Lithium iron phosphate positive electrode material as well as synthesis method and application thereof
The lithium iron phosphate cathode material is synthesized under the principle of lithium ion deintercalation through electrolysis, which solves the problems of high energy consumption and environmental pressure in the synthesis of lithium ion battery cathode materials, and achieves simple process, low cost and high conductivity, which is suitable for mass production. .
Patent Information
- Application Number
- CN202410908966.9
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-07-08
- Publication Date
- 2024-10-29
AI Technical Summary
Existing synthesis methods of lithium-ion battery cathode materials, such as solid-phase methods and liquid-phase methods, have problems such as high energy consumption, environmental pressure, and high equipment costs, and are difficult to adapt to large-scale production needs.
The lithium iron phosphate cathode material is synthesized through the principle of lithium ion deintercalation using the electrolysis method under electrified conditions. The iron phosphate electrode and lithium ferrite are used to coat the iron electrode, and the lithium ions in the electrolytic cell are embedded in the iron phosphate electrode to realize iron phosphate. Synthesis of lithium.
This method has simple process, low energy consumption and low cost, and has the advantages of green and environmental protection. It obtains high conductivity and stability through the inert anode Fe@LFO electrode, and improves the current density and discharge capacity.
Smart Images

Figure CN118854301A_ABST
Abstract
Description
Technical Field
[0001] The present invention relates to the technical field of battery materials, and in particular to a lithium iron phosphate positive electrode material and a synthesis method and application thereof. Background Art
[0002] Lithium-ion batteries are widely used in electric vehicles, consumer electronics and energy storage due to their high energy density, long cycle life and high energy efficiency. Among the positive electrode materials of lithium-ion batteries, lithium iron phosphate materials are currently widely used in the new energy vehicle industry due to their high safety, stable structure and good cycle performance.
[0003] Currently, the synthesis methods of lithium iron phosphate can be divided into solid phase method and liquid phase method.
[0004] Among them, the solid phase method is currently the most widely used method, which generally uses ferrous oxalate, ferric phosphate or ferric oxide as the iron source, lithium carbonate, lithium hydroxide, etc. as the lithium source, ammonium dihydrogen phosphate, diammonium hydrogen phosphate as the phosphorus source, glucose, sucrose, etc. as the carbon source, and various raw materials are mixed according to the metering ratio, ground and dispersed, spray dried, and calcined at high temperature to obtain lithium iron phosphate. This method has a long high-temperature calcination time and high energy consumption. In addition, a large amount of waste gas is generated during the preparation process, which puts pressure on environmental protection.
[0005] The liquid phase method generally uses ferrous sulfate as the iron source, phosphoric acid as the phosphorus source, and lithium hydroxide as the lithium source. The ferrous sulfate solution and the phosphoric acid solution are mixed, and then the lithium hydroxide solution is added to the mixed solution. Lithium iron phosphate is synthesized by hydrothermal reaction under high pressure conditions above 100°C. Although the liquid energy consumption of the liquid phase method is lower than that of the solid phase method, the liquid phase method has high requirements for the high temperature and high pressure resistance of the equipment, and the cost is high, which is not conducive to large-scale production. In addition, wastewater is generated during the preparation process, and the environmental protection cost is high.
[0006] In view of this, the present invention is proposed. Summary of the invention
[0007] The object of the present invention is to provide a lithium iron phosphate positive electrode material and a synthesis method and application thereof, so as to solve or improve the above-mentioned technical problems.
[0008] The present invention can be implemented like this:
[0009] In a first aspect, the present invention provides a method for synthesizing a lithium iron phosphate positive electrode material, comprising the following steps: electrolyzing an electrolytic cell under power-on conditions, and obtaining a lithium iron phosphate positive electrode material at a cathode after electrolysis;
[0010] The electrolytic cell comprises an anode-side electrolyte, a cathode-side electrolyte, a diaphragm, an initial anode connected to a positive electrode of a power source, and an initial cathode connected to a negative electrode of a power source; wherein the diaphragm is arranged between the anode-side electrolyte and the cathode-side electrolyte, at least a portion of the initial anode is located in the anode-side electrolyte, and at least a portion of the initial cathode is located in the cathode-side electrolyte;
[0011] The initial anode is a lithium ferrite-coated iron electrode, and the initial cathode is an iron phosphate electrode; the cathode side electrolyte contains lithium ions.
[0012] In an alternative embodiment, the electrolysis is performed under constant voltage conditions.
[0013] In an optional embodiment, the voltage during the electrolysis process is 0.1V to 0.5V.
[0014] In an optional embodiment, the electrolysis time is 8 h to 15 h.
[0015] In an optional embodiment, the cathode side electrolyte is a lithium salt recovery solution.
[0016] In an optional embodiment, the cathode side electrolyte includes lithium salt recovery liquid recovered by acid leaching of waste lithium iron phosphate electrode sheets.
[0017] In an optional embodiment, the concentration of lithium ions in the cathode side electrolyte is 6 g / L to 12 g / L.
[0018] In an optional embodiment, the anode side electrolyte includes at least one of a sodium sulfate solution and a potassium sulfate solution.
[0019] In an optional embodiment, the concentration of the electrolyte on the anode side is 5 g / L to 20 g / L.
[0020] In an alternative embodiment, the membrane is an anion exchange membrane.
[0021] In an optional embodiment, the preparation of the iron phosphate electrode includes: coating an electrode slurry obtained by mixing iron phosphate, a conductive agent, a binder and a solvent on the surface of a current collector, and drying the mixture.
[0022] In an optional embodiment, the preparation of the iron phosphate electrode includes at least one of the following features:
[0023] Feature 1: The conductive agent includes at least one of conductive carbon black, acetylene black, carbon fiber, carbon nanotube and graphene;
[0024] Feature 2: The binder includes at least one of polyvinylidene fluoride, polyacrylic acid, polymethyl methacrylate and polytetrafluoroethylene;
[0025] Feature 3: The solvent includes N-methylpyrrolidone;
[0026] Feature 4: The mass ratio of the iron phosphate, the conductive agent and the binder solution is (70-90):(5-20):(5-10), wherein the binder solution is obtained by mixing the binder and the solvent;
[0027] Feature 5: In the binder solution, the mass ratio of the binder to the solvent is 1:9 to 2:8;
[0028] Feature 6: Coating amount is 2mg / cm 2 ~6mg / cm 2 ;
[0029] Feature 7: The current collector includes at least one of carbon cloth, graphite felt and titanium mesh;
[0030] Feature 8: Drying temperature is 80℃~100℃;
[0031] Feature 9: Drying time is 12h to 15h.
[0032] In an optional embodiment, the preparation of the lithium ferrite-coated iron electrode includes: using an iron electrode and a nickel electrode as an anode and a cathode, respectively, and subjecting the iron electrode to constant potential polarization in a melted molten salt electrolyte to obtain a lithium ferrite-coated iron electrode having lithium ferrite coated on the iron surface.
[0033] In an optional embodiment, the preparation of the lithium ferrite coated iron electrode includes at least one of the following features:
[0034] Feature 10: The molten salt electrolyte includes lithium carbonate;
[0035] Feature 11: Ag / Ag2SO4 is used as the reference electrode, and the voltage used for constant potential polarization is 0.5V~1.2V;
[0036] Feature 12: The constant potential polarization time is 50min to 70min.
[0037] In a second aspect, the present invention provides a lithium iron phosphate positive electrode material, which is synthesized by the synthesis method of any one of the aforementioned embodiments.
[0038] In a third aspect, the present invention provides a positive electrode plate, wherein the active material in the positive electrode plate includes the lithium iron phosphate positive electrode material of the aforementioned embodiment.
[0039] In a fourth aspect, the present invention provides a battery, comprising the positive electrode sheet of the aforementioned embodiment.
[0040] The beneficial effects of the present invention include:
[0041] The synthesis method of the lithium iron phosphate positive electrode material provided by the present invention is based on the principle of lithium ion deintercalation, and utilizes an electrolytic cell including an iron phosphate electrode, a lithium ferrite-coated iron electrode, and a cathode side electrolyte containing lithium ions. Under power-on conditions, the lithium ions in the cathode side electrolyte are embedded in the iron phosphate electrode to achieve electrolytic synthesis of the lithium iron phosphate positive electrode material. Compared with the traditional solid phase method and liquid phase method, this method has the advantages of simple process, low energy consumption, low cost, and green environmental protection. In addition, in the synthesis method of the lithium iron phosphate positive electrode material provided by the present invention, the inert anode is a Fe@LFO electrode, which has the characteristics of low price, high stability, high conductivity, etc., which is conducive to obtaining a higher current density.
[0042] The lithium iron phosphate positive electrode material synthesized by the method has good stability and conductivity. The battery further prepared by the positive electrode material can have a higher discharge capacity and first efficiency. BRIEF DESCRIPTION OF THE DRAWINGS
[0043] In order to more clearly illustrate the technical solutions of the embodiments of the present invention, the drawings required for use in the embodiments are briefly introduced below. It should be understood that the following drawings only show certain embodiments of the present invention and therefore should not be regarded as limiting the scope. For ordinary technicians in this field, other related drawings can be obtained based on these drawings without creative work.
[0044] Figure 1 This is the XRD diagram of the lithium iron phosphate positive electrode material synthesized in Example 4 of the present invention.
[0045] Figure 2 This is a SEM image of the lithium iron phosphate positive electrode material synthesized in Example 4 of the present invention. DETAILED DESCRIPTION
[0046] In order to make the purpose, technical scheme and advantages of the embodiments of the present invention clearer, the technical scheme in the embodiments of the present invention will be described clearly and completely below. If the specific conditions are not specified in the embodiments, they are carried out according to conventional conditions or conditions recommended by the manufacturer. If the manufacturer of the reagents or instruments used is not specified, they are all conventional products that can be purchased commercially.
[0047] The lithium iron phosphate positive electrode material provided by the present invention and its synthesis method and application are described in detail below.
[0048] The present invention provides a method for synthesizing a lithium iron phosphate (LiFePO4) positive electrode material, comprising the following steps: electrolyzing an electrolytic cell under power-on conditions, and obtaining the lithium iron phosphate positive electrode material at the cathode after electrolysis.
[0049] The electrolytic cell includes an anode-side electrolyte, a cathode-side electrolyte, a diaphragm, an initial anode for connecting to a positive electrode of a power source, and an initial cathode for connecting to a negative electrode of a power source.
[0050] The initial anode is a lithium ferrite coated iron electrode, denoted as Fe@LiFe5O8, abbreviated as Fe@LFO. The substrate of the lithium ferrite coated iron electrode is Fe, and the surface of Fe is coated with lithium ferrite, which is denoted as LiFe5O8.
[0051] The lithium ferrite coated iron electrode is used as an inert anode, and oxygen evolution reaction occurs during the electrolysis process. Compared with other inert electrodes (such as precious metal inert electrodes or carbon-containing inert electrodes), this electrode has the advantages of low price, high stability, and good conductivity. In addition, using the lithium ferrite coated iron electrode as an inert anode can also obtain a higher current density.
[0052] The initial cathode was an iron phosphate electrode.
[0053] A diaphragm is arranged between the anode-side electrolyte and the cathode-side electrolyte, at least a portion of the initial anode is located in the anode-side electrolyte, and at least a portion of the initial cathode is located in the cathode-side electrolyte.
[0054] In some embodiments, the anode side electrolyte, the cathode side electrolyte, the diaphragm, the initial anode and the initial cathode together form an electrolytic cell, the cathode is inserted in the cathode side electrolyte, the anode is inserted in the anode side electrolyte, the diaphragm is arranged between the cathode side electrolyte and the anode side electrolyte to isolate different electrolytes, and the power supply is connected for electrolysis. After the electrolysis is completed, the cathode is taken out, washed and dried to obtain a lithium iron phosphate positive electrode material.
[0055] The reaction occurring on the anode side is as follows:
[0056] H2O-e - →O2↑+H + .
[0057] The reaction occurring on the cathode side is as follows:
[0058] Li+FePO4+e - →LiFePO4.
[0059] In some embodiments, the electrolysis is performed under constant voltage conditions. For example, the voltage during the electrolysis process can be 0.1V to 0.5V, such as 0.1V, 0.2V, 0.3V, 0.4V or 0.5V, or other values within the range of 0.1V to 0.5V. The electrolysis time can be 8h to 15h, such as 8h, 9h, 10h, 11h, 12h, 13h, 14h or 15h, or other values within the range of 8h to 15h.
[0060] In some embodiments, the cathode electrolyte contains lithium ions. For example, the cathode electrolyte can be a lithium salt recovery solution. By using the lithium-containing recovery solution as the cathode electrolyte to synthesize the lithium iron phosphate positive electrode material, it has the advantages of being economical and environmentally friendly, and the recovery solution can be recycled.
[0061] Illustratively, the cathode-side electrolyte may include lithium salt recovery liquid recovered from acid leaching of waste lithium iron phosphate electrode sheets, and may also include other types of lithium salt recovery liquid.
[0062] In some embodiments, the concentration of lithium ions in the cathode side electrolyte can be 6 g / L to 12 g / L, such as 6 g / L, 7 g / L, 8 g / L, 9 g / L, 10 g / L, 11 g / L or 12 g / L, or it can be any other value within the range of 6 g / L to 12 g / L.
[0063] In addition, the cathode side electrolyte may also contain other cations, such as iron ions and aluminum ions. Exemplarily, the concentration of iron ions in the cathode side electrolyte may be 0.1 g / L to 5 g / L, such as 0.1 g / L, 0.5 g / L, 1 g / L, 2 g / L, 3 g / L, 4 g / L or 5 g / L, or other values within the range of 0.1 g / L to 5 g / L. The concentration of aluminum ions in the cathode side electrolyte may be 0.5 g / L to 3 g / L, such as 0.5 g / L, 1 g / L, 2 g / L or 3 g / L, or other values within the range of 0.5 g / L to 3 g / L.
[0064] The anions contained in the cathode side electrolyte may be phosphate ions, for example but not by way of limitation. For example, the concentration of phosphate ions in the cathode side electrolyte may be 0.1 g / L to 3 g / L, such as 0.1 g / L, 0.5 g / L, 1 g / L, 2 g / L or 3 g / L, or other values within the range of 0.1 g / L to 3 g / L.
[0065] In some embodiments, the anode-side electrolyte may illustratively but not limitingly include at least one of a sodium sulfate solution and a potassium sulfate solution.
[0066] For example, the concentration of the electrolyte on the anode side can be 5 g / L to 20 g / L, such as 5 g / L, 8 g / L, 10 g / L, 12 g / L, 15 g / L, 18 g / L or 20 g / L, or it can be any other value within the range of 5 g / L to 20 g / L.
[0067] In some embodiments, the membrane is an anion exchange membrane.
[0068] In continuation of the above, the synthesis method of lithium iron phosphate positive electrode material provided by the present invention is based on the principle of lithium ion deintercalation, using an electrolytic cell including an iron phosphate electrode, a lithium ferrite-coated iron electrode and a cathode electrolyte containing lithium ions, and the lithium ions in the cathode electrolyte are embedded in the iron phosphate electrode under power-on conditions (specifically, in a charging state), so as to realize the electrolytic synthesis of lithium iron phosphate positive electrode material. Compared with the traditional solid phase method and liquid phase method, this method has the advantages of simple process, low energy consumption, low cost and green environmental protection.
[0069] In some embodiments, the iron phosphate electrode can be purchased directly; in other embodiments, the iron phosphate electrode can also be prepared by itself.
[0070] For example, the preparation of the iron phosphate electrode may include: coating an electrode slurry obtained by mixing iron phosphate, a conductive agent, a binder and a solvent on the surface of a current collector, and drying the mixture.
[0071] Wherein, the conductive agent may exemplarily but not limitatively include at least one of conductive carbon black, acetylene black, carbon fiber, carbon nanotube and graphene. The binder may exemplarily but not limitatively include at least one of polyvinylidene fluoride, polyacrylic acid, polymethyl methacrylate and polytetrafluoroethylene. The solvent may exemplarily but not limitatively include N-methylpyrrolidone;
[0072] The mass ratio of iron phosphate, conductive agent and binder solution can be (70-90):(5-20):(5-10), such as 70:20:10, 75:20:5, 80:10:10, 80:15:5, 85:5:10, 85:10:5 or 90:5:5, or other values within the range of (70-90):(5-20):(5-10).
[0073] The binder solution is obtained by mixing a binder with a solvent. In the binder solution, the mass ratio of the binder to the solvent can be 1:9 to 2:8, such as 1:9, 1.5:8.5 or 2:8, or other values within the range of 1:9 to 2:8.
[0074] The coating amount can be 2 mg / cm exemplarily but not limitedly. 2 ~6mg / cm 2 , such as 2mg / cm 2 、3mg / cm 2 , 4mg / cm 2 , 5mg / cm 2 or 6mg / cm 2 etc., or 2 mg / cm 2 ~6mg / cm 2 Other values within the range.
[0075] The current collector may illustratively but not limitatively include at least one of carbon cloth, graphite felt, and titanium mesh.
[0076] The drying process may be carried out in the form of oven drying, and the drying temperature may be 80°C to 100°C, such as 80°C, 85°C, 90°C, 95°C or 100°C, or other values within the range of 80°C to 100°C. The drying time may be 12h to 15h, such as 12h, 12.5h, 13h, 13.5h or 14h, or other values within the range of 12h to 15h.
[0077] In some embodiments, the preparation of the lithium ferrite-coated iron electrode may include: using an iron electrode and a nickel electrode as an anode and a cathode, respectively, and performing constant potential polarization on the iron electrode in a melted molten salt electrolyte to obtain a lithium ferrite-coated iron electrode in which lithium ferrite is coated on the iron surface.
[0078] The molten salt electrolyte includes lithium carbonate, and on this basis, may also include at least one of sodium carbonate, potassium carbonate and calcium carbonate. In some embodiments, the molten salt electrolyte may be obtained by mixing lithium carbonate, sodium carbonate and potassium carbonate in a molar ratio of 43.5:31.5:25.
[0079] The melting temperature only needs to be higher than the melting point of the molten salt electrolyte.
[0080] During the constant potential polarization process, Ag / Ag2SO4 is used as a reference electrode, and the voltage used for constant potential polarization is 0.5V to 1.2V, such as 0.5V, 0.6V, 0.7V, 0.8V, 0.9V, 1.0V, 1.1V or 1.2V, etc., and can also be other values within the range of 0.5V to 1.2V. The time of constant potential polarization can be 50min to 70min, such as 50min, 55min, 60min, 65min or 70min, etc., and can also be other values within the range of 50min to 70min.
[0081] If the voltage used for constant potential polarization is too high, the oxygen evolution reaction will be more violent.
[0082] Correspondingly, the present invention also provides a lithium iron phosphate positive electrode material, which is synthesized by the above-mentioned synthesis method.
[0083] The lithium iron phosphate positive electrode material has good stability and conductivity.
[0084] In addition, the present invention also provides a positive electrode plate, in which the active material includes the above-mentioned lithium iron phosphate positive electrode material.
[0085] The present invention also provides a battery cell, which includes the above-mentioned positive electrode plate.
[0086] For example, the battery cells may be used in, but are not limited to, electrical devices such as vehicles, ships or aircraft.
[0087] The present invention also provides a battery comprising the battery monomer.
[0088] The present invention also provides an electric device, which includes the above-mentioned battery cell and / or battery. As an example, the electric device can be, but not limited to, a mobile phone, a tablet, a laptop computer, an electric toy, an electric tool, a battery car, an electric car, a ship, a spacecraft, etc. Among them, the electric toy can include a fixed or mobile electric toy, such as a game console, an electric car toy, an electric ship toy, and an electric airplane toy, etc., and the spacecraft can include an airplane, a rocket, a space shuttle, and a spacecraft, etc.
[0089] The features and performance of the present invention are further described in detail below in conjunction with the embodiments.
[0090] The lithium ferrite coated iron electrodes in the following examples were prepared in the following manner: 500 g of anhydrous Li2CO3, Na2CO3 and K2CO3 (molar ratio of 43.5:31.5:25.0) were weighed, and the above molten salt electrolytes were evenly mixed and placed in an alumina crucible, and the Al2O3 crucible was placed in a graphite crucible. First, the molten salt electrolyte was dried in an air atmosphere at 300°C for 12 hours, and then the furnace atmosphere was replaced with Ar and a certain positive pressure effect was maintained (Ar gas flow rate was 120 mL / min), the temperature was raised to 800°C and kept for 30 minutes to melt the carbonate, and finally reduced to 650°C for standby use. The Fe sheet electrode (10mm×10mm×0.5mm) and the nickel sheet (10mm×10mm) were bundled on the molybdenum wire current collector as the anode and cathode, respectively. The Ag / Ag2SO4 reference electrode, cathode and anode were inserted into the molten salt electrolyte. The Fe electrode was polarized at a constant potential of 0.5V (relative to the voltage of the Ag / Ag2SO4 reference electrode) for 60min to prepare the Fe@LFO electrode. The residual salt on the surface of the electrode was washed with ultrapure water and dried in vacuum at 60℃ for 12h for use.
[0091] Example 1
[0092] This embodiment provides a lithium iron phosphate positive electrode material, and the synthesis method thereof includes:
[0093] Step (1): Prepare an iron phosphate electrode.
[0094] Mix polyvinylidene fluoride and N-methylpyrrolidone at a mass ratio of 1:9 and stir until polyvinylidene fluoride is completely dissolved to obtain a polyvinylidene fluoride solution. Mix iron phosphate, conductive carbon black and polyvinylidene fluoride solution at a mass ratio of 80:10:10 and stir for 6 hours to obtain an electrode slurry. Use a scraper to coat the electrode slurry on the carbon cloth with a coating amount of 4 mg / cm 2 , and dried in a vacuum drying oven at 80°C for 12 h to obtain an iron phosphate electrode.
[0095] Step (2): Construct an electrolytic cell.
[0096] The iron phosphate electrode prepared in step (1) is used as the initial cathode, and the Fe@LFO electrode is used as the initial anode, which are respectively inserted into the lithium salt recovery liquid and the sodium sulfate solution. The lithium salt recovery liquid and the sodium sulfate solution are separated by an anion exchange membrane. The concentration of lithium ions in the lithium salt recovery liquid is 8 g / L, and the concentration of the sodium sulfate solution is 20 g / L.
[0097] Step (3): Setting a constant voltage for electrolysis.
[0098] The electrolytic cell was set at a constant voltage of 0.2 V (corresponding to a current of 11.8 mA) for electrolysis. After 12 h of electrolysis, the cathode was taken out, washed with deionized water, and dried in a vacuum drying oven at 80° C. for 12 h to obtain a lithium iron phosphate positive electrode material.
[0099] Example 2
[0100] This embodiment provides a lithium iron phosphate positive electrode material, and the synthesis method thereof includes:
[0101] Step (1): Prepare an iron phosphate electrode.
[0102] Mix polyvinylidene fluoride and N-methylpyrrolidone at a mass ratio of 1:9 and stir until polyvinylidene fluoride is completely dissolved to obtain a polyvinylidene fluoride solution. Mix iron phosphate, conductive carbon black and polyvinylidene fluoride solution at a mass ratio of 80:10:10 and stir for 6 hours to obtain an electrode slurry. Use a scraper to coat the electrode slurry on the carbon cloth with a coating amount of 4 mg / cm 2 , and dried in a vacuum drying oven at 80°C for 12 h to obtain an iron phosphate electrode.
[0103] Step (2): Construct an electrolytic cell.
[0104] The iron phosphate electrode prepared in step (1) is used as the initial cathode, and the Fe@LFO electrode is used as the initial anode, which are respectively inserted into the lithium salt recovery liquid and the sodium sulfate solution. The lithium salt recovery liquid and the sodium sulfate solution are separated by an anion exchange membrane. The concentration of lithium ions in the lithium salt recovery liquid is 12 g / L, and the concentration of the sodium sulfate solution is 20 g / L.
[0105] Step (3): Setting a constant voltage for electrolysis.
[0106] The electrolytic cell was set at a constant voltage of 0.1 V (corresponding to a current of 9.9 mA) for electrolysis. After 12 h of electrolysis, the cathode was taken out, washed with deionized water, and dried in a vacuum drying oven at 80° C. for 12 h to obtain a lithium iron phosphate positive electrode material.
[0107] Example 3
[0108] This embodiment provides a lithium iron phosphate positive electrode material, and the synthesis method thereof includes:
[0109] Step (1): Prepare an iron phosphate electrode.
[0110] Mix polyvinylidene fluoride and N-methylpyrrolidone at a mass ratio of 1:9 and stir until polyvinylidene fluoride is completely dissolved to obtain a polyvinylidene fluoride solution. Mix iron phosphate, conductive carbon black and polyvinylidene fluoride solution at a mass ratio of 80:10:10 and stir for 6 hours to obtain an electrode slurry. Use a scraper to coat the electrode slurry on the carbon cloth with a coating amount of 4 mg / cm 2 , and dried in a vacuum drying oven at 80°C for 12 h to obtain an iron phosphate electrode.
[0111] Step (2): Construct an electrolytic cell.
[0112] The iron phosphate electrode prepared in step (1) is used as the initial cathode, and the Fe@LFO electrode is used as the initial anode, which are respectively inserted into the lithium salt recovery liquid and the sodium sulfate solution. The lithium salt recovery liquid and the sodium sulfate solution are separated by an anion exchange membrane. The concentration of lithium ions in the lithium salt recovery liquid is 10 g / L, and the concentration of the sodium sulfate solution is 20 g / L.
[0113] Step (3): Setting a constant voltage for electrolysis.
[0114] The electrolytic cell was set at a constant voltage of 0.3 V (corresponding to a current of 14.1 mA) for electrolysis. After 10 h of electrolysis, the cathode was taken out, washed with deionized water, and dried in a vacuum drying oven at 80° C. for 12 h to obtain a lithium iron phosphate positive electrode material.
[0115] Example 4
[0116] This embodiment provides a lithium iron phosphate positive electrode material, and the synthesis method thereof includes:
[0117] Step (1): Prepare an iron phosphate electrode.
[0118] Mix polyvinylidene fluoride and N-methylpyrrolidone at a mass ratio of 1:9 and stir until polyvinylidene fluoride is completely dissolved to obtain a polyvinylidene fluoride solution. Mix iron phosphate, conductive carbon black and polyvinylidene fluoride solution at a mass ratio of 80:10:10 and stir for 6 hours to obtain an electrode slurry. Use a scraper to coat the electrode slurry on the carbon cloth with a coating amount of 4 mg / cm 2 , and dried in a vacuum drying oven at 80°C for 12 h to obtain an iron phosphate electrode.
[0119] Step (2): Construct an electrolytic cell.
[0120] The iron phosphate electrode prepared in step (1) is used as the initial cathode, and the Fe@LFO electrode is used as the initial anode, which are respectively inserted into the lithium salt recovery liquid and the sodium sulfate solution. The lithium salt recovery liquid and the sodium sulfate solution are separated by an anion exchange membrane. The concentration of lithium ions in the lithium salt recovery liquid is 6 g / L, and the concentration of the sodium sulfate solution is 20 g / L.
[0121] Step (3): Setting a constant voltage for electrolysis.
[0122] The electrolytic cell was set at a constant voltage of 0.5 V (corresponding to a current of 16.6 mA) for electrolysis. After 8 h of electrolysis, the cathode was taken out, washed with deionized water, and dried in a vacuum drying oven at 80° C. for 12 h to obtain a lithium iron phosphate positive electrode material.
[0123] The XRD and SEM images of the lithium iron phosphate cathode material prepared in this example are shown in Figures 1 and 2. Figure 1 and Figure 2 shown.
[0124] Depend on Figure 1 It can be seen that the XRD of lithium iron phosphate prepared by this method corresponds to the standard card and has no obvious impurity peaks.
[0125] Depend on Figure 2 It can be seen that the lithium iron phosphate particles prepared by this method have no obvious agglomeration and have uniform particle size distribution.
[0126] Example 5
[0127] This embodiment provides a lithium iron phosphate positive electrode material, and the synthesis method thereof includes:
[0128] Step (1): Prepare an iron phosphate electrode.
[0129] Mix polyacrylic acid and N-methylpyrrolidone at a mass ratio of 1.5:8.5 and stir until the polyacrylic acid is completely dissolved to obtain a polyacrylic acid solution. Mix iron phosphate, carbon nanotubes and polyacrylic acid solution at a mass ratio of 70:20:10 for 6 hours to obtain an electrode slurry. Use a scraper to apply the electrode slurry on the graphite felt with a coating amount of 2 mg / cm 2, and dried in a vacuum drying oven at 90°C for 15 h to obtain an iron phosphate electrode.
[0130] Step (2): Construct an electrolytic cell.
[0131] The iron phosphate electrode prepared in step (1) is used as the initial cathode, and the Fe@LFO electrode is used as the initial anode, which are respectively inserted into the lithium salt recovery liquid and the potassium sulfate solution. The lithium salt recovery liquid and the potassium sulfate solution are separated by an anion exchange membrane. The concentrations of lithium ions, iron ions, aluminum ions and phosphate ions in the lithium salt recovery liquid are 8 g / L, 0.1 g / L, 0.5 g / L and 0.1 g / L, respectively, and the concentration of the potassium sulfate solution is 5 g / L.
[0132] Step (3): Setting a constant voltage for electrolysis.
[0133] The electrolytic cell was set at a constant voltage of 0.1 V (corresponding to a current of 10.3 mA) for electrolysis. After 15 h of electrolysis, the cathode was taken out, washed with deionized water, and dried in a vacuum drying oven at 80° C. for 12 h to obtain a lithium iron phosphate positive electrode material.
[0134] Example 6
[0135] This embodiment provides a lithium iron phosphate positive electrode material, and the synthesis method thereof includes:
[0136] Step (1): Prepare an iron phosphate electrode.
[0137] Polymethyl methacrylate and N-methyl pyrrolidone were mixed and stirred at a mass ratio of 2:8 until the polymethyl methacrylate was completely dissolved to obtain a polymethyl methacrylate solution. Iron phosphate, graphene and polymethyl methacrylate solution were mixed and stirred at a mass ratio of 90:5:5 for 6 hours to obtain an electrode slurry. The electrode slurry was coated on a titanium mesh with a scraper at a coating amount of 6 mg / cm 2 , and dried in a vacuum drying oven at 100°C for 13 h to obtain an iron phosphate electrode.
[0138] Step (2): Construct an electrolytic cell.
[0139] The iron phosphate electrode prepared in step (1) is used as the initial cathode, and the Fe@LFO electrode is used as the initial anode, which are respectively inserted into the lithium salt recovery liquid and the sodium sulfate solution. The lithium salt recovery liquid and the sodium sulfate solution are separated by an anion exchange membrane. The concentrations of lithium ions, iron ions, aluminum ions and phosphate ions in the lithium salt recovery liquid are 12 g / L, 5 g / L, 3 g / L and 3 g / L, respectively, and the concentration of the sodium sulfate solution is 10 g / L.
[0140] Step (3): Setting a constant voltage for electrolysis.
[0141] The electrolytic cell was set at a constant voltage of 0.3 V (corresponding to a current of 12.7 mA) for electrolysis. After electrolysis for 10 h, the cathode was taken out, washed with deionized water, and dried in a vacuum drying oven at 80° C. for 12 h to obtain a lithium iron phosphate positive electrode material.
[0142] Comparative Example 1
[0143] This comparative example provides a lithium iron phosphate material, and its preparation method is as follows: polyvinylidene fluoride and N-methyl pyrrolidone are mixed and stirred at a mass ratio of 1:9 until the polyvinylidene fluoride is completely dissolved to obtain a polyvinylidene fluoride solution. Commercially available lithium iron phosphate, conductive carbon black and polyvinylidene fluoride solution are mixed and stirred at a mass ratio of 80:10:10 for 6 hours to obtain an electrode slurry. The slurry is coated on a carbon cloth with a scraper, and the coating amount is 4 mg / cm 2 , and dried in a vacuum drying oven at 80°C for 12 hours to obtain lithium iron phosphate material.
[0144] Comparative Example 2
[0145] The difference between this comparative example and Example 4 is that in step (2), the initial anode is a platinum electrode, and the size of the platinum electrode is the same as the size of the Fe@LFO electrode in Example 4.
[0146] Comparative Example 3
[0147] The difference between this comparative example and Example 4 is that in step (2), the initial anode is a carbon anode.
[0148] Comparative Example 4
[0149] The difference between this comparative example and Example 4 is that in step (2), the initial anode is an iron anode.
[0150] Comparative Example 5
[0151] The difference between this comparative example and Example 4 is that in step (3), the voltage is 0.05V.
[0152] Comparative Example 6
[0153] The difference between this comparative example and Example 4 is that in step (3), the voltage is 0.6V.
[0154] Test example
[0155] The lithium iron phosphate materials prepared in Examples 1 to 6 and Comparative Examples 1 to 6 were cut into circles (with a diameter of 10 mm) using a cutting machine, and were assembled into button cells with a metallic lithium negative electrode and a lithium hexafluorophosphate electrolyte for testing. The test conditions included: a constant current charge and discharge method, an upper limit charge voltage of 3V to 4.2V, and a lower limit discharge voltage of 3.0V.
[0156] The test results are shown in Table 1.
[0157] Table 1 Test results
[0158]
[0159]
[0160] It can be seen from Table 1 that the discharge capacity of the lithium iron phosphate positive electrode material synthesized by the method provided in the embodiment of the present invention can reach more than 156 mAh / g, and the first efficiency of power reduction can reach more than 96.7%.
[0161] From the comparison between Example 2 and Example 1, Example 3 and Example 4, it can be seen that the lithium iron phosphate positive electrode material prepared under the conditions of high lithium ion concentration, low voltage and long electrolysis time has the best performance.
[0162] From the comparison between Example 4 and Comparative Example 1, it can be seen that the lithium iron phosphate positive electrode material prepared by directly using commercially available lithium iron phosphate and conductive agent and binder solution is not as good as the lithium iron phosphate positive electrode material prepared by the synthesis method provided by the present invention in terms of discharge capacity and first effect.
[0163] It can be seen from Example 4 and Comparative Example 2 that under the same conditions, the use of the Fe@LFO electrode as the anode has a higher current density than the platinum electrode, indicating that the Fe@LFO electrode has better conductivity.
[0164] From the comparison between Example 4 and Comparative Examples 2 and 3, it can be seen that even though an inert anode is used to synthesize the lithium iron phosphate positive electrode material, the effect of using the Fe@LFO electrode as the initial anode is better.
[0165] From the comparison between Example 4 and Comparative Example 4, it can be seen that the use of an inert anode to synthesize lithium iron phosphate positive electrode material can have a better effect than that of a non-inert anode.
[0166] It can be seen from the comparison between Example 4 and Comparative Examples 5 and 6 that if the voltage is improperly set during the electrolysis process of step (3), the discharge capacity and the first effect of the material will be reduced.
[0167] In summary, the solution provided by the present invention has at least the following advantages:
[0168] (1) The synthesis method of the lithium iron phosphate positive electrode material provided by the present invention is based on the principle of lithium ion deintercalation, using an electrolytic cell including an iron phosphate electrode, a lithium ferrite-coated iron electrode, and a cathode electrolyte containing lithium ions, and the lithium ions in the cathode electrolyte are intercalated into the iron phosphate electrode under power-on conditions (specifically, in a charging state), thereby realizing the electrolytic synthesis of lithium iron phosphate. Compared with the traditional solid phase method and liquid phase method, this method has the advantages of simple process, low energy consumption, low cost, and green environmental protection.
[0169] (2) In the synthesis method of the lithium iron phosphate positive electrode material provided by the present invention, the inert anode is a Fe@LFO electrode, which has the characteristics of low price, high stability, high conductivity, etc., and has good practical application prospects.
[0170] (3) In the present invention, the lithium salt solution is a recovery liquid, and the recovery liquid is used to directly synthesize the lithium iron phosphate positive electrode material, which is economical and environmentally friendly, and the recovery liquid can be recycled.
[0171] The above are only preferred embodiments of the present invention and are not intended to limit the present invention. For those skilled in the art, the present invention may have various modifications and variations. Any modification, equivalent replacement, improvement, etc. made within the spirit and principle of the present invention shall be included in the protection scope of the present invention.
Claims
1. A method for synthesizing a lithium iron phosphate positive electrode material, characterized in that: The following steps are involved: The electrolytic cell is electrolyzed under power-on conditions, and a lithium iron phosphate positive electrode material is obtained at the cathode after electrolysis; The electrolytic cell comprises an anode-side electrolyte, a cathode-side electrolyte, a diaphragm, an initial anode for connecting to a positive electrode of a power source, and an initial cathode for connecting to a negative electrode of a power source; wherein the diaphragm is arranged between the anode-side electrolyte and the cathode-side electrolyte, at least a portion of the initial anode is located in the anode-side electrolyte, and at least a portion of the initial cathode is located in the cathode-side electrolyte; The initial anode is a lithium ferrite-coated iron electrode, the initial cathode is an iron phosphate electrode, and the cathode-side electrolyte contains lithium ions.
2. The synthesis method according to claim 1, characterized in that Electrolysis is carried out under constant voltage conditions; Preferably, the voltage during the electrolysis process is 0.1V to 0.5V; Preferably, the electrolysis time is 8 h to 15 h.
3. The synthesis method according to claim 1, characterized in that The cathode side electrolyte is a lithium salt recovery solution; Preferably, the cathode side electrolyte comprises a lithium salt recovery solution recovered from acid leaching of waste lithium iron phosphate electrode sheets; Preferably, the concentration of lithium ions in the cathode side electrolyte is 6 g / L to 12 g / L.
4. The synthesis method according to claim 1, characterized in that The anode-side electrolyte includes at least one of a sodium sulfate solution and a potassium sulfate solution; Preferably, the concentration of the anode-side electrolyte is 5 g / L to 20 g / L.
5. The synthesis method according to claim 1, characterized in that The diaphragm is an anion exchange membrane.
6. The synthesis method according to any one of claims 1 to 5, characterized in that: The preparation of the iron phosphate electrode comprises: coating an electrode slurry obtained by mixing iron phosphate, a conductive agent, a binder and a solvent on the surface of a current collector, and drying; Preferably, the preparation of the iron phosphate electrode includes at least one of the following features: Feature 1: The conductive agent includes at least one of conductive carbon black, acetylene black, carbon fiber, carbon nanotube and graphene; Feature 2: The binder includes at least one of polyvinylidene fluoride, polyacrylic acid, polymethyl methacrylate and polytetrafluoroethylene; Feature 3: The solvent includes N-methylpyrrolidone; Feature 4: The mass ratio of the iron phosphate, the conductive agent and the binder solution is (70-90):(5-20):(5-10), wherein the binder solution is obtained by mixing the binder and the solvent; Feature 5: In the binder solution, the mass ratio of the binder to the solvent is 1:9 to 2:8; Feature 6: Coating amount is 2mg / cm 2 ~6mg / cm 2 ; Feature 7: The current collector includes at least one of carbon cloth, graphite felt and titanium mesh; Feature 8: Drying temperature is 80℃~100℃; Feature 9: Drying time is 12h to 15h.
7. The synthesis method according to any one of claims 1 to 5, characterized in that: The preparation of the lithium ferrite coated iron electrode comprises: using an iron electrode and a nickel electrode as an anode and a cathode respectively, and subjecting the iron electrode to constant potential polarization in a melted molten salt electrolyte to obtain a lithium ferrite coated iron electrode having lithium ferrite coated on the iron surface; Preferably, the preparation of the lithium ferrite coated iron electrode includes at least one of the following features: Feature 10: The molten salt electrolyte includes lithium carbonate; Feature 11: Ag / Ag2SO4 is used as the reference electrode, and the voltage used for constant potential polarization is 0.5V~1.2V; Feature 12: The constant potential polarization time is 50min to 70min.
8. A lithium iron phosphate positive electrode material, characterized in that: The lithium iron phosphate positive electrode material is synthesized by the synthesis method described in any one of claims 1 to 7.
9. A positive electrode sheet, characterized in that: The active material in the positive electrode sheet includes the lithium iron phosphate positive electrode material according to claim 8.
10. A battery, characterized in that: The battery comprises the positive electrode sheet according to claim 9.
Citation Information
Cited By
A method for treating waste lithium iron phosphate by diaphragm electrolysis and cooperatively synthesizing lithium iron phosphate precursor
CN122707143A