intumescent fire retardant coatings, non-intumescent fire retardant coatings are generally composed of inorganic base materials and inorganic fillers. They are generally water-soluble, and the coating will not change in volume at high temperatures, nor will it produce toxic smoke. They are also low-cost, and their fire-proof principle is to form a protective layer on the surface, which slows down the temperature rise of the substrate, blocks oxygen and slows down the combustion reaction. However, since the inorganic fillers in non-intumescent fire retardant coatings account for too large a proportion in the coating system and the inorganic fillers have poor dispersibility, the coating has poor adhesion to the substrate. Therefore, it is very meaningful to improve the preparation of low-cost inorganic fillers and thus improve the application scope of non-intumescent fire retardant coatings. Summary of the invention

[0005] In order to overcome the above problems in the prior art, the present invention provides a method for preparing a modified calcium carbonate filler for a non-expanding fire retardant coating.

[0006] The preparation method comprises the following steps:

[0007] S1. Preparation of nano calcium carbonate: calcium carbonate powder is taken, ball milling medium is added, and the powder is placed in a ball mill; polyethylene glycol aqueous solution is added to the ball mill, inert gas is filled in, and the ball mill is sealed; grinding is performed once, cooling is performed once; grinding is performed twice, and cooling is performed twice; the ball milling medium is separated after taking out, and the powder is dried; the dried powder is spread flat, and laser irradiation treatment is performed;

[0008] S2. Preparation of calcium carbonate suspension: Take quicklime and add water to obtain lime milk suspension; introduce CO2 gas into the lime milk suspension until the pH of the suspension drops to 7.5-8 to obtain calcium carbonate suspension;

[0009] S3. Preparation of modified calcium carbonate filler: weigh the nano calcium carbonate described in step S1, add water and ultrasonically disperse it; Preparation of modified calcium carbonate filler: weigh the nano calcium carbonate described in step S1, add water and ultrasonically disperse it, add it to the calcium carbonate suspension described in step S2, stir, centrifuge, and dry to obtain modified calcium carbonate filler.

[0010] Furthermore, the weight ratio of the calcium carbonate powder to the polyethylene glycol aqueous solution is (5-10):1, and the weight ratio of the calcium carbonate powder to the ball milling medium is 1:(5-10).

[0011] Preferably, the weight ratio of the calcium carbonate powder to the polyethylene glycol aqueous solution is 8:1, and the weight ratio of the calcium carbonate powder to the ball milling medium is 1:8.

[0012] Furthermore, the polyethylene glycol is polyethylene glycol 200, and the weight ratio of polyethylene glycol 200 to water in the polyethylene glycol aqueous solution is (1-4):100.

[0013] Preferably, the polyethylene glycol is polyethylene glycol 200, and the weight ratio of polyethylene glycol 200 to water in the polyethylene glycol aqueous solution is 1:50.

[0014] Furthermore, the ball milling medium in step S1 is one or a combination of zirconia balls or steel balls.

[0015] Preferably, the ball milling medium in step S1 is a zirconia ball.

[0016] Furthermore, the particle size of the ball milling medium in step S1 is 0.2 mm.

[0017] Furthermore, the inert gas is nitrogen or argon.

[0018] Furthermore, in the step S1, the grinding rate of the first grinding process is 500-1000 r / min, and the grinding time is 1-3 h, and the grinding rate of the second grinding process is 1500-2500 r / min, and the grinding time is 20-40 min.

[0019] Preferably, in step S1, the grinding rate of the first grinding process is 800 r / min, and the grinding time is 2 h, and the grinding rate of the second grinding process is 2000 r / min, and the grinding time is 30 min.

[0020] Furthermore, the primary cooling and secondary cooling methods described in step S1 are both liquid nitrogen cooling.

[0021] Furthermore, in steps S1 and S3, the drying temperature is 80-120° C., and the drying time is 2-4 hours.

[0022] Preferably, the drying temperature in steps S1 and S3 is 110° C. and the drying time is 3 hours.

[0023] Furthermore, the laser irradiation processing conditions in step S1 are: laser power is 40-100W, scanning speed is 5-10mm / s; and the laser irradiation method is single-pass laser irradiation.

[0024] Preferably, the laser irradiation processing conditions in step S1 are: laser power is 80W, and scanning speed is 8mm / s.

[0025] Furthermore, the ultrasonic dispersion conditions in step S3 are as follows: ultrasonic dispersion power is 400-800W, and ultrasonic time is 10-30min.

[0026] The present invention also provides a modified calcium carbonate for non-expanding fire retardant coating prepared by the above preparation method.

[0027] The present invention prepares a calcium carbonate suspension by a bubbling method, and adds the prepared nano-calcium carbonate to the calcium carbonate suspension to prepare a modified calcium carbonate filler of calcium carbonate-wrapped nano-calcium carbonate, and the modified calcium carbonate filler prepared by the bubbling method has good dispersibility. Secondly, the nano-calcium carbonate is prepared by a multiple ball milling liquid nitrogen cooling method, which can produce a large amount of fresh reaction interfaces, and the generated internal and external interaction forces can enhance its surface defects. At the same time, the surface is treated by laser irradiation, so that the surface absorbs laser energy due to a sudden change in temperature and generates high-pressure plasma, so that more free radicals are formed on the surface of the nano-calcium carbonate, which is beneficial for the subsequent better wrapping of the nano-calcium carbonate in the calcium carbonate suspension, improves the dispersibility of the modified calcium carbonate filler, and solves the defects of its application in non-expanding fire-retardant coatings. Since the non-expanding fire-retardant coating prepared by using the modified calcium carbonate filler can be well dispersed in the coating, the distribution of the modified calcium carbonate filler is more uniform. Therefore, its fireproof performance is further improved.

[0028] Compared with the prior art, the preparation method of the modified calcium carbonate filler for non-expandable fire retardant coating provided by the present invention has the following beneficial effects:

[0029] 1. Polyethylene glycol is added to perform wet ball milling for multiple times, and nano calcium carbonate is prepared by multiple grinding cooling and laser irradiation treatment, so that more free radicals are formed on the surface of the nano calcium carbonate; calcium carbonate is generated by a bubbling method, and the prepared nano calcium carbonate is added thereto to prepare a modified calcium carbonate filler in which the nano calcium carbonate is wrapped by calcium carbonate, thereby obtaining a modified calcium carbonate filler with better dispersibility, which can be better dispersed in a fire retardant coating.

[0030] 2. The modified calcium carbonate filler prepared by the method of the present invention is used in non-expanding fire retardant coatings, which can improve the defect of poor bonding strength in the non-expanding fire retardant coatings and at the same time improve the fire resistance of the non-expanding fire retardant coatings. BRIEF DESCRIPTION OF THE DRAWINGS

[0031] Figure 1 The process flow chart of the preparation of the modified calcium carbonate filler for the non-expanding fire retardant coating of the present invention is as follows DETAILED DESCRIPTION

[0032] The present invention will be further described below by the description of specific embodiments, but this is not a limitation of the present invention, and those skilled in the art can make various modifications or improvements according to the basic thinking of the present invention, as long as they do not depart from the basic thinking of the present invention, all within the scope of the present invention. In the following examples, those without specifying specific conditions are all carried out according to normal conditions, and those without specifying the manufacturer of the reagents used are all conventional products that can be obtained commercially.

[0033] Example 1

[0034] Example 1 provides a method for preparing a modified calcium carbonate filler for a non-expanding fire retardant coating, the steps being as follows:

[0035] 1. Take 1kg of micron-grade calcium carbonate powder, add 5kg of zirconium oxide balls, and place them in a ball mill. The particle size of the zirconium oxide balls is 0.2mm. Take 200g of polyethylene glycol aqueous solution and add it to the ball mill. The polyethylene glycol aqueous solution is made of polyethylene glycol 200 and water in a weight ratio of 1:100. Fill the ball mill with nitrogen, seal the ball mill, and grind it at a grinding rate of 500r / min for 3h. After grinding, use liquid nitrogen atmosphere for rapid cooling, and then perform secondary grinding. The secondary grinding rate is 1500r / min, and the grinding time is 40min. After grinding, quickly place it in liquid nitrogen atmosphere for cooling. After cooling, take out the zirconium oxide balls, and dry the ground sample at 80℃ for 4h. Then take the dried powder and spread it flat, and perform single-pass laser irradiation treatment. The laser power is 40W and the scanning speed is 5mm / s.

[0036] 2. Take 1.5 kg of quicklime and add 1.5 kg of water to obtain a lime milk suspension; introduce CO2 gas into the lime milk suspension until the pH of the suspension drops to 7.5 to obtain a calcium carbonate suspension;

[0037] 3. Weigh the nano calcium carbonate prepared in step 1, add water and ultrasonically disperse for 30 min at an ultrasonic dispersion power of 400 W, then add it to the calcium carbonate suspension prepared in step 2, stir for 1 h, centrifuge, discard the upper liquid, and dry it at 80 ° C for 4 h to obtain the modified calcium carbonate filler prepared in step 1.

[0038] Example 2

[0039] Example 2 provides a method for preparing a modified calcium carbonate filler for a non-expanding fire retardant coating, the steps being as follows:

[0040] 1. Take 1kg of micron-grade calcium carbonate powder, add 10kg of steel balls, and place in a ball mill with a particle size of 0.2mm; take 100g of polyethylene glycol aqueous solution and add it to the ball mill, wherein the polyethylene glycol aqueous solution is made of polyethylene glycol 200 and water in a weight ratio of 1:25, fill the ball mill with argon gas, seal the ball mill and grind it, the grinding rate is 1000r / min, the time is 1h, after grinding, use liquid nitrogen atmosphere for rapid cooling, and then perform secondary grinding, the secondary grinding rate is 2500r / min, the grinding time is 20min, after grinding, quickly place it in liquid nitrogen atmosphere for cooling; after cooling, take out the steel balls, and dry the ground sample at 120℃ for 2h; then take the dried powder and spread it flat, and perform single-pass laser irradiation treatment, the laser power is 100W, and the scanning speed is 10mm / s;

[0041] 2. Take 2 kg of quicklime and add 2 kg of water to obtain a lime milk suspension; introduce CO2 gas into the lime milk suspension until the pH of the suspension drops to 8 to obtain a calcium carbonate suspension;

[0042] 3. Weigh the nano calcium carbonate prepared in step 1, add water and ultrasonically disperse for 10 min at an ultrasonic dispersion power of 800 W, then add it to the calcium carbonate suspension prepared in step 2, stir for 0.5 h, centrifuge, discard the upper liquid, and dry it at 120 ° C for 2 h to obtain the modified calcium carbonate filler prepared in Example 2.

[0043] Example 3

[0044] Example 3 provides a method for preparing a modified calcium carbonate filler for a non-expanding fire retardant coating, the steps are as follows:

[0045] 1. Take 1kg of micron-grade calcium carbonate powder, add 8kg of zirconium oxide balls, and place them in a ball mill. The particle size of the zirconium oxide balls is 0.2mm; take 125g of polyethylene glycol aqueous solution and add it to the ball mill, wherein the polyethylene glycol aqueous solution is made of polyethylene glycol 200 and water in a weight ratio of 1:50, fill the ball mill with nitrogen, seal the ball mill, and grind it at a grinding rate of 800r / min for 2h. After grinding, use liquid nitrogen atmosphere for rapid cooling, and then perform secondary grinding. The secondary grinding rate is 2000r / min, and the grinding time is 30min. After grinding, quickly place it in liquid nitrogen atmosphere for cooling; after cooling, take out the zirconium oxide balls, and dry the ground sample at 110℃ for 3h; then take the dried powder and spread it flat, and perform single-pass laser irradiation treatment, the laser power is 80W, and the scanning speed is 8mm / s;

[0046] 2. Take 1.2 kg of quicklime and add 1.2 kg of water to obtain a lime milk suspension; introduce CO2 gas into the lime milk suspension until the pH of the suspension drops to 8 to obtain a calcium carbonate suspension;

[0047] 3. Weigh the nano calcium carbonate prepared in step 1, add water and ultrasonically disperse for 20 min at an ultrasonic dispersion power of 500 W, then add it to the calcium carbonate suspension prepared in step 2, stir for 2 h, centrifuge, discard the upper liquid, and dry it at 110 ° C for 3 h to obtain the modified calcium carbonate filler prepared in Example 3.

[0048] Example 4

[0049] Example 4 provides a method for preparing a modified calcium carbonate filler for a non-expanding fire retardant coating, the steps being as follows:

[0050] 1. Take 1kg of micron-grade calcium carbonate powder, add 6kg of steel balls, and place in a ball mill, the particle size of the steel balls is 0.2mm; take 167g of polyethylene glycol aqueous solution and add it to the ball mill, wherein the polyethylene glycol aqueous solution is made of polyethylene glycol 200 and water in a weight ratio of 3:100, fill the ball mill with nitrogen, seal the ball mill and grind it, the grinding rate is 600r / min, the time is 2.5h, after grinding, use liquid nitrogen atmosphere for rapid cooling, and then perform secondary grinding, the secondary grinding rate is 1800r / min, the grinding time is 35min, after grinding, quickly put it in liquid nitrogen atmosphere for cooling; after cooling, take out the steel balls, and dry the ground sample at 100℃ for 2h; then take the dried powder and spread it flat, and perform single-pass laser irradiation treatment, the laser power is 100W, and the scanning speed is 8mm / s;

[0051] 2. Take 1 kg of quicklime and add 1 kg of water to obtain a lime milk suspension; introduce CO2 gas into the lime milk suspension until the pH of the suspension drops to 7.5 to obtain a calcium carbonate suspension;

[0052] 3. Weigh the nano calcium carbonate prepared in step 1, add water and ultrasonically disperse for 25 min at an ultrasonic dispersion power of 600 W, then add it to the calcium carbonate suspension prepared in step 2, stir for 1.5 h, centrifuge, discard the upper liquid, and dry it at 100 ° C for 1 h to obtain the modified calcium carbonate filler prepared in Example 4.

[0053] Comparative Example 1

[0054] Comparative Example 1 provides a method for preparing a modified calcium carbonate filler for a non-expanding fire retardant coating, the steps being as follows:

[0055] Take 1kg of micron-sized calcium carbonate powder, add 8kg of zirconium oxide balls, and place them in a ball mill, wherein the particle size of the zirconium oxide balls is 0.2mm; take 125g of ethanol aqueous solution and add it to the ball mill, wherein the ethanol aqueous solution is made of anhydrous ethanol and water in a weight ratio of 1:50, fill the ball mill with nitrogen, seal the ball mill and grind it, the grinding rate is 800r / min, the time is 2h, after the grinding, use liquid nitrogen atmosphere for rapid cooling, and then perform secondary grinding, the secondary grinding rate is 2000r / min, the grinding time is 30min, after the grinding, quickly put it into liquid nitrogen atmosphere for cooling; after the cooling, take out the zirconium oxide balls, and dry the ground sample at 110°C for 3h; then take the dried powder and spread it flat, and perform a single-pass laser irradiation treatment, the laser power is 80W, and the scanning speed is 8mm / s, that is, compared with Example 3, the wet ball milling additive polyethylene glycol aqueous solution is replaced by ethanol aqueous solution, and the other materials, proportions and preparation steps are not changed.

[0056] Comparative Example 2

[0057] Comparative Example 2 provides a method for preparing a modified calcium carbonate filler for a non-expanding fire retardant coating, the steps are as follows:

[0058] Take 1kg of micron-grade calcium carbonate powder, add 8kg of zirconium oxide balls, and place them in a ball mill, wherein the particle size of the zirconium oxide balls is 0.2mm; take 125g of polyethylene glycol aqueous solution and add it to the ball mill, wherein the polyethylene glycol aqueous solution is prepared by polyethylene glycol 200 and water in a weight ratio of 1:50, fill the ball mill with nitrogen, seal the ball mill and grind it, the grinding rate is 800r / min, the time is 2h, and liquid nitrogen atmosphere is used for rapid cooling after grinding, the zirconium oxide balls are taken out after cooling, and the ground sample is dried at 110°C for 3h; then the dried powder is spread out and subjected to single-pass laser irradiation treatment, the laser power is 80W, and the scanning speed is 8mm / s; that is, compared with Example 3, secondary grinding and liquid nitrogen cooling are not performed, and the remaining materials, proportions and preparation steps are not changed.

[0059] Comparative Example 3

[0060] Comparative Example 3 provides a method for preparing a modified calcium carbonate filler for a non-expanding fire retardant coating, the steps are as follows:

[0061] Take 1kg of micron-grade calcium carbonate powder, add 8kg of zirconium oxide balls, and place them in a ball mill, wherein the particle size of the zirconium oxide balls is 0.2mm; take 125g of polyethylene glycol aqueous solution and add it to the ball mill, wherein the polyethylene glycol aqueous solution is made of polyethylene glycol 200 and water in a weight ratio of 1:50, fill the ball mill with nitrogen, seal the ball mill and grind it, the grinding rate is 800r / min, the time is 2h, after the grinding is completed, use liquid nitrogen atmosphere for rapid cooling, and then perform secondary grinding, the secondary grinding rate is 2000r / min, the grinding time is 30min, and after the grinding is completed, quickly put it into liquid nitrogen atmosphere for cooling; after the cooling is completed, take out the zirconium oxide balls, and dry the ground sample at 110°C for 3h; that is, compared with Example 3, no single-pass laser irradiation treatment is performed, and the remaining materials, proportions and preparation steps are not changed.

[0062] Comparative Example 4

[0063] Comparative Example 4 provides a method for preparing a modified calcium carbonate filler for a non-expandable fire retardant coating, the steps are as follows:

[0064] Take 1kg of micron-sized calcium carbonate powder, add 8kg of zirconium oxide balls, and place them in a ball mill, wherein the particle size of the zirconium oxide balls is 0.2mm; take 125g of ethanol aqueous solution and add it to the ball mill, wherein the polyethylene glycol aqueous solution is made of polyethylene glycol 200 and water in a weight ratio of 1:50, fill the ball mill with nitrogen, seal the ball mill and grind it, the grinding rate is 800r / min, the time is 2h, after the grinding, use 0℃ ice-water mixture to cool, and then perform secondary grinding, the secondary grinding rate is 2000r / min, the grinding time is 30min, after the grinding, quickly put it into the atmosphere of 0℃ ice-water mixture to cool; after the cooling, take out the zirconium oxide balls, and dry the ground sample at 110℃ for 3h; then take the dried powder and spread it flat, and perform laser irradiation treatment, the laser power is 80W, and the scanning speed is 8mm / s, that is, compared with Example 3, the cooling method is replaced by 0℃ ice-water mixture cooling from liquid nitrogen cooling, and the other materials, proportions and preparation steps are not changed.

[0065] Comparative Example 5

[0066] The difference between the preparation method of a modified calcium carbonate filler for a non-expanding fire retardant coating provided in Comparative Example 5 and Example 3 is that the particle size of the zirconium oxide ball is 0.4 mm, and the other materials, proportions and preparation steps remain unchanged.

[0067] Comparative Example 6

[0068] The difference between the preparation method of a modified calcium carbonate filler for a non-expanding fire retardant coating provided in Comparative Example 6 and Example 3 is that the particle size of the zirconium oxide ball is 0.08 mm, and the other materials and proportion preparation steps are unchanged.

[0069] Comparative Example 7

[0070] Comparative Example 7 provides a method for preparing nano calcium carbonate, which differs from Example 3 in that only step 1 is implemented to prepare nano calcium carbonate.

[0071] Comparative Example 8

[0072] Comparative Example 8 provides a method for preparing a traditional calcium carbonate filler, which differs from Example 3 in that only step 2 is implemented to prepare a calcium carbonate suspension, centrifuge, discard the upper liquid, put it in an oven at 110° C. and dry it for 3 hours to obtain calcium carbonate powder.

[0073] Test Example 1: Dispersion performance test of modified calcium carbonate filler for non-expandable fire retardant coating prepared by the method of the present invention

[0074] The corresponding modified calcium carbonate filler was prepared by the preparation methods of Examples 1 to 4 and Comparative Examples 1 to 8 of the present invention, 2.0 g was weighed respectively, placed in a 250 mL beaker, 80 mL of first-grade water was added to the beaker, and stirred at a speed of 1000 r / min at 25° C. for 30 min to obtain a suspension. The suspensions prepared above were allowed to stand for 30 min respectively, and 5 mL of the upper suspension was taken after standing with a pipette, and the volume was fixed to 100 mL with first-grade water, and shaken well; 3 parallel samples were taken, placed in a cuvette, and placed in a spectrophotometer to determine the transmittance of the solution at a wavelength of 550 m, and the transmittance of the 3 parallel samples was recorded respectively, and the average transmittance was calculated and recorded.

[0075] Table 1 Dispersibility test results of modified calcium carbonate filler for non-expandable fire retardant coating prepared by the method of the present invention

[0076] Examples or Comparative Examples Average light transmittance (%) Example 1 38.3 Example 2 35.7 Example 3 34.2 Example 4 35.1 Comparative Example 1 47.8 Comparative Example 2 50.4 Comparative Example 3 46.3 Comparative Example 4 44.8 Comparative Example 5 51.5 Comparative Example 6 52.7 Comparative Example 7 33.4 Comparative Example 8 61.3

[0077] Test Example 2 Performance test of fire retardant coating using modified calcium carbonate filler prepared by the method of the present invention

[0078] The corresponding modified calcium carbonate fillers and the fillers of Comparative Examples 7 and 8 were prepared by the preparation methods of Examples 1 to 4 and Comparative Examples 1 to 6 of the present invention, and non-expanding fire retardant coatings were prepared according to the formula in Table 2 below. The prepared fire retardant coatings were subjected to performance tests, including substrate adhesion strength test and fire resistance test.

[0079] Table 2 Mixing ratio of non-expanding fire retardant coating

[0080] raw material Number of copies 42.5 Ordinary Portland cement 200 Anhydrous sodium sulfate 50 Japan Nopco NXZ defoamer 3 water 1150 Vinyl acetate-ethylene copolymer emulsion 400 Calcium carbonate-based filler prepared in the present invention / comparative example 500

[0081] 42.5 ordinary Portland cement, anhydrous sodium sulfate and the calcium carbonate-based filler powder prepared in the embodiment / comparative example of the present invention in the formula of Table 2 are added into a mixer and mixed evenly, and then water and vinyl acetate-ethylene copolymer emulsion are stirred evenly, poured into the mixed powder, stirred at a speed of 200 r / min for 5 minutes, and then NXZ defoamer is added and stirred for 2 minutes to prepare a non-expanding fire retardant coating containing the calcium carbonate-based filler in the embodiment / comparative example of the present invention.

[0082] Bond strength test: The bonding strength of the non-expanding fire retardant coating is tested using the GB 14907-2018 steel structure fire retardant coating standard. The specific test method is to pour the prepared non-expanding fire retardant coating in the middle of the steel sheet substrate. The size of the steel sheet is 70mm×70mm×6mm, and the size of the fire retardant coating poured in the middle is 40mm×40mm×15mm. After pouring, it is cured for 28 days according to the conditions specified in the standard. Then, apply high-adhesive E12 epoxy resin in the 40mm×40mm area in the center of the coating, and then stick the steel connector and press it with a 1kg weight. Carefully remove the adhesive overflowing around the connector, and continue to cure for 3 days according to the standard requirements. Remove the weight, cut the coating along the periphery of the steel connector to the bottom surface of the plate, and then install the bonded specimen on the universal material testing machine, apply tension in the vertical direction along the bottom plate of the specimen, and apply load at a speed of 2000N / minN / min until the specimen is destroyed, and record the maximum load when the specimen is destroyed. The bonding strength is calculated according to the standard formula, and the unit is expressed in MPa.

[0083] Fire resistance test: The specific test method is to pour the prepared non-expanding fire retardant coating in the middle of the steel sheet substrate. The size of the steel sheet is 70mm×70mm×6mm, the coating thickness is 15mm, and it is cured for 28 days in accordance with the GB 14907-2018 standard for steel structure fire retardant coatings. After the curing, the sample is placed on the iron frame with the coating facing down. An alcohol blowtorch is placed under the iron frame with the flame nozzle 10cm away from the coating surface. The temperature sensor is attached to the back of the steel sheet and connected to the temperature patrol meter through a wire to record the temperature change on the back of the steel sheet. The time required for the temperature on the back of the steel sheet to rise from 25°C to 250°C is recorded as the fire resistance time of the coating, expressed in min.

[0084] Table 3 Performance test of fillers prepared by the methods of the present invention / comparative examples for non-expanding fire retardant coatings

[0085] Examples or Comparative Examples Adhesion strength (MPa) Refractory time (min) Example 1 0.93 32.3 Example 2 0.92 31.2 Example 3 0.96 33.8 Example 4 0.91 30.6 Comparative Example 1 0.71 20.2 Comparative Example 2 0.75 22.9 Comparative Example 3 0.76 21.5 Comparative Example 4 0.82 24.3 Comparative Example 5 0.77 23.0 Comparative Example 6 0.80 23.7 Comparative Example 7 0.89 25.6 Comparative Example 8 0.48 16.3

[0086] It can be obtained from the dispersion performance test of Table 1 that the modified calcium carbonate filler for non-expanding fire retardant coating prepared by the method of the present invention has excellent dispersion performance, and Example 3 is the best embodiment method of the present invention. Except for Comparative Example 7, the calcium carbonate fillers prepared by the implementation methods of the other comparative examples are not as good as the present invention. The difference between Comparative Example 7 and Example 3 is that the difference between Example 3 and Example 3 is that only step 1 is implemented, that is, nano calcium carbonate is prepared. This may be because the filler prepared in Comparative Example 7 is nano-scale, so the dispersion performance will be better, but combined with Table 3, it can be obtained that the method of the embodiment / comparative example is used to prepare a non-expanding fire retardant coating. The nano calcium carbonate filler of Comparative Example 7 is applied to the fire retardant coating, and its fire resistance is not as good as the present invention. This is because the modified calcium carbonate filler prepared by the method of the present invention is a nano calcium carbonate filler wrapped with calcium carbonate. Therefore, during the high-temperature combustion process, part of the calcium carbonate filler in the coating can release more carbon dioxide gas to isolate the air and continue to burn, and the decomposition process of calcium carbonate is an endothermic reaction, and the surface temperature can be further reduced during the decomposition process, thereby achieving a better fire retardant effect.

[0087] The modified calcium carbonate filler prepared by the method of the present invention is prepared into nano calcium carbonate by adding polyethylene glycol, grinding and cooling for many times and pre-treating with laser irradiation, so that more free radicals are formed on the surface of the nano calcium carbonate; then calcium carbonate is generated by a bubbling method, and the nano calcium carbonate obtained after the pre-treatment is added thereto to prepare a modified calcium carbonate filler in which the nano calcium carbonate is wrapped by calcium carbonate. The particle size of the obtained modified calcium carbonate filler is more uniform, and the dispersion performance of the filler is improved. When applied to a non-expanding fire retardant coating, the defect of poor bonding strength in the non-expanding fire retardant coating can be improved, and the fire resistance of the non-expanding fire retardant coating is improved.

[0088] The above shows and describes the basic principles, main features and advantages of the present invention. Those skilled in the art should understand that the present invention is not limited to the above embodiments, and the above embodiments and descriptions are only for explaining the principles of the present invention. Without departing from the spirit and scope of the present invention, the present invention may have various changes and improvements, and these changes and improvements all fall within the scope of the present invention to be protected.

Claims

1. A method for preparing a modified calcium carbonate filler for a non-expanding fire retardant coating, characterized in that: The following steps are involved: S1. Preparation of nano calcium carbonate: calcium carbonate powder is taken, ball milling medium is added, and the powder is placed in a ball mill; polyethylene glycol aqueous solution is added to the ball mill, inert gas is filled in, and the ball mill is sealed; grinding is performed once, cooling is performed once; grinding is performed twice, and cooling is performed twice; the ball milling medium is separated after taking out, and the powder is dried; the dried powder is spread flat, and laser irradiation treatment is performed; S2. Preparation of calcium carbonate suspension: Take quicklime and add water to obtain lime milk suspension; introduce CO2 gas into the lime milk suspension until the pH of the suspension drops to 7.5-8 to obtain calcium carbonate suspension; S3. Preparation of modified calcium carbonate filler: weigh the nano calcium carbonate described in step S1, add water to ultrasonically disperse it, add it to the calcium carbonate suspension described in step S2, stir, centrifuge, and dry to obtain a modified calcium carbonate filler.

2. The method for preparing a modified calcium carbonate filler for non-expandable fire retardant coating according to claim 1, characterized in that: The weight ratio of the calcium carbonate powder to the polyethylene glycol aqueous solution is 5-10:1, and the weight ratio of the calcium carbonate powder to the ball milling medium is 1:5-10.

3. The method for preparing a modified calcium carbonate filler for non-expandable fire retardant coating according to claim 1, characterized in that: The polyethylene glycol is polyethylene glycol 200, and the weight ratio of polyethylene glycol 200 to water in the polyethylene glycol aqueous solution is 1 to 4:

100.

4. The method for preparing a modified calcium carbonate filler for non-expandable fire retardant coating according to claim 1, characterized in that: The ball milling medium in step S1 is one or a combination of zirconia balls or steel balls.

5. The method for preparing a modified calcium carbonate filler for non-expandable fire retardant coating according to claim 1, characterized in that: The inert gas is nitrogen or argon.

6. The method for preparing a modified calcium carbonate filler for non-expandable fire retardant coating according to claim 1, characterized in that: In the step S1, the grinding rate of the first grinding process is 500-1000 r / min, and the grinding time is 1-3 hours. The grinding rate of the second grinding process is 1500-2500 r / min, and the grinding time is 20-40 minutes.

7. The method for preparing a modified calcium carbonate filler for non-expandable fire retardant coating according to claim 1, characterized in that: The primary cooling and secondary cooling in step S1 are both liquid nitrogen cooling.

8. The method for preparing a modified calcium carbonate filler for non-expandable fire retardant coating according to claim 1, characterized in that: The drying temperature in steps S1 and S3 is 80-120° C., and the drying time is 2-4 hours.

9. The method for preparing a modified calcium carbonate filler for non-expandable fire retardant coating according to claim 1, wherein the laser irradiation treatment conditions in step S1 are: laser power is 40 to 100 W, and scanning speed is 5 to 10 mm / s.

10. Modified calcium carbonate filler for non-expanding fire retardant coating prepared according to the preparation method according to any one of claims 1 to 9.

Citation Information

Cited By

  • Preparation method and application of heavy calcium carbonate powder with high oil absorption value

    CN120665456A

  • Preparation method and application of high oil absorption value heavy calcium carbonate powder

    CN120665456B