Copper-based catalyst as well as preparation method and application thereof

A copper-based catalyst was prepared by combining co-precipitation or sol-gel method with liquid-phase heat treatment and pyrolysis technology. This solved the problem of deactivation due to thermal sintering of Cu components, improved the stability of the catalyst and methanol selectivity, and achieved efficient CO2 hydrogenation to methanol.

CN118925732APending Publication Date: 2024-11-12TAIYUAN UNIVERSITY OF TECHNOLOGY +1

Patent Information

Application Number
CN202410968836.4
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-07-19
Publication Date
2024-11-12

AI Technical Summary

Technical Problem

Existing copper-based catalysts are prone to thermal sintering and deactivation during the CO2 hydrogenation to methanol process, resulting in insufficient catalytic activity and selectivity, as well as a short catalyst lifetime.

Method used

Copper-based catalyst precursors were prepared by co-precipitation or sol-gel method, and carbon films were formed on the outer layer of the catalyst by liquid-phase heat treatment and pyrolysis technology, using polyethylene glycol or glycerol as heat treatment medium. This avoided thermal aging of active component crystals and formed a highly dispersed state by combining small Cu particles, thereby improving catalytic activity and stability.

Benefits of technology

This improved the thermal stability and methanol selectivity of the catalyst, extended the catalyst's lifespan, and enabled a highly efficient CO2 hydrogenation process for methanol production.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118925732A_ABST
    Figure CN118925732A_ABST
Patent Text Reader

Abstract

The invention belongs to the technical field of catalysts, and particularly relates to a copper-based catalyst and a preparation method and application thereof. The preparation method comprises the following steps: preparing a first precursor from Cu salt, Zn salt and Al salt by adopting a coprecipitation method or a sol-gel method, mixing the first precursor with a heat treatment medium for liquid-phase heat treatment, and the heat treatment medium comprises polyethylene glycol and / or glycerol; and carrying out solid-liquid separation, drying and pyrolysis on the obtained slurry catalyst to obtain the copper-based catalyst. A complete liquid phase method coupling pyrolysis technology is adopted, polyethylene glycol or glycerol is used during liquid phase heat treatment, a carbon film is formed on the outer layer of the catalyst to effectively separate and load active components, free growth of active component grains due to heat aging during use is avoided, and the heat stability of the catalyst is improved. The surface of the catalyst is modified by a heat treatment medium, so that the catalytic activity is further improved, agglomeration is reduced, agglomeration and growth of active components are avoided, and relatively small Cu crystal grains have more open planes and defect / edge sites and show relatively high methanol selectivity.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention belongs to the technical field of catalysts, and in particular relates to a copper-based catalyst and a preparation method and application thereof. Background Art

[0002] CO2 is recognized as the largest greenhouse gas and is primarily responsible for global warming. CO2 hydrogenation to produce methanol is a CCU technology, the main process of which is to combine the hydrogen produced by the dissociation of water with carbon dioxide in the atmosphere through a catalyst to produce methanol. However, CO2 molecules are extremely stable. To achieve the activation and conversion of CO2, the core is still the need to use efficient catalysts to reduce the activation energy barrier of the CO2 reaction. In domestic and foreign research, through the analysis of the thermodynamics and kinetic mechanisms of the reaction process, it is not difficult to find that the key difficulties are mainly concentrated in two aspects: the "seesaw" effect of the activity and selectivity of the catalyst, and the problem of catalyst life.

[0003] The high stability of the catalyst is the key to the smooth and continuous operation of the methanol industry. Existing copper-based catalysts have obvious differences in catalytic activity, service life and selectivity for industrial methanol synthesis catalysts. In the field of catalyst preparation, the composition and ratio of the catalyst are already open and transparent, and the preparation method of the catalyst naturally becomes the main direction for scientific researchers to overcome difficulties; studies have found that different preparation processes will significantly change the structure, phase composition and surface state of the active metal of the catalyst, which in turn has a significant impact on the activity and stability of the catalyst. Therefore, the preparation of methanol synthesis catalysts with high stability and excellent catalytic activity has become a problem that technicians in this field urgently need to solve.

[0004] Cu-based catalysts are currently widely used in the industry to produce methanol from syngas, but Cu is also an active component of the water-gas shift reaction. In CO hydrogenation, this effect can increase the H2 / CO ratio, which is beneficial to the reaction to a certain extent, but in CO2 hydrogenation, it will increase the proportion of CO in the product, thereby reducing the selectivity of methanol. On the other hand, CO selective hydrogenation is an exothermic reaction, and hot spots are easily generated in the catalyst bed, which in turn causes the Cu component to sinter and deactivate the catalyst. Summary of the invention

[0005] In view of this, the purpose of the present invention is to provide a copper-based catalyst and its preparation method and application. The copper-based catalyst obtained by the preparation method of the present invention solves the problem of easy thermal sintering and deactivation of the Cu component, and is applied to CO2 hydrogenation to produce methanol with high methanol selectivity.

[0006] In order to achieve the above-mentioned object of the invention, the present invention provides the following technical solutions:

[0007] The present invention provides a method for preparing a copper-based catalyst, comprising the following steps:

[0008] Prepare a first precursor by using a coprecipitation method or a sol-gel method with Cu salt, Zn salt and Al salt;

[0009] The first precursor and a heat treatment medium are mixed and subjected to liquid phase heat treatment to obtain a slurry catalyst; the heat treatment medium comprises polyethylene glycol and / or glycerol;

[0010] Separating the slurry catalyst from solid to liquid, performing Soxhlet extraction on the obtained solid and then drying it to obtain a second precursor;

[0011] The second precursor is pyrolyzed to obtain a copper-based catalyst.

[0012] Preferably, the Cu salt includes one or more of copper citrate, copper nitrate and copper acetate.

[0013] Preferably, the Zn salt includes one or more of zinc citrate, zinc nitrate and zinc acetate.

[0014] Preferably, the Al salt includes aluminum isopropoxide and / or aluminum nitrate.

[0015] Preferably, the molar ratio of Cu in the Cu salt, Zn in the Zn salt and Al in the Al salt is 1-7:0.5-4:0.5-4.

[0016] Preferably, the polyethylene glycol includes one or more of polyethylene glycol-200, polyethylene glycol-300, polyethylene glycol-400, polyethylene glycol-600, polyethylene glycol-800, polyethylene glycol-1000, polyethylene glycol-1500, polyethylene glycol-4000 and polyethylene glycol-6000.

[0017] Preferably, the liquid phase heat treatment is carried out in an inert atmosphere, the temperature of the liquid phase heat treatment is 200 to 400° C., and the holding time is 0.5 to 20 hours.

[0018] Preferably, the pyrolysis temperature is 200-1000° C., and the insulation time is 2-15 hours.

[0019] The present invention also provides a copper-based catalyst obtained by the preparation method described in the above technical scheme, comprising an active component and an auxiliary agent, wherein the active component comprises oxides of Cu and Zn, and the auxiliary agent is an oxide of Al; the molar ratio of Cu, Zn and Al is 1-7:0.5-4:0.5-4.

[0020] The present invention also provides the use of the copper-based catalyst described in the above technical solution in preparing methanol by hydrogenating carbon dioxide.

[0021] Compared with the prior art, the present invention has the following beneficial effects:

[0022] The present invention provides a method for preparing a copper-based catalyst, comprising the following steps:

[0023] Prepare a first precursor by using a coprecipitation method or a sol-gel method with Cu salt, Zn salt and Al salt;

[0024] The first precursor and a heat treatment medium are mixed and subjected to liquid phase heat treatment to obtain a slurry catalyst; the heat treatment medium comprises polyethylene glycol and / or glycerol;

[0025] Separating the slurry catalyst from solid to liquid, performing Soxhlet extraction on the obtained solid and then drying it to obtain a second precursor;

[0026] The second precursor is pyrolyzed to obtain a copper-based catalyst.

[0027] The present invention adopts a complete liquid phase method coupled with pyrolysis technology, and uses a heat treatment medium polyethylene glycol (PEG) or glycerol during liquid phase heat treatment. A carbon film is formed on the outer layer of the catalyst to effectively separate and load the active components, thereby avoiding the free growth of active ingredient grains due to thermal aging during use, avoiding catalyst deactivation, and improving the thermal stability of the catalyst. Moreover, polyethylene glycol or glycerol can modify the surface of the catalyst, thereby further improving its catalytic activity and reducing agglomeration, preventing catalyst sintering, avoiding the migration, agglomeration, and growth of active components, and solving the problem of easy thermal sintering and deactivation of the Cu component. At the same time, smaller Cu grains not only have more open planes and defect / edge sites, but can also produce a larger area with the carrier interface, which is conducive to combining with intermediate species and plays an important role in the overall activity of the catalyst. The catalyst synthesized by the present invention has a large specific surface area. The specific surface area of ​​the catalyst in Example 2 is 71.4m 2 / g, which is conducive to the formation of highly dispersed Cu species, uniform dispersion of copper grains, high surface effective copper content, which can effectively improve the reaction activity of the catalyst. Smaller particles can produce stronger interaction forces and show higher methanol selectivity.

[0028] Moreover, the heat treatment medium polyethylene glycol (PEG) used in the present invention is a green organic solvent, which has the advantages of high water solubility, biocompatibility, non-toxicity, high biochemical stability and low cost. The present invention adopts a complete liquid phase preparation technology, which has the characteristics of simple operation, high stability, and not easy to deactivate. The present invention adopts a complete liquid phase preparation technology coupled with a pyrolysis technology to prepare a high-performance CO2 hydrogenation to methanol catalyst.

[0029] The data from the examples show that CuAl2O4 and ZnAl2O4 spinel structures are formed in the catalyst prepared by the present invention, and there is no obvious change before and after the reaction. The stable spinel structure exhibits excellent catalytic ability in terms of thermal catalytic performance and good recyclability in the process of catalyzing CO2 decomposition. BRIEF DESCRIPTION OF THE DRAWINGS

[0030] In order to more clearly illustrate the embodiments of the present invention or the technical solutions in the prior art, the drawings required for use in the embodiments will be briefly introduced below. Obviously, the drawings described below are only some embodiments of the present invention. For ordinary technicians in this field, other drawings can be obtained based on these drawings without paying creative work.

[0031] Figure 1 The crystal structure of catalyst Cat-01 before and after reaction;

[0032] Figure 2 TEM and HRTEM images of Cat-03;

[0033] Figure 3 The activity evaluation results of catalyst Cat-02;

[0034] Figure 4 The activity evaluation results of the catalyst in Example 3 at a reaction temperature of 533K. DETAILED DESCRIPTION

[0035] The present invention provides a method for preparing a copper-based catalyst, comprising the following steps:

[0036] Prepare a first precursor by using a coprecipitation method or a sol-gel method with Cu salt, Zn salt and Al salt;

[0037] The first precursor and a heat treatment medium are mixed and subjected to liquid phase heat treatment to obtain a slurry catalyst; the heat treatment medium comprises polyethylene glycol and / or glycerol;

[0038] Separating the slurry catalyst from solid to liquid, performing Soxhlet extraction on the obtained solid and then drying it to obtain a second precursor;

[0039] The second precursor is pyrolyzed to obtain a copper-based catalyst.

[0040] In the present invention, unless otherwise specified, the materials and equipment used are commercially available products in the art.

[0041] In the present invention, a first precursor is prepared by using a coprecipitation method or a sol-gel method to prepare Cu salt, Zn salt and Al salt.

[0042] In the present invention, the Cu salt preferably includes one or more of copper citrate, copper nitrate and copper acetate.

[0043] In the present invention, the Zn salt preferably includes one or more of zinc citrate, zinc nitrate, zinc acetate and zinc oxide.

[0044] In the present invention, the Al salt preferably includes aluminum isopropoxide and / or aluminum nitrate.

[0045] In the present invention, the molar ratio of Cu in the Cu salt, Zn in the Zn salt and Al in the Al salt is preferably 1-7:0.5-4:0.5-4, more preferably 3:1:2, 4:1:2, 2:2:1, 3:2:1, 1:1:1, 2:1:1 or 2:1:2.

[0046] In the present invention, the coprecipitation method preferably comprises the following steps:

[0047] The Cu salt, Zn salt and Al salt are mixed to obtain a metal salt solution; the metal salt solution and the alkali solution are dripped in parallel, and the obtained precipitate is washed to obtain a first precursor.

[0048] In the present invention, the molar ratio of Cu, Zn and Al in the metal salt solution is preferably 1-7:0.5-4:0.5-4, more preferably 3:1:2 or 2:1:2, and the total cation concentration in the metal salt solution is preferably 1-5 mol / L, and the total cations include Cu 2+ 、Zn 2+ and Al 3+ .

[0049] In the present invention, the alkali in the alkali solution preferably includes Na2CO3 and / or sodium hydroxide, and the concentration of the alkali solution is preferably 1 to 2 mol / L. When the alkali includes Na2CO3 and sodium hydroxide, the Na2CO3 reacts with Al2O3 in the metal salt solution. 3+ The molar ratio is preferably 2:1.

[0050] In the present invention, the temperature of the parallel flow addition is preferably 25-100°C, more preferably 30°C, the parallel flow addition process is preferably accompanied by stirring, and the stirring speed is preferably 300r / min; the pH value of the reaction solution is preferably controlled to be 7-10 during the parallel flow addition process.

[0051] In the present invention, the co-current addition preferably further includes crystallization, the crystallization temperature is preferably 70° C., and the crystallization time is preferably overnight. The first precursor obtained by the co-precipitation method is preferably a hydroxide and / or carbonate precipitate.

[0052] In the present invention, the sol-gel method preferably includes method 1, method 2 or method 3, and the method 1 includes the following steps:

[0053] Mixing Cu salt, Zn salt and ethylene glycol to obtain a CuZn ethylene glycol mixed solution; mixing Al salt, citric acid and water for hydrolysis to obtain an aluminum sol;

[0054] The CuZn ethylene glycol mixed solution and the aluminum sol are mixed and refluxed, and the obtained sol is aged to obtain a gel as the first precursor.

[0055] In the present invention, the usage ratio of the Cu salt, the Zn salt and the ethylene glycol is preferably 0.3 mol:0.1 mol:50-130 mL, more preferably 0.3 mol:0.1 mol:85 mL.

[0056] In the present invention, the usage ratio of the Al salt, citric acid and water is preferably 0.2 mol: 0.01-0.2 mol: 50-120 mL, more preferably 0.2 mol: 0.04 mol: 100 mL.

[0057] In the present invention, the hydrolysis temperature is preferably 50-110° C., more preferably 75° C., and the hydrolysis time is preferably 1-8 h, more preferably 3 h.

[0058] In the present invention, the reflux time is preferably 30 minutes to 3 hours; the aging time is preferably 1 day to 15 days, more preferably 5 days, and the aging is preferably carried out at room temperature.

[0059] The second method comprises the following steps:

[0060] Mixing Cu salt and ethanol to obtain a copper salt solution; mixing Zn salt and water to obtain a Zn salt solution; hydrolyzing Al salt to obtain aluminum sol;

[0061] The copper salt solution is added dropwise to the aluminum sol, and then mixed with the Zn salt solution. The obtained gel is aged to obtain a first precursor.

[0062] The method three comprises the following steps:

[0063] Mixing Cu salt, Zn salt and ethanol to obtain a mixed solution; hydrolyzing Al salt to obtain aluminum sol;

[0064] The mixed solution is added dropwise to the aluminum sol, mixed with water for hydrolysis, and the obtained sol is aged to obtain a first precursor.

[0065] After obtaining the first precursor, the present invention mixes the first precursor and a heat treatment medium to perform liquid phase heat treatment to obtain a slurry catalyst; the heat treatment medium includes polyethylene glycol and / or glycerol.

[0066] In the present invention, the polyethylene glycol preferably includes one or more of polyethylene glycol-200, polyethylene glycol-300, polyethylene glycol-400, polyethylene glycol-600, polyethylene glycol-800, polyethylene glycol-1000, polyethylene glycol-1500, polyethylene glycol-4000 and polyethylene glycol-6000.

[0067] In the present invention, the liquid phase heat treatment is preferably carried out in an inert atmosphere, and the gas of the inert atmosphere preferably includes one or more of N2, He, Ar and CO2. The temperature of the liquid phase heat treatment is preferably 200-400°C, more preferably 280°C, the holding time is preferably 0.5-20h, and the pressure is preferably 0-10MPa; the heating rate from room temperature to the liquid phase heat treatment temperature is preferably 1-5°C / min, more preferably 2°C / min. The first precursor and the heat treatment medium are mixed as follows: the first precursor is dispersed in the heat treatment medium; the mixing temperature is preferably 25-50°C. During the liquid phase heat treatment process, polyethylene glycol has reducing properties and may reduce elemental copper.

[0068] After obtaining the slurry catalyst, the present invention separates the slurry catalyst into solid and liquid, performs Soxhlet extraction on the obtained solid and then dries it to obtain the second precursor.

[0069] In the present invention, the solid-liquid separation method preferably comprises: standing, centrifuging, discarding the supernatant, and taking the solid layer.

[0070] In the present invention, the solvent of the Soxhlet extraction is preferably a low boiling point (lower than 100°C) organic solvent, and the low boiling point organic solvent preferably includes one or more of anhydrous ether, petroleum ether, anhydrous ethanol and chloroform. The present invention uses Soxhlet extraction to remove excess heat treatment medium (such as polyethylene glycol), with simple steps and good effects; the present invention selects a low boiling point solvent, which is conducive to enhancing the extraction capacity.

[0071] In the present invention, the Soxhlet extraction time is preferably 1 to 7 days, more preferably 2 days.

[0072] After obtaining the second precursor, the present invention pyrolyzes the second precursor to obtain a copper-based catalyst.

[0073] In the present invention, the pyrolysis is preferably carried out in a pyrolysis atmosphere, and the pyrolysis atmosphere preferably includes one or more of N2, He, Ar, CO2 and CO. The pyrolysis atmosphere preferably also includes O2, and the volume proportion of O2 in the pyrolysis atmosphere is preferably 0-20%. The oxygen content described in the present invention will not cause Cu sintering; the pyrolysis temperature is preferably 200-1000°C, more preferably 600-1000°C, specifically preferably 600°C, 700°C, 800°C, 900°C or 1000°C, and the holding time is preferably 2-15h, more preferably 10h. The heating rate from room temperature to the pyrolysis temperature is preferably 2°C / min. The present invention decomposes excess polyethylene glycol under high-temperature pyrolysis by regulating the pyrolysis temperature, atmosphere and time.

[0074] In the present invention, after the pyrolysis, the step preferably further comprises: granulating the obtained powdered catalyst to obtain a granular catalyst. The present invention has no special requirements for the granulation method, and the particle size of the obtained granular catalyst can be 40 to 60 meshes.

[0075] The present invention also provides a copper-based catalyst obtained by the preparation method described in the above technical scheme, comprising an active component and an auxiliary agent, wherein the active component comprises oxides of Cu and Zn, and the auxiliary agent is an oxide of Al; the molar ratio of Cu, Zn and Al is 1-7:0.5-4:0.5-4.

[0076] In the present invention, the molar ratio of Cu, Zn and Al in the copper-based catalyst is preferably 3:1:2, and the Cu, Zn and Al form CuAl2O4 and ZnAl2O4 spinel structures, which have strong thermal stability and are not easily deactivated.

[0077] The present invention also provides the use of the copper-based catalyst described in the above technical solution in preparing methanol by hydrogenating carbon dioxide.

[0078] In the present invention, the copper-based catalyst is preferably further subjected to hydrogen reduction before use, and the hydrogen reduction comprises: placing the copper-based catalyst in a fixed bed reactor, heating to a reduction temperature in a H2 atmosphere for a reduction reaction. The temperature of the reduction reaction is preferably 553K, and the time is preferably 4h; the heating rate from room temperature to the reduction reaction temperature is preferably 1-5°C / min.

[0079] In the present invention, the conditions for preparing methanol by hydrogenating carbon dioxide include: the reaction temperature is preferably 200-300°C, more preferably 220-270°C, and even more preferably 250°C; the heating rate from room temperature to the reaction temperature is preferably 1-5°C / min; the reaction pressure is preferably 3-7MPa, more preferably 4-5MPa; the volume ratio of CO2 / H2 is preferably 1:3-1:5, more preferably 1:4; the total flow rate is preferably 40-400mL / min, more preferably 100mL / min.

[0080] In order to further illustrate the present invention, the copper-based catalyst provided by the present invention and its preparation method and application are described in detail below in conjunction with the accompanying drawings and examples, but they should not be construed as limiting the scope of protection of the present invention.

[0081] Example 1

[0082] 1) Weigh 0.3 mol Cu(NO3)2·3H2O and 0.1 mol Zn(NO3)2·6H2O and dissolve them in 85 mL ethylene glycol, stir evenly to obtain mixed solution #1;

[0083] 2) Dissolve 0.2 mol of aluminum isopropoxide and 0.04 mol of citric acid in 100 mL of deionized water in a beaker and hydrolyze (75°C / 3h) to form aluminum sol. Add 1# mixed solution and stir under reflux (30min) until a blue sol is formed. Aging the sol at room temperature for 5 days to obtain 2# gel;

[0084] 3) Disperse 2# gel evenly in polyethylene glycol-200 (200 mL), and obtain a slurry catalyst by heat treatment. The slurry catalyst is separated by solid-liquid centrifugation, and the separated solid phase is placed in a Soxhlet extractor and extracted with anhydrous ethanol for 2 days, and the extracted catalyst is dried overnight;

[0085] Heat treatment process: The prepared Cu-based catalyst precursor is dispersed in the heat treatment medium polyethylene glycol and placed together in a reactor for liquid phase heat treatment. Gas (N2) needs to be introduced during the heat treatment process. The temperature is raised from 50°C to 280°C at a heating rate of 2°C / min. The heat preservation time is 10h to obtain a slurry catalyst.

[0086] 4) The catalyst dried in 3) was placed in a tubular furnace and heated to 600°C at a heating rate of 2°C / min in nitrogen for high-temperature pyrolysis for 10 h (pyrolysis atmosphere was N2) to obtain a finished catalyst, which was recorded as Cat-01.

[0087] Figure 1 The crystal structure of the catalyst Cat-01 before and after the reaction. It can be seen that there is no obvious change before and after the reaction. 0 The minimum grain size of (111) is 25 nm, indicating that Cu 0 The dispersion of the grains is good; the diffraction peak intensity of the catalyst CuAl2O4 / ZnAl2O4 is the strongest, indicating that the catalyst Cat-01 forms enough CuAl2O4 / ZnAl2O4 spinel and has a good crystal shape.

[0088] In the following examples and comparative examples, the conditions not specified are the same as those in Example 1.

[0089] Example 2

[0090] 1) Weigh 0.4 mol Cu(NO3)2·3H2O and 0.1 mol Zn(NO3)2·6H2O, dissolve them in ethylene glycol, and stir them evenly to obtain a mixed solution #1;

[0091] 2) Dissolve 0.2 mol of aluminum isopropoxide and citric acid in deionized water in a beaker and hydrolyze to form aluminum sol. Add 1# mixed solution and stir and reflux until a blue sol is formed. Aging the sol at room temperature to obtain 2# gel;

[0092] 3) Disperse the 2# gel evenly in polyethylene glycol-1000 and obtain a slurry catalyst by heat treatment. The slurry catalyst is separated by solid-liquid centrifugation, and the separated solid phase is placed in a Soxhlet extractor and extracted with anhydrous ethanol. The extracted catalyst is dried overnight;

[0093] 4) The catalyst dried in 3) was placed in a tubular furnace in nitrogen and heated to 700°C at a heating rate of 2°C / min for high-temperature pyrolysis to obtain a finished catalyst, which was recorded as Cat-02.

[0094] Example 3

[0095] 1) Weigh 0.2 mol Cu(NO3)2·3H2O and 0.2 mol Zn(NO3)2·6H2O, dissolve them in ethylene glycol, and stir them evenly to obtain a mixed solution #1;

[0096] 2) Dissolve 0.1 mol of aluminum isopropoxide and citric acid in deionized water in a beaker and hydrolyze to form aluminum sol. Add 1# mixed solution and stir and reflux until a blue sol is formed. Aging the sol at room temperature to obtain 2# gel;

[0097] 3) Disperse the 2# gel evenly in polyethylene glycol-1500 and obtain a slurry catalyst by heat treatment. The slurry catalyst is separated by solid-liquid centrifugation, and the separated solid phase is placed in a Soxhlet extractor and extracted with anhydrous ethanol. The extracted catalyst is dried overnight;

[0098] 4) The catalyst dried in 3) was placed in a tubular furnace in nitrogen and heated to 800°C at a heating rate of 2°C / min for high-temperature pyrolysis to obtain a finished catalyst, which was recorded as Cat-03.

[0099] Figure 2 The TEM and HRTEM images of Cat-03, the scale of the left image is 200nm, and the scale of the right image is 20nm; Figure 2 As can be seen in Figure A, the morphology of the nano-Cu is either a hollow cube or an equilateral triangle, and there are a small number of rod-like structures. At the same time, there is an amorphous protective film on the surface of the sample, which is the C film produced by the decomposition of polyethylene glycol.

[0100] Example 4

[0101] 1) Weigh 0.3 mol Cu(NO3)2·3H2O and 0.2 mol Zn(NO3)2·6H2O, dissolve them in ethylene glycol, and stir them evenly to obtain a mixed solution #1;

[0102] 2) Dissolve 0.1 mol of aluminum isopropoxide and citric acid in deionized water in a beaker and hydrolyze to form aluminum sol. Add 1# mixed solution and stir and reflux until a blue sol is formed. Aging the sol at room temperature to obtain 2# gel;

[0103] 3) Disperse the 2# gel evenly in polyethylene glycol-4000 and obtain a slurry catalyst by heat treatment. The slurry catalyst is separated by solid-liquid centrifugation, and the separated solid phase is placed in a Soxhlet extractor and extracted with anhydrous ethanol. The extracted catalyst is dried overnight;

[0104] 4) The catalyst dried in 3) was placed in a tubular furnace in nitrogen and heated to 900°C at a heating rate of 2°C / min for high-temperature pyrolysis to obtain a finished catalyst, which was recorded as Cat-04.

[0105] Example 5

[0106] 1) Weigh 0.3 mol Cu(NO3)2·3H2O and 0.1 mol Zn(NO3)2·6H2O, dissolve them in ethylene glycol, and stir them evenly to obtain a mixed solution #1;

[0107] 2) Dissolve 0.2 mol of aluminum isopropoxide and citric acid in deionized water in a beaker and hydrolyze to form aluminum sol. Add 1# mixed solution and stir and reflux until a blue sol is formed. Aging the sol at room temperature to obtain 2# gel;

[0108] 3) Disperse the 2# gel evenly in polyethylene glycol-6000 and obtain a slurry catalyst by heat treatment. The slurry catalyst is separated by solid-liquid centrifugation, and the separated solid phase is placed in a Soxhlet extractor and extracted with anhydrous ethanol. The extracted catalyst is dried overnight;

[0109] 4) The catalyst dried in 3) was placed in a tubular furnace in nitrogen and heated to 1000° C. at a heating rate of 2° C. / min for high-temperature pyrolysis to obtain a finished catalyst, which was recorded as Cat-05.

[0110] Example 6

[0111] 1) The previous steps are the same as those in Example 1;

[0112] 2) The dried catalyst was placed in a tubular furnace in nitrogen and heated to 700°C at a heating rate of 2°C / min for high-temperature pyrolysis to obtain a finished catalyst, which was recorded as Cat-06.

[0113] Example 7

[0114] 1) The previous steps are the same as those in Example 1;

[0115] 2) The dried catalyst was placed in a tubular furnace in nitrogen and heated to 800°C at a heating rate of 2°C / min for high-temperature pyrolysis to obtain a finished catalyst, which was recorded as Cat-07.

[0116] Example 8

[0117] 1) The previous steps are the same as those in Example 1;

[0118] 2) The dried catalyst was placed in a tubular furnace in nitrogen and heated to 900°C at a heating rate of 2°C / min for high-temperature pyrolysis to obtain a finished catalyst, which was recorded as Cat-08.

[0119] Example 9

[0120] 1) The previous steps are the same as those in Example 2;

[0121] 2) The dried catalyst was placed in a tubular furnace in nitrogen and heated to 800°C at a heating rate of 2°C / min for high-temperature pyrolysis to obtain a finished catalyst, which was recorded as Cat-09.

[0122] Example 10

[0123] 1) Add the prepared molar ratio of 3:1:2 Cu(NO3)2·3H2O, Zn(NO3)2·6H2O and Al(NO3)3·9H2O mixed solution (total concentration 1.5 mol / L) and 2 mol / L Na2CO3 solution dropwise in a 30°C water bath with vigorous stirring, continue stirring, crystallize in an oven at 70°C overnight, filter and wash with deionized water;

[0124] 2) The filter cake obtained by filtration and washing in 1) is uniformly dispersed in polyethylene glycol-200, and subjected to heat treatment to obtain a slurry catalyst. The slurry catalyst is subjected to solid-liquid centrifugal separation, and the separated solid phase is placed in a Soxhlet extractor and extracted with anhydrous ethanol, and the extracted catalyst is dried overnight;

[0125] 3) The catalyst dried in 2) was placed in a tubular furnace in nitrogen and heated to 600° C. at a heating rate of 2° C. / min for high-temperature pyrolysis to obtain a finished catalyst, which was recorded as Cat-10.

[0126] Embodiment 11

[0127] 1) Add the prepared molar ratio of 3:1:2 Cu(NO3)2·3H2O, Zn(NO3)2·6H2O and Al(NO3)3·9H2O mixed solution (total concentration 1.5 mol / L) and 2 mol / L Na2CO3 solution dropwise in a 30°C water bath with vigorous stirring, continue stirring, crystallize in an oven at 70°C overnight, filter and wash;

[0128] 2) The filter cake obtained by filtration and washing in 1) is uniformly dispersed in polyethylene glycol-400, and subjected to heat treatment to obtain a slurry catalyst. The slurry catalyst is subjected to solid-liquid centrifugal separation, and the separated solid phase is placed in a Soxhlet extractor and extracted with anhydrous ethanol, and the extracted catalyst is dried overnight;

[0129] 3) The catalyst dried in 2) was placed in a tubular furnace in nitrogen and heated to 600° C. at a heating rate of 2° C. / min for high-temperature pyrolysis to obtain a finished catalyst, which was recorded as Cat-11.

[0130] Example 12

[0131] 1) Add the prepared molar ratio of 3:1:2 Cu(NO3)2·3H2O, Zn(NO3)2·6H2O and Al(NO3)3·9H2O mixed solution (total concentration 1.5 mol / L) and 2 mol / L Na2CO3 solution dropwise in a 30°C water bath with vigorous stirring, continue stirring, crystallize in an oven at 70°C overnight, filter and wash;

[0132] 2) The filter cake obtained by filtration and washing in 1) is uniformly dispersed in polyethylene glycol-800, and subjected to heat treatment to obtain a slurry catalyst. The slurry catalyst is subjected to solid-liquid centrifugal separation, and the separated solid phase is placed in a Soxhlet extractor and extracted with anhydrous ethanol, and the extracted catalyst is dried overnight;

[0133] 3) The catalyst dried in 2) was placed in a tubular furnace in nitrogen and heated to 600° C. at a heating rate of 2° C. / min for high-temperature pyrolysis to obtain a finished catalyst, which was recorded as Cat-12.

[0134] Embodiment 13

[0135] 1) Dissolve 0.1 mol Cu(NO3)2·3H2O in ethanol and 0.1 mol Zn(NO3)2·6H2O in deionized water;

[0136] 2) Dissolve 0.1 mol of aluminum isopropoxide and citric acid in deionized water and place in a beaker to hydrolyze to form aluminum sol;

[0137] 3) adding the ethanol solution dissolved in step 1) dropwise to the aluminum sol in step 2); then adding an aqueous solution of zinc nitrate, stirring until a viscous gel is formed, and obtaining a catalyst precursor after aging;

[0138] 4) The catalyst precursor is uniformly dispersed in polyethylene glycol-200, and a slurry catalyst is obtained by heat treatment. The slurry catalyst is separated by solid-liquid centrifugation, and the separated solid phase is placed in a Soxhlet extractor and extracted with anhydrous ethanol, and the extracted catalyst is dried overnight;

[0139] 5) The dried catalyst was placed in a tubular furnace in nitrogen and heated to 600°C at a heating rate of 2°C / min for high-temperature pyrolysis to obtain a finished catalyst, which was recorded as Cat-13.

[0140] Embodiment 14

[0141] 1) Grind 0.1 mol of aluminum isopropoxide and dissolve it in 80 mL of ethylene glycol. Stir at 75°C for 2 h to hydrolyze to form aluminum sol;

[0142] 2) Slowly drop a mixed solution containing 0.2 mol copper nitrate, 0.1 mol zinc nitrate and 70 mL ethanol into the aluminum sol with a peristaltic pump and stir;

[0143] 3) Add 100 mL of distilled water for hydrolysis, and stir under open reflux until a sol is formed. The sol is aged at room temperature to obtain a catalyst precursor.

[0144] 4) The catalyst precursor is uniformly dispersed in polyethylene glycol-200, and a slurry catalyst is obtained by heat treatment. The slurry catalyst is separated by solid-liquid centrifugation, and the separated solid phase is placed in a Soxhlet extractor and extracted with anhydrous ethanol, and the extracted catalyst is dried overnight;

[0145] 5) The dried catalyst was placed in a tubular furnace in nitrogen and heated to 600° C. at a heating rate of 2° C. / min for high-temperature pyrolysis to obtain a finished catalyst, which was recorded as Cat-14.

[0146] Embodiment 15

[0147] Cu(NO3)2·3H2O, Zn(NO3)2·6H2O and Al(NO3)3·9H2O in a molar ratio of 2:1:2 were prepared into a metal salt solution with a volume of 250 mL, so that the total cation concentration was 1 mol / L; at the same time, Na2CO3 and NaOH were prepared into an alkaline solution with a concentration of 1 mol / L, wherein c(CO3 2- )=2c(Al 3+ ).

[0148] The metal salt solution and the alkali solution are added into a three-necked flask with a small amount of distilled water in parallel, and the pH is always controlled at 7 during the pumping process. Stirring is carried out continuously at a speed of 300r / min. After the addition is completed, stirring is continued and crystallization is carried out in an oven at 70°C overnight. The precipitate is then filtered and washed to neutrality, uniformly dispersed in a polyethylene glycol-200 solution, and a slurry catalyst is obtained by heat treatment.

[0149] The slurry catalyst was separated by solid-liquid centrifugation, and the separated solid phase was placed in a Soxhlet extractor for extraction with anhydrous ethanol. The extracted catalyst was kept dry overnight. The dried catalyst was placed in a tubular furnace in nitrogen and heated to 600°C at a heating rate of 2°C / min for high-temperature pyrolysis to obtain a finished catalyst, which was recorded as Cat-15.

[0150] The prepared catalyst was tableted and granulated to obtain a catalyst with a size of 40 to 60 mesh. The catalyst was reacted under the conditions of reaction pressure P = 3.0 MPa, temperature T = 250°C, CO2:H2 = 3:1, and a total flow rate of 100 mL / min. The catalyst was reacted for 15 days without any deactivation.

[0151] Example 16

[0152] 1) Weigh 0.2 mol Cu(NO3)2·3H2O and 0.2 mol Zn(NO3)2·6H2O, dissolve them in ethylene glycol, and stir them evenly to obtain a mixed solution #1;

[0153] 2) Dissolve 0.1 mol of aluminum isopropoxide and citric acid in deionized water in a beaker and hydrolyze to form aluminum sol. Add 1# mixed solution and stir and reflux until a blue sol is formed. Aging the sol at room temperature to obtain 2# gel;

[0154] 3) Disperse the 2# gel evenly in liquid paraffin and obtain a slurry catalyst by heat treatment. The slurry catalyst is separated by solid-liquid centrifugation, and the separated solid phase is placed in a Soxhlet extractor and extracted with anhydrous ethanol. The extracted catalyst is dried overnight;

[0155] 4) The catalyst dried in 3) was placed in a tubular furnace in nitrogen and heated to 600° C. at a heating rate of 2° C. / min for high-temperature pyrolysis to obtain a finished catalyst, which was designated as Cat-16.

[0156] Compared with liquid paraffin as a heat treatment medium, polyethylene glycol (PEG) as a heat treatment medium is a green organic solvent with the advantages of high water solubility, good biocompatibility, non-toxicity, strong stability and low cost. It can modify the catalyst surface, thereby further improving its catalytic activity and reducing agglomeration. From the current evaluation results, no deactivation phenomenon was found in the Cu-Zn-Al catalyst prepared by the complete liquid phase method. Using polyethylene glycol as a heat treatment medium, the CO2 conversion rate and methanol selectivity are higher.

[0157] Application Example 1

[0158] The prepared catalyst was granulated, and 1.5 mL of the catalyst was placed in a fixed bed reactor and reduced at 553 K for 4 h under a H2 atmosphere with a programmed temperature increase (heating rate of 5°C / min); then carbon dioxide and hydrogen were introduced, and the temperature was programmed to 523 K (heating rate of 5°C / min), the boost pressure was 3.0 MPa, and H2:CO2 (volume ratio) was 3:1. The catalyst activity evaluation results are shown in Table 1.

[0159] When the catalyst of Example 1 was used, the reaction temperature was changed to 473K, 493K, 543K and 573K, respectively, which were recorded as Cat-01-1, Cat-01-2, Cat-01-3 and Cat-01-4. The evaluation results of the catalyst activity are shown in Table 2.

[0160] When the catalyst of Example 1 was used, the pressure was changed to 4 MPa and 5 MPa, respectively, which were recorded as Cat-01-5 and Cat-01-6. The evaluation results of the catalyst activity are shown in Table 2.

[0161] When the catalyst of Example 1 was used, the volume ratio of H2 and CO2 was changed, and H2:CO2 was 4:1 and 5:1 respectively, which were recorded as Cat-01-7 and Cat-01-8 respectively. The evaluation results of the catalyst activity are shown in Table 2.

[0162] When the catalyst of Example 3 was used, the reaction temperature was changed to 533 K, which was recorded as Cat-03-1. The evaluation results of the catalyst activity are shown in Table 2.

[0163] Table 1 shows the results of CO2 hydrogenation reaction of catalysts of different embodiments, and Table 2 shows the results of CO2 hydrogenation reaction after changing the application conditions; the second column of the table shows the average conversion rate of CO2, and the third to seventh columns of the table respectively represent the selectivity of dimethyl ether (DME), methanol (MeOH), ethanol (EtOH), carbon monoxide (CO) and alkane (CnHm) in the product. Catalyst Cat-02 can react for at least 480 hours without deactivation, and it is expected to maintain activity for a longer time. The catalysts of the other embodiments reacted for 10 to 15 days without deactivation.

[0164] Table 1 Example catalyst CO2 hydrogenation reaction results

[0165] <![CDATA[Conv.(CO2%)]]> S(DME) S(MeOH) S(EtOH) S(CO) S(CnHm) Cat-01 7.8 0.00 67.82 0.01 31.1 1.07 Cat-02 8 0.00 74.43 2.02 22.21 1.34 Cat-03 10.65 0.00 68.29 0.12 30.37 1.22 Cat-04 8 0.00 75.11 0.23 23.76 0.9 Cat-05 6.71 0.00 62.99 3.43 31.76 1.98 Cat-06 5.11 0.00 52.34 0.17 44.74 2.66 Cat-07 12.3 0.00 71.62 0.02 28.04 0.32 Cat-08 10.22 0.00 48.71 0.09 50.87 0.34 Cat-09 6.21 0.00 53.15 0.05 46.18 0.62 Cat-10 14.5 / 47.85 1.68 47.93 2.54 Cat-11 13.82 / 34.71 0.05 63.13 2.11 Cat-12 15.07 / 40.81 0.04 57.28 1.87 Cat-13 6.76 / 56.71 0.05 42.91 0.33 Cat-14 6.54 / 60.46 0.11 38.69 0.74 Cat-15 12.71 / 46.56 0.71 52.52 0.21 Cat-16 6.99 / 62.77 0.02 36.87 0.34

[0166] Table 2 CO2 hydrogenation reaction results after changing the application conditions

[0167]

[0168] It can be seen from Table 1 that the CO2 single-pass conversion rate can reach more than 10%, and the methanol selectivity can reach more than 70%.

[0169] Figure 3 The activity evaluation results (CO2 conversion rate and methanol selectivity) of the catalyst Cat-02 in Example 2 show that the catalyst can stably maintain the carbon dioxide conversion rate and a relatively high methanol selectivity.

[0170] Figure 4 The results of the catalyst in Example 3 at a reaction temperature of 533 K are as follows: the average CO2 single-pass conversion rate is 16.9%, and the average methanol selectivity is 71.7%.

[0171] Comparative Example 1

[0172] Co-precipitation is one of the traditional methods for preparing catalysts. The general operation is to add the precipitant and metal salts in parallel under stirring, and then wash, filter, dry, roast, grind and shape the resulting precipitate to obtain the desired catalyst.

[0173] Take Cu(NO3)2·3H2O, Zn(NO3)2·6H2O and Al(NO3)3·9H2O in a molar ratio of 2:1:2 to prepare a 250 mL metal salt solution so that the total cation concentration is 1 mol / L; at the same time, take Na2CO3 and NaOH to prepare an alkaline solution with a concentration of 1 mol / L, where c(CO3 2- )=2c(Al 3+ ).

[0174] Add the metal salt solution and the alkali solution into a three-necked flask with a small amount of distilled water in parallel, and always control the pH value to 7 during the pumping process, keep stirring at a speed of 300r / min, continue stirring after the addition is completed, and crystallize in a 70°C oven. Then filter the precipitate, wash it to neutrality, and calcine it at 350°C in a muffle furnace (the calcination temperature is the optimal temperature for preparing the catalyst by the co-precipitation method). After tableting and granulation, a granular catalyst with a particle size of 40 to 60 mesh is obtained.

[0175] This catalyst reacted under the conditions of reaction pressure P = 3.0 MPa, temperature T = 250°C, CO2:H2 = 3:1 (volume ratio), and a total flow rate of 100 mL / min. The reaction conditions were the same as the deactivation conditions tested in Example 15. After 5 days of reaction, the catalyst deactivated rapidly. The stability of the catalyst prepared by the comparative method was far different from that of the catalyst of the present invention.

[0176] The present invention adopts a complete liquid phase method combined with pyrolysis to prepare the CuZnAl catalyst, which solves the problem of thermal sintering deactivation of the Cu component, and not only allows the catalyst to maintain excellent stability, but also allows the catalyst to have a higher methanol synthesis ability.

[0177] Although the above-mentioned embodiments have made a detailed description of the present invention, they are only some embodiments of the present invention, rather than all embodiments. People can also obtain other embodiments based on the embodiments of the present invention without creative work, and these embodiments all fall within the scope of protection of the present invention.

Claims

1. A method for preparing a copper-based catalyst, characterized in that: The following steps are involved: Prepare a first precursor by using a coprecipitation method or a sol-gel method with Cu salt, Zn salt and Al salt; The first precursor and a heat treatment medium are mixed and subjected to liquid phase heat treatment to obtain a slurry catalyst; the heat treatment medium comprises polyethylene glycol and / or glycerol; Separating the slurry catalyst from solid to liquid, performing Soxhlet extraction on the obtained solid and then drying it to obtain a second precursor; The second precursor is pyrolyzed to obtain a copper-based catalyst.

2. The preparation method according to claim 1, characterized in that: The Cu salt includes one or more of copper citrate, copper nitrate and copper acetate.

3. The preparation method according to claim 1, characterized in that: The Zn salt includes one or more of zinc citrate, zinc nitrate and zinc acetate.

4. The preparation method according to claim 1, characterized in that: The Al salt includes aluminum isopropoxide and / or aluminum nitrate.

5. The preparation method according to any one of claims 1 to 4, characterized in that: The molar ratio of Cu in the Cu salt, Zn in the Zn salt and Al in the Al salt is 1-7:0.5-4:0.5-4.

6. The preparation method according to claim 1, characterized in that: The polyethylene glycol includes one or more of polyethylene glycol-200, polyethylene glycol-300, polyethylene glycol-400, polyethylene glycol-600, polyethylene glycol-800, polyethylene glycol-1000, polyethylene glycol-1500, polyethylene glycol-4000 and polyethylene glycol-6000.

7. The preparation method according to claim 1, characterized in that: The liquid phase heat treatment is carried out in an inert atmosphere, the temperature of the liquid phase heat treatment is 200 to 400° C., and the insulation time is 0.5 to 20 hours.

8. The preparation method according to claim 1, characterized in that: The pyrolysis temperature is 200-1000° C., and the insulation time is 2-15 hours.

9. The copper-based catalyst obtained by the preparation method according to any one of claims 1 to 8, characterized in that: The invention comprises active components and auxiliary agents, wherein the active components comprise oxides of Cu and Zn, and the auxiliary agent is oxide of Al; and the molar ratio of Cu, Zn and Al is 1-7:0.5-4:0.5-4.

10. Use of the copper-based catalyst according to claim 9 in preparing methanol by hydrogenation of carbon dioxide.

Citation Information

Patent Citations

  • Methanol synthesis catalyst and preparation method thereof

    CN110624599A

  • Carbon-modified copper-based catalyst and preparation method and application thereof

    CN111530467A

  • Copper-based catalyst for preparing methanol through hydrogenation of carbon dioxide and preparation method of copper-based catalyst

    CN117085689A

Cited By

  • Porous Cudelta+ / ZnO / Al2O3 catalyst based on sol template confinement anchoring as well as preparation method and application of porous Cudelta+ / ZnO / Al2O3 catalyst

    CN121775847A