Preparation method of super-hydrophobic anticorrosive paint with double dynamic covalent bonds
By constructing dynamic disulfide bonds on the surface of graphene and carbon nanotubes and using a curing agent containing dynamic ester bonds, a super-hydrophobic anti-corrosion coating with double dynamic covalent bonds was prepared, which solved the problem of easy corrosion of grounding grid materials and achieved The self-healing and recyclable performance of the coating improves the anti-corrosion performance and safety of the grounding grid.
Patent Information
- Application Number
- CN202411015758.2
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-07-26
- Publication Date
- 2024-10-29
AI Technical Summary
Existing grounding grid materials are susceptible to corrosion in the soil environment, resulting in performance degradation and possible safety accidents. Moreover, traditional coatings lack long-lasting and environmentally friendly properties.
Construct dynamic disulfide bonds on the surface of graphene and carbon nanotubes, and use a curing agent containing dynamic ester bonds to prepare a super-hydrophobic anti-corrosion coating with double dynamic covalent bonds. Through steps such as ultrasonic treatment and magnetic stirring, an excellent self-healing and Recyclable coating.
The long-lasting work and green and environmentally friendly performance of the super-hydrophobic coating are achieved, and the anti-corrosion performance and safety of the grounding grid are significantly improved.
Smart Images

Figure CN118852947A_ABST
Abstract
Description
Technical Field
[0001] The invention belongs to the technical field of grounding grid anti-corrosion, and specifically relates to a method for preparing a super hydrophobic anti-corrosion coating with double dynamic covalent bonds. Background Art
[0002] The grounding grid plays a vital role in power facilities, and its primary task is to protect the safety of personnel and other equipment. As the power system continues to develop towards higher voltage and larger capacity, the requirements for system operation safety and reliability are also increasing, and the demand for grounding grid performance is also gradually increasing. At present, my country usually uses ordinary carbon steel to build grounding grids, but this material is easily affected by soil environmental corrosion, resulting in a decrease in the performance of the grounding grid, or even failure to operate normally, which may cause serious accidents.
[0003] When the surface can show the characteristics of water contact angle>150° and rolling angle<10° during characterization test, it is considered that the surface has superhydrophobic properties, and the superhydrophobic effect can play an anti-icing role. In order to achieve long-term operation and green environmental protection of the coating, the present invention constructs dynamic disulfide bonds on the surface of graphene and carbon nanotubes, and selects a curing agent containing dynamic ester bonds to cure the coating to prepare a superhydrophobic anticorrosive coating with excellent self-healing and recyclable properties. Summary of the invention
[0004] The object of the present invention is to provide a method for preparing a super hydrophobic anticorrosive coating with double dynamic covalent bonds.
[0005] A method for preparing a super hydrophobic anticorrosive coating having dual dynamic covalent bonds comprises the following steps:
[0006] (1) Dissolving 1-3 parts of a disulfide bond modifier in 80-100 parts of ethanol and 8-12 parts of deionized water according to weight, adding glacial acetic acid to the solution to adjust the pH to 4, and then ultrasonically treating the solution for 10-14 hours to obtain a modifier dispersion;
[0007] (2) placing 0.5-1.5 parts of graphene or carbon nanotubes in 8-12 parts of ethanol solution and ultrasonically treating for 1-3 hours to obtain a graphene or carbon nanotube dispersion;
[0008] (3) adding the graphene or carbon nanotube dispersion to the modifier dispersion, reflux at 70-90° C. for 4-8 hours, and then magnetically stirring for 1-3 hours, and finally centrifuging, washing, drying and grinding the solution to obtain graphene or carbon nanotubes with dynamic disulfide bonds on the surface;
[0009] (4) adding 30-50 parts of ethanol and 0.5-2 parts of a fluorosilane modifier to 4-6 parts of graphene or carbon nanotubes containing dynamic disulfide bonds on the surface, stirring until the mixture is uniformly dispersed, and then repeating ultrasonic treatment and stirring for 3-8 times and drying to obtain fluorosilane-modified graphene or carbon nanotubes containing dynamic disulfide bonds;
[0010] (5) mixing 3-7 parts of epoxy resin stock solution with 15-25 parts of organic solvent, and stirring with 1-3 parts of fluorosilane-modified graphene containing dynamic disulfide bonds until the mixture is uniform, to obtain an anti-corrosion coating component A;
[0011] (6) mixing 1-3 parts of a curing agent containing a dynamic ester bond with 10-20 parts of an organic solvent, adding 3-7 parts of fluorinated modified carbon nanotubes containing disulfide bonds and stirring until the mixture is uniform, thereby obtaining an anticorrosive coating component B;
[0012] (7) The anti-corrosion coating component A and the anti-corrosion coating component B are mixed in a weight ratio of 1:(0.5-2) and stirred evenly to obtain a super hydrophobic anti-corrosion coating.
[0013] The disulfide bond-containing modifier is bis(triethoxysilylpropyl) disulfide.
[0014] The fluorosilane modifier is tridecafluorooctyltriethoxysilane and / or heptadecafluorodecyltriethoxysilane.
[0015] The curing agent containing dynamic ester bonds is methyl hexahydrophthalic anhydride.
[0016] The carbon nanotubes have a length of 5-50 μm.
[0017] The organic solvent is ethyl acetate and / or butyl acetate.
[0018] The ultrasonic treatment and stirring are ultrasonic treatment for 10-20 minutes followed by glass rod stirring or magnetic stirring for 10-20 minutes; the sufficient stirring is glass rod stirring or magnetic stirring for 30-50 minutes; and the uniform stirring is glass rod or magnetic stirring for 5-10 minutes.
[0019] The prepared super-hydrophobic anti-corrosion coating is sprayed on a substrate and cured at room temperature to obtain a super-hydrophobic anti-corrosion coating with self-repairing function.
[0020] The substrate is one or more of metal, ceramic, glass, fiber and plastic.
[0021] The spray coating amount is 0.02-0.05 mL / cm 2 .
[0022] Beneficial effects of the present invention: The present invention prepares a super hydrophobic anti-corrosion coating with excellent self-repairing and recyclable properties by constructing dynamic disulfide bonds on the surfaces of graphene and carbon nanotubes and selecting a curing agent containing dynamic ester bonds to cure the coating. BRIEF DESCRIPTION OF THE DRAWINGS
[0023] Figure 1 This is a scanning electron microscope image of Example 1. DETAILED DESCRIPTION
[0024] In order to better explain the present invention, it will be described in more detail. However, it should be noted that the present invention is not limited to the embodiments mentioned herein, but can be implemented in a variety of different forms. Therefore, the embodiments provided herein are only intended to more fully disclose the content of the present invention, rather than to limit its implementation.
[0025] Example 1
[0026] A method for preparing a super hydrophobic anti-corrosion coating with self-repairing function comprises the following steps:
[0027] (1) Dissolve 2 parts of bis(triethoxysilylpropyl) disulfide in 90 parts of ethanol and 10 parts of deionized water according to weight; add an appropriate amount of glacial acetic acid to the solution until the pH is 4, and then treat the solution with ultrasound for 12 hours to obtain a modifier dispersion;
[0028] (2) placing 1 part of graphene in 10 parts of ethanol solution and ultrasonically treating for 2 hours to ensure uniform dispersion, thereby obtaining a graphene dispersion, adding the graphene dispersion to the modifier dispersion, reflux treating (80° C., 6 h) and then magnetically stirring for 2 hours, and finally centrifuging, washing, drying and grinding the solution to obtain graphene with dynamic disulfide bonds on the surface;
[0029] (3) placing 1 part of carbon nanotubes (length 15 μm) into 10 parts of ethanol solution and ultrasonically treating for 2 hours to ensure uniform dispersion, thereby obtaining a carbon nanotube dispersion; adding the carbon nanotube dispersion to the modifier dispersion, reflux treatment (80° C., 6 h) and magnetic stirring for 2 hours, and finally centrifuging, washing, drying and grinding the solution to obtain carbon nanotubes with dynamic disulfide bonds on the surface;
[0030] (4) adding 50 parts of ethanol and 1 part of tridecafluorooctyltriethoxysilane to 5 parts of graphene containing dynamic disulfide bonds on the surface, stirring until uniformly dispersed, repeating ultrasonic treatment and stirring and drying for 8 times to obtain fluorosilane-modified graphene containing dynamic disulfide bonds;
[0031] (5) adding 50 parts of ethanol and 1 part of tridecafluorooctyltriethoxysilane to 5 parts of carbon nanotubes containing dynamic disulfide bonds, stirring thoroughly until the mixture is evenly dispersed, and then repeating ultrasonic treatment and stirring for 8 times and drying to obtain fluorosilane-modified carbon nanotubes containing dynamic disulfide bonds;
[0032] (6) Mixing 2 parts of epoxy resin stock solution with 15 parts of ethyl acetate, adding 1 part of fluorosilane-modified graphene containing dynamic disulfide bonds, and stirring until the mixture is uniform, thereby obtaining an anti-corrosion coating component A;
[0033] (7) 2 parts of methyl hexahydrophthalic anhydride and 15 parts of ethyl acetate were mixed, and 3 parts of fluorinated modified carbon nanotubes containing disulfide bonds were added and stirred until the mixture was uniform, thereby obtaining an anti-corrosion coating component B;
[0034] (8) mixing the anti-corrosion coating component A and the anti-corrosion coating component B in a weight ratio of 1:1 and stirring evenly to obtain a super hydrophobic anti-corrosion coating;
[0035] The ultrasonic treatment and stirring are ultrasonic treatment for 12 minutes followed by glass rod stirring or magnetic stirring for 12 minutes; the sufficient stirring is glass rod stirring or magnetic stirring for 35 minutes; and the uniform stirring is glass rod or magnetic stirring for 6 minutes.
[0036] A super hydrophobic anti-corrosion coating with a self-repairing function, wherein the super hydrophobic anti-corrosion coating prepared above is sprayed on a ceramic substrate, and cured at room temperature to obtain a super hydrophobic anti-corrosion coating with a self-repairing function; the coating amount of the spraying is 0.02 mL / cm 2 .
[0037] Example 2
[0038] A method for preparing a super hydrophobic anti-corrosion coating with self-repairing function comprises the following steps:
[0039] (1) Dissolve 2 parts of bis(triethoxysilylpropyl) disulfide in 90 parts of ethanol and 10 parts of deionized water according to weight; add an appropriate amount of glacial acetic acid to the solution until the pH is 4, and then treat the solution with ultrasound for 12 hours to obtain a modifier dispersion;
[0040] (2) placing 1 part of graphene in 10 parts of ethanol solution and ultrasonically treating for 2 hours to ensure uniform dispersion, thereby obtaining a graphene dispersion, adding the graphene dispersion to the modifier dispersion, reflux treating (80° C., 6 h) and then magnetically stirring for 2 hours, and finally centrifuging, washing, drying and grinding the solution to obtain graphene with dynamic disulfide bonds on the surface;
[0041] (3) placing 1 part of carbon nanotubes (length 25 μm) into 10 parts of ethanol solution and ultrasonically treating for 2 hours to ensure uniform dispersion, thereby obtaining a carbon nanotube dispersion; adding the carbon nanotube dispersion to the modifier dispersion, reflux treatment (80° C., 6 h) and magnetic stirring for 2 hours, and finally centrifuging, washing, drying and grinding the solution to obtain carbon nanotubes with dynamic disulfide bonds on the surface;
[0042] (4) adding 50 parts of ethanol and 1 part of heptadecafluorodecyltriethoxysilane to 5 parts of graphene containing dynamic disulfide bonds on the surface, stirring thoroughly until the mixture is evenly dispersed, repeating ultrasonic treatment and stirring for 8 times and then drying to obtain fluorosilane-modified graphene containing dynamic disulfide bonds;
[0043] (5) adding 50 parts of ethanol and 1 part of heptadecafluorodecyltriethoxysilane to 5 parts of carbon nanotubes containing dynamic disulfide bonds, stirring until uniformly dispersed, repeating ultrasonic treatment and stirring for 8 times and then drying to obtain fluorosilane-modified carbon nanotubes containing dynamic disulfide bonds;
[0044] (6) Mixing 3 parts of epoxy resin stock solution with 20 parts of ethyl acetate, adding 2 parts of fluorosilane-modified graphene containing dynamic disulfide bonds, and stirring until the mixture is uniform, thereby obtaining an anti-corrosion coating component A;
[0045] (7) Mixing 1 part of methyl hexahydrophthalic anhydride with 10 parts of ethyl acetate, adding 5 parts of fluorinated modified carbon nanotubes containing disulfide bonds, and stirring thoroughly until the mixture is uniform, thereby obtaining an anticorrosive coating component B;
[0046] (8) mixing the anti-corrosion coating component A and the anti-corrosion coating component B in a weight ratio of 1:2 and stirring evenly to obtain a super hydrophobic anti-corrosion coating;
[0047] The ultrasonic treatment and stirring are ultrasonic treatment for 15 minutes followed by glass rod stirring or magnetic stirring for 15 minutes; the sufficient stirring is glass rod stirring or magnetic stirring for 40 minutes; and the uniform stirring is glass rod or magnetic stirring for 8 minutes.
[0048] A super hydrophobic anti-corrosion coating with a self-repairing function, wherein the super hydrophobic anti-corrosion coating prepared above is sprayed on a stainless steel substrate, and cured at room temperature to obtain a super hydrophobic anti-corrosion coating with a self-repairing function; the coating amount of the spraying is 0.03 mL / cm 2 .
[0049] Example 3
[0050] A method for preparing a super hydrophobic anti-corrosion coating with self-repairing function comprises the following steps:
[0051] (1) Dissolve 2 parts of bis(triethoxysilylpropyl) disulfide in 90 parts of ethanol and 10 parts of deionized water according to weight; add an appropriate amount of glacial acetic acid to the solution until the pH is 4, and then treat the solution with ultrasound for 12 hours to obtain a modifier dispersion;
[0052] (2) placing 1 part of graphene in 10 parts of ethanol solution and ultrasonically treating for 2 hours to ensure uniform dispersion, thereby obtaining a graphene dispersion, adding the graphene dispersion to the modifier dispersion, reflux treating (80° C., 6 h) and then magnetically stirring for 2 hours, and finally centrifuging, washing, drying and grinding the solution to obtain graphene with dynamic disulfide bonds on the surface;
[0053] (3) placing 1 part of carbon nanotubes (length 50 μm) into 10 parts of ethanol solution and ultrasonically treating for 2 hours to ensure uniform dispersion, thereby obtaining a carbon nanotube dispersion; adding the carbon nanotube dispersion to the modifier dispersion, reflux treatment (80° C., 6 h) and magnetic stirring for 2 hours, and finally centrifuging, washing, drying and grinding the solution to obtain carbon nanotubes with dynamic disulfide bonds on the surface;
[0054] (4) adding 40 parts of ethanol and 2 parts of heptadecafluorodecyltriethoxysilane to 6 parts of graphene containing dynamic disulfide bonds on the surface, stirring until uniformly dispersed, repeating ultrasonic treatment and stirring and drying for 6 times to obtain fluorosilane-modified graphene containing dynamic disulfide bonds;
[0055] (5) adding 6 parts of carbon nanotubes containing dynamic disulfide bonds to 40 parts of ethanol and 1 part of heptadecafluorodecyltriethoxysilane, stirring until uniformly dispersed, repeating ultrasonic treatment and stirring for 6 times and then drying to obtain fluorosilane-modified carbon nanotubes containing dynamic disulfide bonds;
[0056] (6) Mix 5 parts of epoxy resin stock solution with 25 parts of butyl acetate, add 3 parts of fluorosilane-modified graphene containing dynamic disulfide bonds, and stir until the mixture is uniform to obtain an anti-corrosion coating component A;
[0057] (7) 3 parts of methyl hexahydrophthalic anhydride and 20 parts of butyl acetate were mixed, and 7 parts of fluorinated modified carbon nanotubes containing disulfide bonds were added and stirred until the mixture was uniform, thereby obtaining an anti-corrosion coating component B;
[0058] (8) mixing the anti-corrosion coating component A and the anti-corrosion coating component B in a weight ratio of 2:1 and stirring evenly to obtain a super hydrophobic anti-corrosion coating;
[0059] The ultrasonic treatment and stirring are ultrasonic treatment for 18 minutes followed by glass rod stirring or magnetic stirring for 18 minutes; the sufficient stirring is glass rod stirring or magnetic stirring for 45 minutes; and the uniform stirring is glass rod or magnetic stirring for 8 minutes.
[0060] A super hydrophobic anti-corrosion coating with a self-repairing function, wherein the super hydrophobic anti-corrosion coating prepared above is sprayed on a plastic substrate, and cured at room temperature to obtain a super hydrophobic anti-corrosion coating with a self-repairing function; the coating amount of the spraying is 0.03 mL / cm 2 .
[0061] Example 4
[0062] A method for preparing a super hydrophobic anti-corrosion coating with self-repairing function comprises the following steps:
[0063] ((1) According to weight proportions, 2 parts of bis(triethoxysilylpropyl) disulfide were dissolved in 90 parts of ethanol and 10 parts of deionized water; an appropriate amount of glacial acetic acid was added to the solution until the pH value was 4, and then the solution was ultrasonically treated for 12 hours to obtain a modifier dispersion;
[0064] (2) placing 1 part of graphene in 10 parts of ethanol solution and ultrasonically treating for 2 hours to ensure uniform dispersion, thereby obtaining a graphene dispersion, adding the graphene dispersion to the modifier dispersion, reflux treating (80° C., 6 h) and then magnetically stirring for 2 hours, and finally centrifuging, washing, drying and grinding the solution to obtain graphene with dynamic disulfide bonds on the surface;
[0065] (3) placing 1 part of carbon nanotubes (length 5 μm) into 10 parts of ethanol solution and ultrasonically treating for 2 hours to ensure uniform dispersion, thereby obtaining a carbon nanotube dispersion; adding the carbon nanotube dispersion to the modifier dispersion, reflux treatment (80° C., 6 h) and magnetic stirring for 2 hours, and finally centrifuging, washing, drying and grinding the solution to obtain carbon nanotubes with dynamic disulfide bonds on the surface;
[0066] (4) adding 35 parts of ethanol and 1.5 parts of tridecafluorooctyltriethoxysilane to 4 parts of graphene containing dynamic disulfide bonds on the surface, stirring until uniformly dispersed, repeating ultrasonic treatment and stirring and drying for 4 times to obtain fluorosilane-modified graphene containing dynamic disulfide bonds;
[0067] (5) adding 4 parts of carbon nanotubes containing dynamic disulfide bonds to 35 parts of ethanol and 1.5 parts of tridecafluorooctyltriethoxysilane, stirring until uniformly dispersed, repeating ultrasonic treatment and stirring and drying for 6 times to obtain fluorosilane-modified carbon nanotubes containing dynamic disulfide bonds;
[0068] (6) 6 parts of epoxy resin stock solution and 25 parts of butyl acetate were mixed, and 2.5 parts of fluorosilane-modified graphene containing dynamic disulfide bonds were added and stirred until the mixture was uniform, thereby obtaining an anti-corrosion coating component A;
[0069] (7) 2.5 parts of methyl hexahydrophthalic anhydride and 20 parts of butyl acetate were mixed, and 6 parts of fluorinated modified carbon nanotubes containing disulfide bonds were added and stirred until the mixture was uniform, thereby obtaining an anticorrosive coating component B;
[0070] (8) mixing the anti-corrosion coating component A and the anti-corrosion coating component B in a weight ratio of 1:1 and stirring evenly to obtain a super hydrophobic anti-corrosion coating;
[0071] The ultrasonic treatment and stirring are ultrasonic treatment for 10-20 minutes followed by glass rod stirring or magnetic stirring for 10-20 minutes; the sufficient stirring is glass rod stirring or magnetic stirring for 30-50 minutes; and the uniform stirring is glass rod or magnetic stirring for 5-10 minutes.
[0072] A super hydrophobic anti-corrosion coating with a self-repairing function, wherein the super hydrophobic anti-corrosion coating prepared above is sprayed on a glass substrate, and cured at room temperature to obtain a super hydrophobic anti-corrosion coating with a self-repairing function; the coating amount of the spraying is 0.05 mL / cm 2 .
[0073] Experimental example:
[0074] The present invention uses a contact angle meter to perform contact angle and rolling angle tests. When performing the contact angle test, the contact angle at the interface between the droplet and the solid-liquid interface is measured. When performing the rolling angle test, the droplet is placed on a solid surface, the solid surface is gradually tilted until the droplet begins to flow, and the rolling angle at this time is measured. Scientifically, a contact angle of >150° and a rolling angle of <10° are defined as a super-hydrophobic surface, and the larger the contact angle and the smaller the rolling angle, the stronger the hydrophobic performance.
[0075] Table 1 Contact angle and rolling angle of the sample in Example 1 after being placed in different pH solutions for 24 hours
[0076] pH 1 3 5 7 9 11 13 Contact Angle 153° 155° 156° 167° 161° 160° 157° Roll Angle 8° 6° 4° 2° 4° 5° 9°
[0077] The polarization current is measured by placing the sample in an electrolytic cell, using platinum as the counter electrode, and using an electrochemical workstation using the Tafel curve method. The smaller the polarization current, the better the anti-corrosion performance.
[0078] Table 2 Comparison of polarization current of samples from different embodiments
[0079] Sample Pure Q235 steel Example 1 Example 2 Example 3 Example 4 Polarization current (A) 0.0009 0.000017 0.000013 0.000016 0.000012
[0080] The above-mentioned embodiments only express several implementation methods of the present invention, and the descriptions thereof are relatively specific and detailed, but they cannot be understood as limiting the scope of the invention patent. It should be pointed out that, for ordinary technicians in this field, several variations and improvements can be made without departing from the concept of the present invention, and these all belong to the protection scope of the present invention. Therefore, the protection scope of the patent of the present invention shall be subject to the attached claims.
Claims
1. A method for preparing a super hydrophobic anticorrosive coating having dual dynamic covalent bonds, characterized in that: The steps include: (1) Dissolving 1-3 parts of a disulfide bond modifier in 80-100 parts of ethanol and 8-12 parts of deionized water according to weight, adding glacial acetic acid to the solution to adjust the pH to 4, and then ultrasonically treating the solution for 10-14 hours to obtain a modifier dispersion; (2) placing 0.5-1.5 parts of graphene or carbon nanotubes in 8-12 parts of ethanol solution and ultrasonically treating for 1-3 hours to obtain a graphene or carbon nanotube dispersion; (3) adding the graphene or carbon nanotube dispersion to the modifier dispersion, reflux at 70-90° C. for 4-8 hours, and then magnetically stirring for 1-3 hours, and finally centrifuging, washing, drying and grinding the solution to obtain graphene or carbon nanotubes with dynamic disulfide bonds on the surface; (4) adding 30-50 parts of ethanol and 0.5-2 parts of a fluorosilane modifier to 4-6 parts of graphene or carbon nanotubes containing dynamic disulfide bonds on the surface, stirring until the mixture is uniformly dispersed, and then repeating ultrasonic treatment and stirring for 3-8 times and drying to obtain fluorosilane-modified graphene or carbon nanotubes containing dynamic disulfide bonds; (5) mixing 3-7 parts of epoxy resin stock solution with 15-25 parts of organic solvent, and stirring with 1-3 parts of fluorosilane-modified graphene containing dynamic disulfide bonds until the mixture is uniform, to obtain an anti-corrosion coating component A; (6) mixing 1-3 parts of a curing agent containing a dynamic ester bond with 10-20 parts of an organic solvent, adding 3-7 parts of fluorinated modified carbon nanotubes containing disulfide bonds and stirring until the mixture is uniform, thereby obtaining an anticorrosive coating component B; (7) The anti-corrosion coating component A and the anti-corrosion coating component B are mixed in a weight ratio of 1:(0.5-2) and stirred evenly to obtain a super hydrophobic anti-corrosion coating.
2. The method for preparing a super hydrophobic anticorrosive coating having dual dynamic covalent bonds according to claim 1, wherein The disulfide bond-containing modifier is bis(triethoxysilylpropyl) disulfide.
3. The preparation method of the super hydrophobic anticorrosive coating with dual dynamic covalent bonds according to claim 1, characterized in that, The fluorosilane modifier is tridecafluorooctyltriethoxysilane and / or heptadecafluorodecyltriethoxysilane.
4. The preparation method of the super hydrophobic anticorrosive coating with dual dynamic covalent bonds according to claim 1, characterized in that, The curing agent containing dynamic ester bonds is methyl hexahydrophthalic anhydride.
5. The preparation method of the super hydrophobic anticorrosive coating with dual dynamic covalent bonds according to claim 1, characterized in that, The carbon nanotubes have a length of 5-50 μm.
6. The preparation method of the super hydrophobic anticorrosive coating with dual dynamic covalent bonds according to claim 1, characterized in that, The organic solvent is ethyl acetate and / or butyl acetate.
7. The method for preparing a super hydrophobic anticorrosive coating having dual dynamic covalent bonds according to claim 1, wherein: The ultrasonic treatment and stirring are ultrasonic treatment for 10-20 minutes followed by glass rod stirring or magnetic stirring for 10-20 minutes; the sufficient stirring is glass rod stirring or magnetic stirring for 30-50 minutes; and the uniform stirring is glass rod or magnetic stirring for 5-10 minutes.
8. A super hydrophobic anti-corrosion coating with self-repairing function, characterized in that: The super hydrophobic anti-corrosion coating prepared in claim 1 is sprayed on a substrate and cured at room temperature to obtain a super hydrophobic anti-corrosion coating with a self-repairing function.
9. The super hydrophobic anticorrosive coating with self-repairing function according to claim 8, characterized in that: The substrate is one or more of metal, ceramic, glass, fiber and plastic.
10. The super hydrophobic anti-corrosion coating with self-repairing function according to claim 8, characterized in that: The spray coating amount is 0.02-0.05 mL / cm 2 .
Citation Information
Patent Citations
Surface modified silicon dioxide particles
CN102027074A
Metal surface in-situ copolymerized multifunctional lubricating layer and preparation method thereof
CN109880486A
Self-repairing in-situ fluorescent tracing type heat-resistant weather-resistant epoxy resin and preparation method thereof
CN111499837A
Preparation method of normal-temperature curing wear-resistant anticorrosive super-hydrophobic coating
CN113913087A
Disulfide bond-containing composite material with high dielectric constant as well as preparation method and application of disulfide bond-containing composite material
CN116120710A
Cited By
Dynamic covalent bond cross-linked I-PDMS / DEA (at) alpha-ZrP-SH self-repairing anti-friction super-hydrophobic anticorrosive paint and preparation method and coating thereof
CN119799158A
Self-repairing finishing varnish and preparation method thereof
CN121160193A
Carbon tube doped self-repairing quick-curing water-based anticorrosive coating and preparation method thereof
CN123042587A