Porous polyimide retainer material with gradient pore structure, preparation method of porous polyimide retainer material and bearing

By designing a gradient pore structure in the porous polyimide cage, the problem in the existing technology of being unable to achieve both on-demand sustained oil release and long lubrication life is solved, achieving high precision and long-lasting performance under different bearing guidance methods. Long-life operation avoids the problem of excessive oil production.

CN118855862APending Publication Date: 2024-10-29LUOYANG BEARING RES INST CO LTD

Patent Information

Application Number
CN202310482230.5
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2023-04-29
Publication Date
2024-10-29

AI Technical Summary

Technical Problem

Existing porous polyimide cages cannot achieve both on-demand sustained oil release and long lubrication life. Especially under vacuum or high temperature conditions, excessive oil production causes friction torque fluctuations, which cannot meet the requirements of spacecraft on bearing life and reliability. Sexually demanding.

Method used

A porous polyimide cage material with a gradient pore structure is used. By combining two porous polyimide layers in the inner and outer directions, the porosity on the side close to the guide surface is low and the porosity on the side far away from the guide surface is high. It is designed as Gradient structure to achieve slow release of oil on demand and extend lubrication life.

Benefits of technology

It realizes the slow release of oil on demand under different bearing guidance methods, avoids the problem of excessive oil output under high porosity, improves the operating reliability and life of the bearing, and meets the needs of high precision and long life.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118855862A_ABST
    Figure CN118855862A_ABST
Patent Text Reader

Abstract

The invention belongs to the field of bearing retainers, and particularly relates to a porous polyimide retainer material with a gradient pore structure, a preparation method of the porous polyimide retainer material and a bearing. The porous polyimide retainer material comprises at least two porous polyimide layers which are combined together in the inner and outer directions, the porosity of the porous polyimide layer close to the guide surface side is low, and the porosity of the porous polyimide layer far away from the guide surface side is high. By utilizing the characteristics, the retainer has the characteristic of slow-release oil discharge, the friction torque fluctuation or exceeding of index requirements caused by excessive oil discharge during vacuum or high-temperature running-in of the high-porosity retainer is avoided, and high precision and reliability during bearing operation are ensured. Meanwhile, by means of the characteristics of high porosity and high oil content of the material far away from the guide surface side, the lubricating oil is continuously conveyed to the side close to the guide surface along with consumption of the lubricating oil close to the guide surface side, so that the lubricating service life is prolonged.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention belongs to the field of bearing cages, and in particular relates to a porous polyimide cage material with a gradient pore structure, a preparation method thereof, and a bearing. Background Art

[0002] Porous polyimide cage materials have the characteristics of high mechanical strength, excellent tribological properties, aging resistance, radiation resistance, etc. They also have good high and low temperature adaptability and lubricant compatibility. The lubricant can form a good circulation in the interconnected pores inside the material, achieving the effect of long-term on-demand oil supply, which greatly improves the stability, reliability and life of the bearing operation. It is now widely used in long-life spacecraft gyro motors, navigators, and momentum wheel bearings.

[0003] The applicant has previously conducted relatively systematic research on aspects such as aperture adjustment (CN111763429A) and aperture concentration (CN113563626A) of porous polyimide retainers. Related products have been well applied in aerospace products, and civilian products based on this technology have also significantly improved the performance of related bearings.

[0004] At present, the pore structure of porous polyimide retainers is uniform as a whole, but in actual applications, it is found that if the porosity of the material is low, the oil content is low, and the ground running-in test meets the technical indicators, but the theoretical lubrication life is short; if the porosity of the material is high, the oil content is high, and the theoretical lubrication life is long, but more oil is released during vacuum or high-temperature running-in, resulting in fluctuations in friction torque or exceeding the index requirements.

[0005] With the development of my country's aerospace industry, host users have put forward higher requirements on the life and reliability of bearings. The existing porous polyimide cages can no longer meet the requirements of on-demand slow release of oil and long lubrication life. Summary of the invention

[0006] The object of the present invention is to provide a porous polyimide cage material with a gradient pore structure to solve the problem that the existing porous polyimide cage cannot have both the desired slow release of oil and a long lubrication life.

[0007] The second object of the present invention is to provide a method for preparing the porous polyimide retainer material to solve the above problems.

[0008] The third object of the present invention is to provide a bearing to further improve the service life and reliability of the bearing.

[0009] In order to achieve the above purpose, the technical solution adopted by the present invention is:

[0010] A porous polyimide retainer material with a gradient pore structure comprises at least two porous polyimide layers combined together in the inner and outer directions, the porous polyimide layer close to the guide surface has a low porosity, and the porous polyimide layer away from the guide surface has a high porosity.

[0011] The porous polyimide cage material with a gradient pore structure provided by the present invention is designed with a gradient of the cage pore structure according to the bearing guiding mode. When the bearing is externally guided, the gap between the inner diameter of the bearing outer ring and the outer diameter of the cage is small. When the bearing rotates, the lubricating oil overflows due to friction or temperature. When the porosity of the outer layer (close to the guiding surface side) of the porous polyimide cage is small and the oil content is low, the oil output is small. The porosity of the inner layer (away from the guiding surface side) of the cage is large and the oil content is high, which can meet the theoretical lubrication life. Similarly, when the bearing is internally guided, the gap between the outer diameter of the bearing inner ring and the inner diameter of the cage is small. When the porosity of the inner layer of the porous polyimide cage is small and the oil content is low, the oil output is small. The porosity of the outer layer of the cage is large and the oil content is high, which can meet the theoretical lubrication life.

[0012] The above characteristics can be used to make the cage have the characteristics of slow release of oil on demand, avoiding excessive oil release of high-porosity cages during vacuum or high-temperature running-in, resulting in friction torque fluctuations or exceeding index requirements, ensuring high precision and reliability during bearing operation. At the same time, relying on the high porosity and high oil content of the material far from the guide surface, as the lubricant near the guide surface is consumed, the lubricant is continuously transported to the side close to the guide surface, thereby increasing the lubrication life.

[0013] To further optimize the performance of the cage material in terms of slow oil release and improved lubrication life, preferably, the porosity of the porous polyimide layer farthest from the guide surface is 1.2 to 2 times the porosity of the porous polyimide layer closest to the guide surface.

[0014] Further preferably, the porosity of the porous polyimide layer on the side farthest from the guide surface is 20-35%. Maintaining the porosity within the above range can meet the use requirements of most bearings.

[0015] Preferably, the porous polyimide layer near the guide surface has a small pore size, and the porous polyimide layer far from the guide surface has a large pore size. Further making the pore size present a gradient change characteristic can further optimize its slow release of oil and lubrication life performance.

[0016] Preferably, the pore size of the porous polyimide layer farthest from the guide surface is 1.1 to 2.5 times the pore size of the porous polyimide layer closest to the guide surface. The pore size change is controlled within the above range, which is easy to manufacture and has a better use effect.

[0017] More preferably, the pore size of the porous polyimide layer on the side farthest from the guide surface is 0.9-2.5 μm. Maintaining the pore size within the above range can meet the use requirements of most bearings.

[0018] The method for preparing the porous polyimide cage material having a gradient pore structure comprises the following steps:

[0019] (1) preparing raw materials for retainers with different pore structures, first feeding and pre-pressing the raw materials corresponding to one of the retainers with pore structures to obtain a preform; then feeding and pre-pressing the raw materials corresponding to the retainers with other pore structures inside or outside the preform to obtain a retainer preform;

[0020] (2) Sintering the retainer preform.

[0021] The method for preparing the porous polyimide retainer material with a gradient pore structure of the present invention mainly prepares each layer of preforms in sequence to obtain a preform with high consistency and good bonding performance, and then sintering the whole to obtain the final product. The method is easy to implement and can be implemented using existing molding molds, and has basically no effect on the production cost of the retainer.

[0022] Preferably, the pre-pressing is an integral pressing, and the pressure of the first pre-pressing is 500-2000 kN / cm 2 The pressure of the last pre-pressing is 2 to 7 times of the pressure of the first pre-pressing; the holding time of the first pre-pressing and the last pre-pressing is 3 to 8 minutes. The above pressing scheme can improve the integrity of the cage preform and ensure the bonding strength between different layers of materials.

[0023] Preferably, in step (2), the sintering temperature is 360-380°C and the holding time is 30-60 minutes. By adopting the above sintering conditions, a better forming effect can be achieved.

[0024] Preferably, the raw material is composed of the following components in mass fraction: 80-100% of monoether anhydride type polyimide and 0-20% of polytetrafluoroethylene molding powder. The raw materials used for retainers with different pore structures can be easily prepared by using the above raw materials.

[0025] The bearing comprises a retaining frame, wherein the retaining frame is made of the above-mentioned porous polyimide retaining frame material with a gradient pore structure.

[0026] The bearing using the above-mentioned retainer will not have the problem of excessive oil discharge when the high-oil content bearing is running in at high temperature, thus avoiding the friction torque fluctuation or exceeding the index requirements caused by excessive oil discharge, thereby improving the operating reliability of the bearing; because it also has a porous polyimide layer with high porosity, it can increase the oil content and extend the service life of the bearing. BRIEF DESCRIPTION OF THE DRAWINGS

[0027] Figure 1 A physical picture of the porous polyimide cage material prepared in Example 1 of the present invention;

[0028] Figure 2 A diagram of a finished cage made from the cage material of Example 1;

[0029] Figure 3 This is the appearance picture of the retainer made of the material of Example 1 after a 600-hour bearing bench running-in test. DETAILED DESCRIPTION

[0030] The present invention provides a porous polyimide cage material with a gradient pore structure, which can realize on-demand slow release of oil while having high porosity and high oil content, thus meeting the needs of high-precision, long-life and high-reliability bearings.

[0031] The structural feature of the porous polyimide retainer is that the porous polyimide retainer includes at least two porous polyimide layers combined together in the inner and outer directions, the porous polyimide layer close to the guide surface has a low porosity, and the porous polyimide layer away from the guide surface has a high porosity.

[0032] Due to the different porosity in the inner and outer directions, the characteristics of the gradient pore structure are reflected. The position of the guide surface is related to the guiding method of the bearing, that is, whether it is externally guided or internally guided. In the case of external guidance, the side close to the guide surface is the outer side of the cage, and the side away from the guide surface is the inner side. In the case of internal guidance, the side close to the guide surface is the inner side of the cage, and the side away from the guide surface is the outer side.

[0033] Taking the internal guide as an example, the gap between the outer diameter of the inner ring of the bearing and the inner diameter of the cage is small. When the porosity of the inner layer of the porous polyimide cage is small and the oil content is low, the oil output is small. The porosity of the outer layer of the cage is large and the oil content is high, which can meet the theoretical lubrication life.

[0034] The manufacturing process of the porous polyimide retainer with a gradient pore structure is further described below.

[0035] A porous polyimide cage material with a gradient pore structure, the preparation of which comprises the following five steps:

[0036] Step 1: Selection of monoether anhydride polyimide molding powder

[0037] The structural formula of monoether anhydride polyimide is as follows:

[0038]

[0039] The monoether anhydride polyimide molding powder is prepared by polycondensation, cyclization and dehydration of 4,4-oxydiphthalic anhydride (ODPA) and 4,4-diaminodiphenyl ether (ODA).

[0040] Generally speaking, the particle size of the molding powder used for small porosity structures is 8 to 20 μm, and the particle size of the molding powder used for large porosity structures is 15 to 40 μm.

[0041] Step 2: Prepare the polyimide blend according to weight percentage

[0042] Take 80-100% of monoether anhydride polyimide molding powder and 0-20% of polytetrafluoroethylene molding powder by weight percentage, then put them into an FM high-speed mixer for stirring to prepare a polyimide blend. Use a 20x microscope to observe the color difference of the polyimide blend. The polyimide blend without obvious color difference is a qualified product and is vacuum-sealed for storage. If it is 100% polyimide, no preparation is required.

[0043] Generally speaking, porous polyimide materials with different pore structures can be prepared by adjusting the particle size of monoether anhydride polyimide molding powder and the relative amount of polytetrafluoroethylene molding powder. For example, porous polyimide materials with small porosity structures can be obtained by using monoether anhydride polyimide molding powder with larger particle size and increasing the relative amount of polytetrafluoroethylene molding powder.

[0044] Step 3: Mold Construction

[0045] In the following embodiments, the porosity of the porous polyimide cage is 15-35%, and the pore size is 0.7-2.5 μm. The inner diameter d of the cage is 15-60 mm, the outer diameter D is 20-70 mm, D / d=1.1-1.4; the height H is 7-16 mm. The finished cage with larger or smaller actual size can be manufactured according to the method of the present invention.

[0046] In the retainer mold: the outer diameter of the mandrel of the outer tube blank mold = the outer diameter of the mandrel of the inner tube blank mold = the said (d-2) mm, the inner diameter of the outer shell of the outer tube blank mold = the said (D+3) mm, the inner diameter of the outer shell of the inner tube blank mold < the inner diameter of the outer shell of the outer tube blank mold, the height of the inner and outer shells = the mandrel height > 4(H+3), the outer diameters of the inner and outer layer mold punches respectively match the inner diameters of their outer shells, the inner diameters of the inner and outer layer mold punches respectively match the outer diameters of their mandrels, the heights of the inner and outer layer mold punches are the same as their outer shells, the inner diameters of the inner and outer layer mold bases respectively match the outer diameters of their mandrels, the outer diameters of the inner and outer layer mold bases respectively match the inner diameters of their outer shells, and all are slipped with the mold cavity.

[0047] In the above cage mold, the outer tube mold is used to form the outer layer of the cage, and the inner tube mold is used to form the inner layer of the cage. The structure of the outer tube mold and the inner tube mold is the same as the existing porous polyimide forming mold (including a jacket, a core, a punch and a base; for example, refer to CN109808114A for the introduction of traditional tubular forming molds), and the cage preform is mainly prepared by switching the outer tube mold and the inner tube mold (see the fourth step for details).

[0048] Step 4: Pre-pressing of monoether anhydride polyimide molding powder

[0049] The inner tube blank mold filled with polyimide mixture is placed on a program-controlled press and pressurized to 500-2000 kN / cm 2 , keep the pressure for 3-8 minutes and demould, put the inner tube preform after demoulding onto the mandrel of the outer tube mold, and then put another polyimide mixture into the mold, add a certain height of limit fixture inside the mold punch, that is, on the mold mandrel, and the height of the limit fixture is h 限位 ,h 限位 =h 预制体 +h 底座 +h 冲头 -h 芯轴 , place the mold in the upper and lower clamps, place it on a program-controlled press and press it to 1000-5000 kN / cm 2 , and fix it with a screw and maintain pressure for 3-8 minutes.

[0050] Step 5: Double-layer matching fixed volume sintering molding

[0051] Place it in a sintering furnace, heat it to 360-380°C after 60-90 minutes, keep it warm for 30-60 minutes and end the program. Take it out and cool it to room temperature. Remove the upper and lower clamps and demold it to obtain a porous polyimide retainer material with a gradient pore structure.

[0052] The material prepared by the above method has the advantages of slow oil release and long lubrication life. At the same time, the interface between the two microporous structures is clear, the interface bonding force is strong, and stratification is not easy to occur.

[0053] The implementation process of the present invention is described in detail below in conjunction with specific embodiments.

[0054] 1. Specific embodiments of the porous polyimide cage material with gradient pore structure and its preparation method and bearing of the present invention are as follows:

[0055] Example 1

[0056] The porous polyimide retainer material with a gradient pore structure of this embodiment includes two inner and outer porous polyimide layers, the inner layer is a small porosity structure, and the outer layer is a large porosity structure. The porosity and pore size characteristics of the inner and outer layers are detailed in Table 1. The porous polyimide retainer is suitable for the inner guide method.

[0057] The method for preparing the porous polyimide cage material with a gradient pore structure of this embodiment comprises the following steps:

[0058] ① Selection of monoether anhydride polyimide molding powder

[0059] The monoether anhydride polyimide molding powder is prepared by polycondensation and cyclization dehydration of 4.4-oxydiphthalic anhydride (ODPA) and 4.4 diaminodiphenyl ether (ODA). The molding powder particle size (D 50 )8μm, and the particle size of the molding powder used for the macroporous structure was obtained by graded sieving (D 50 )15μm.

[0060] ② Prepare the polyimide blend according to weight percentage

[0061] The mixed materials used in the small porosity structure are divided into particle sizes (D 50 ) 8μm polyimide molding powder 97%, polytetrafluoroethylene molding powder 3%, and then put them together in an FM high-speed mixer to mix and prepare a polyimide blend. Use a 20x microscope to observe the color difference of the polyimide blend. The polyimide blend without obvious color difference is a qualified product and is vacuum-sealed for storage. The material used for the macroporous structure is 100% polyimide.

[0062] ③Mold composition

[0063] The inner diameter of the retainer is set to d=29.0mm, the outer diameter is D=35.0mm, and the height is H=11.0mm. In the retainer mold: the outer diameter of the mandrel of the outer tube mold = the outer diameter of the mandrel of the inner tube mold = the (d-2) mm=27.0mm, the inner diameter of the outer shell of the outer tube mold = the (D+3) mm=38.0mm, the inner diameter of the outer shell of the inner tube mold < the inner diameter of the outer shell of the outer tube mold, the inner diameter of the inner shell of the inner tube mold is controlled at 32.0mm, the inner and outer shell heights = the mandrel height>4(H+3)=56.0mm, the outer shell heights of the inner and outer molds are controlled at 60mm, the mandrel height is controlled at 60mm, the punch height is controlled at 60mm, and the base height is controlled at 15mm. The outer diameters of the inner and outer layer mold punches respectively match the inner diameters of their outer sleeves, the inner diameters of the inner and outer layer mold punches respectively match the outer diameters of their core shafts, the heights of the inner and outer layer mold punches are the same as their outer sleeves, the inner diameters of the inner and outer layer mold bases respectively match the outer diameters of their core shafts, the outer diameters of the inner and outer layer mold bases respectively match the inner diameters of their outer sleeves, and all are slipped with the mold cavity.

[0064] ④Monoether anhydride type polyimide molding powder is pre-pressed

[0065] The mixture used for the small porosity structure is loaded into the inner tube blank mold and placed on a program-controlled press to press to 500 kN / cm 2 , hold the pressure for 3 minutes and demould, the height of the inner tube preform is 26.5mm, put the inner tube preform on the mandrel of the outer tube mold, and then put the mixture used for the large porosity structure into the outer tube mold, and add a certain height of limit fixture on the mold punch, that is, on the mold mandrel, and the height of the limit fixture is h 限位 ,h 限位 =h 预制体 +h 底座 +h 冲头 -h 芯轴 = (26.5 + 15 + 60-60) = 41.5 mm, place the mold in the upper and lower clamps, place it on a program-controlled press and press it to 1000 kN / cm 2 , and fix it with a screw and maintain pressure for 3 minutes.

[0066] ⑤Double-layer matching constant volume sintering molding

[0067] The material was placed in a sintering furnace, heated to 370° C. after 60 minutes, and the program was terminated after keeping the temperature for 30 minutes. The material was taken out and cooled to room temperature, and demolded to obtain a porous polyimide retainer material with a gradient pore structure.

[0068] Example 2

[0069] The porous polyimide retainer material with a gradient pore structure of this embodiment includes two inner and outer porous polyimide layers, the inner layer is a large porosity structure, and the outer layer is a small porosity structure. The porosity and pore size characteristics of the inner and outer layers are detailed in Table 1. The porous polyimide retainer is suitable for external guidance.

[0070] The porous polyimide cage material with a gradient pore structure of this embodiment is prepared according to the method of embodiment 1. The difference from embodiment 1 is that:

[0071] In step ①, the particle size of the molding powder used for the small porosity structure is obtained by graded sieving (D 50 )13μm, the molding powder used for the macroporous structure was purchased from Shanghai Synthetic Resin Research Institute, and the particle size (D 50 ) is 25μm.

[0072] In step ②, the mixture used for the small porosity structure is selected according to the weight percentage of the particle size (D 50 ) 90% of 13μm polyimide molding powder and 10% of polytetrafluoroethylene molding powder; the mixture used for the macroporous structure is selected according to the weight percentage of the particle size (D 50 ) 25μm polyimide molding powder 95%, polytetrafluoroethylene molding powder 5%.

[0073] In step ③, the inner diameter of the retainer is set to d=51.0mm, the outer diameter is D=58.5mm, and the height is H=14.0mm. In the retainer mold: the outer diameter of the mandrel of the outer tube mold = the outer diameter of the mandrel of the inner tube mold = the (d-2) mm=49.0mm, the inner diameter of the outer shell of the outer tube mold = the (D+3) mm=61.5mm, the inner diameter of the outer shell of the inner tube mold is controlled at 55.0mm, the inner and outer shell heights = the mandrel height>4(H+3)=68.0mm, the outer shell heights of the inner and outer molds are controlled at 70mm, the mandrel height is controlled at 70mm, the punch height is controlled at 70mm, and the base height is controlled at 15mm.

[0074] In step ④, the mixture used for the large porosity structure is loaded into the inner tube blank mold and placed on a program-controlled press to press to 1500 kN / cm 2 , hold the pressure for 8 minutes and demould, the height of the inner tube preform is 32.0mm, put the inner tube preform on the mandrel of the outer tube mold, and then put the mixture used for the small porosity structure into the outer tube mold, the height of the limit tooling is h 限位 ,h 限位 =h 预制体 +h 底座 +h 冲头 -h 芯轴 = (32.0 + 15 + 70-70) = 47.0 mm, placed on a program-controlled press and pressurized to 3000 kN / cm2 , maintain pressure for 5 minutes.

[0075] In step ⑤, the sintering process is to heat to 375°C after 70 minutes and the program ends after keeping warm for 45 minutes.

[0076] Example 3

[0077] The porous polyimide retainer material with a gradient pore structure of this embodiment includes two inner and outer porous polyimide layers, the inner layer is a small porosity structure, and the outer layer is a large porosity structure. The porosity and pore size characteristics of the inner and outer layers are detailed in Table 1. The porous polyimide retainer is suitable for the inner guide method.

[0078] The porous polyimide cage material with a gradient pore structure of this embodiment is prepared according to the method of embodiment 1. The difference from embodiment 1 is that:

[0079] In step ①, the particle size of the molding powder used for the small porosity structure is obtained by graded sieving (D 50 )17μm, the molding powder used for the macroporous structure was purchased from Shanghai Synthetic Resin Research Institute, and the particle size (D 50 ) is 35μm.

[0080] In step ②, the mixture used for the small porosity structure is selected according to the weight percentage of the particle size (D 50 ) 17μm polyimide molding powder 90%, polytetrafluoroethylene molding powder 10%; the mixture used for the macroporous structure is selected according to the weight percentage of the particle size (D 50 ) 35μm polyimide molding powder 90%, polytetrafluoroethylene molding powder 10%.

[0081] In step ③, the inner diameter of the retainer is set to d=16.0mm, the outer diameter is D=21.5mm, and the height is H=7.5mm. In the retainer mold: the outer diameter of the mandrel of the outer tube mold = the outer diameter of the mandrel of the inner tube mold = the (d-2) mm=14.0mm, the inner diameter of the outer shell of the outer tube mold = the (D+3) mm=24.5mm, the inner diameter of the outer shell of the inner tube mold is controlled at 20.0mm, the height of the inner and outer shells = the mandrel height>4(H+3)=42.0mm, the height of the inner and outer shells is controlled at 50mm, the mandrel height is controlled at 50mm, the punch height is controlled at 50mm, and the base height is controlled at 15mm.

[0082] In step ④, the mixture used for the small porosity structure is placed in the inner tube blank mold and placed on a program-controlled press to press to 1000 kN / cm 2 , hold the pressure for 5 minutes and demould, the height of the inner tube preform is 23.5mm, put the inner tube preform on the mandrel of the outer tube mold, and then put the mixture used for the large porosity structure into the outer tube mold, the height of the limit tooling is h限位 ,h 限位 =h 预制体 +h 底座 +h 冲头 -h 芯轴 = (23.5 + 15 + 50-50) = 38.5 mm, placed on a program-controlled press and pressurized to 4000 kN / cm 2 , maintain pressure for 5 minutes.

[0083] In step ⑤, the sintering process is to heat to 370° C. after 70 minutes, and the program ends after keeping warm for 40 minutes.

[0084] Example 4

[0085] The porous polyimide retainer material with a gradient pore structure of this embodiment includes two inner and outer porous polyimide layers, the inner layer is a large porosity structure, and the outer layer is a small porosity structure. The porosity and pore size characteristics of the inner and outer layers are detailed in Table 1. The porous polyimide retainer is suitable for external guidance.

[0086] The porous polyimide cage material with a gradient pore structure of this embodiment is prepared according to the method of embodiment 1. The difference from embodiment 1 is that:

[0087] In step ①, the particle size of the molding powder used for the small porosity structure is obtained by graded sieving (D 50 )10μm, the molding powder used for the macroporous structure was purchased from Shanghai Synthetic Resin Research Institute, and the particle size (D 50 ) is 40μm.

[0088] In step ②, the mixture used for the small porosity structure is selected according to the weight percentage of the particle size (D 50 ) 10μm polyimide molding powder 97%, polytetrafluoroethylene molding powder 3%; the mixture used for the macroporous structure is selected according to the weight percentage of the particle size (D 50 )40μm polyimide molding powder 80%, polytetrafluoroethylene molding powder 20%.

[0089] In step ③, the inner diameter of the retainer is set to d=40.0mm, the outer diameter is D=49.5mm, and the height is H=11.5mm. In the retainer mold: the outer diameter of the mandrel of the outer tube mold = the outer diameter of the mandrel of the inner tube mold = the (d-2) mm=38.0mm, the inner diameter of the outer shell of the outer tube mold = the (D+3) mm=52.5mm, the inner diameter of the outer shell of the inner tube mold is controlled at 43.0mm, the inner and outer shell heights = the mandrel height>4(H+3)=58.0mm, the outer shell heights of the inner and outer molds are controlled at 60mm, the mandrel height is controlled at 60mm, the punch height is controlled at 60mm, and the base height is controlled at 15mm.

[0090] In step ④, the mixture used for the macroporous structure is loaded into the inner tube blank mold and placed on a program-controlled press to press to 2000 kN / cm 2 , hold the pressure for 8 minutes and demould, the height of the inner tube preform is 37.0mm, put the inner tube preform on the mandrel of the outer tube mold, and then put the mixture used for the small porosity structure into the outer tube mold, the height of the limit tooling is h 限位 ,h 限位 =h 预制体 +h 底座 +h 冲头 -h 芯轴 = (37.0 + 15 + 60-60) = 52.0 mm, placed on a program-controlled press and pressurized to 4000 kN / cm 2 , maintain pressure for 5 minutes.

[0091] In step ⑤, the sintering process is to heat to 380° C. after 60 minutes, and the program ends after keeping warm for 50 minutes.

[0092] Example 5

[0093] The porous polyimide retainer material with a gradient pore structure of this embodiment includes two inner and outer porous polyimide layers, the inner layer is a small porosity structure, and the outer layer is a large porosity structure. The porosity and pore size characteristics of the inner and outer layers are detailed in Table 1. The porous polyimide retainer is suitable for the inner guide method.

[0094] The porous polyimide cage material with a gradient pore structure of this embodiment is prepared according to the method of embodiment 1. The difference from embodiment 1 is that:

[0095] In step ①, the particle size of the molding powder used for the small porosity structure is obtained by graded sieving (D 50 )20μm, the molding powder used for the macroporous structure was purchased from Shanghai Synthetic Resin Research Institute, and the particle size (D 50 ) is 30μm.

[0096] In step ②, the mixture used for the small porosity structure is selected according to the weight percentage of the particle size (D 50 ) 80% of 20μm polyimide molding powder and 20% of polytetrafluoroethylene molding powder; the mixture used for the macroporous structure is selected according to the weight percentage of the particle size (D 50 ) 30μm polyimide molding powder 95%, polytetrafluoroethylene molding powder 5%.

[0097] In step ③, the inner diameter of the retainer is set to d=58.5mm, the outer diameter is D=68.0mm, and the height is H=15.5mm. In the retainer mold: the outer diameter of the mandrel of the outer tube mold = the outer diameter of the mandrel of the inner tube mold = the (d-2) mm=56.5mm, the inner diameter of the outer shell of the outer tube mold = the (D+3) mm=71.0mm, the inner diameter of the outer shell of the inner tube mold is controlled at 65.0mm, the inner and outer shell heights = the mandrel height>4(H+3)=74.0mm, the outer shell heights of the inner and outer molds are controlled at 80mm, the mandrel height is controlled at 80mm, the punch height is controlled at 80mm, and the base height is controlled at 15mm.

[0098] In step ④, the mixture used for the small porosity structure is loaded into the inner tube blank mold and placed on a program-controlled press to press to 800 kN / cm 2 , hold the pressure for 6 minutes and demould, the height of the inner tube preform is 39.5mm, put the inner tube preform on the mandrel of the outer tube mold, and then put the mixture used for the large porosity structure into the outer tube mold, the height of the limit tooling is h 限位 ,h 限位 =h 预制体 +h 底座 +h 冲头 -h 芯轴 = (39.5 + 15 + 60-60) = 54.5 mm, placed on a program-controlled press and pressurized to 5000 kN / cm 2 , maintain pressure for 8 minutes.

[0099] In step ⑤, the sintering process is to heat to 370° C. after 90 minutes and to end the process after keeping the temperature for 60 minutes.

[0100] Based on the above cage materials, conventional methods such as machining are used to process the cages, and then bearings of different specifications are produced.

[0101] 2. Experimental Examples

[0102] Experimental Example 1

[0103] The actual picture of the porous polyimide cage material prepared in Example 1 is as follows: Figure 1 As shown. Figure 1 It can be seen that the interface between the two microporous structures is clear, which can make the interface located at the center line of the finished cage, or at any position according to the bearing design.

[0104] In addition, since both structural materials are monoether anhydride polyimide, they have the same molecular structure and strong interface bonding strength. After sintering and bonding together, it is not easy to delaminate when processing the cage. Figure 2 shown.

[0105] Experimental Example 2

[0106] This experimental example illustrates the pore structure characteristics of the porous polyimide cage of each embodiment and tests the tensile strength. The test method is based on the standard GJB 9288-2017. The specific results are shown in Table 1. When measuring the pores of the inner layer and the outer layer, the remaining outer layer and the inner layer need to be machined off respectively, so that the remaining parts can be tested.

[0107] Table 1 Performance test results of porous polyimide cages of different embodiments

[0108]

[0109] From the results in Table 1, it can be seen that the porous polyimide cage material prepared by the present invention has an obvious gradient pore structure, and the pore sizes of the outer layer and the inner layer of the cage can be designed and prepared according to the operation requirements of the bearing. At the same time, the porous polyimide cage material prepared by the present invention has a high tensile strength, and there is no delamination at the fracture, and the interface bonding force is good.

[0110] The porous polyimide cage with gradient pore structure prepared in Example 1 was used for a 600-hour bearing bench running-in test. Under high temperature conditions (50° C.), the current was stable. After the second disassembly, there was no excess lubricating oil inside the bearing, no wear marks on the outer diameter of the cage, and clear wear marks on the pocket holes without dispersion. Figure 3 shown.

[0111] The porous polyimide cage with gradient pore structure can be widely used in the field of controlled torque gyroscopes, momentum wheels, reaction flywheels, aerospace long-life bearing cages, meeting the future development needs of my country's aerospace long-life bearings, with significant economic and social benefits.

Claims

1. A porous polyimide cage material with a gradient pore structure, characterized in that: The porous polyimide retainer includes at least two porous polyimide layers combined together in the inner and outer directions, the porous polyimide layer close to the guide surface has a low porosity, and the porous polyimide layer away from the guide surface has a high porosity.

2. The porous polyimide cage material with a gradient pore structure according to claim 1, characterized in that: The porosity of the porous polyimide layer on the side farthest from the guide surface is 1.2 to 2 times the porosity of the porous polyimide layer on the side closest to the guide surface.

3. The porous polyimide cage material with a gradient pore structure according to claim 2, characterized in that: The porous polyimide layer on the side farthest from the guide surface has a porosity of 20 to 35%.

4. The porous polyimide cage material with a gradient pore structure according to any one of claims 1 to 3, characterized in that: The pore size of the porous polyimide layer on the side close to the guide surface is small, and the pore size of the porous polyimide layer on the side far from the guide surface is large.

5. The porous polyimide cage material with gradient pore structure according to claim 4, characterized in that: The pore size of the porous polyimide layer on the side farthest from the guide surface is 1.1 to 2.5 times the pore size of the porous polyimide layer on the side closest to the guide surface.

6. The porous polyimide cage material with a gradient pore structure according to claim 5, characterized in that: The pore size of the porous polyimide layer on the side farthest from the guide surface is 0.9-2.5 μm.

7. The method for preparing a porous polyimide cage material having a gradient pore structure according to any one of claims 1 to 6, characterized in that: The following steps are involved: (1) preparing raw materials for retainers with different pore structures, first feeding and pre-pressing the raw materials corresponding to one of the retainers with pore structures to obtain a preform; then feeding and pre-pressing the raw materials corresponding to the retainers with other pore structures inside or outside the preform to obtain a retainer preform; (2) Sintering the retainer preform.

8. The method for preparing the porous polyimide cage material with gradient pore structure according to claim 7, characterized in that: The pre-pressing is an integral pressing, and the pressure of the first pre-pressing is 500-2000 kN / cm 2 The pressure of the last pre-pressing is 2 to 7 times of the pressure of the first pre-pressing; the holding time of the first pre-pressing and the last pre-pressing is 3 to 8 minutes.

9. The method for preparing the porous polyimide cage material with gradient pore structure according to claim 7, characterized in that: In step (2), the sintering temperature is 360-380° C., and the heat preservation time is 30-60 minutes.

10. The method for preparing the porous polyimide cage material with gradient pore structure according to claim 7, 8 or 9, characterized in that: The raw material consists of the following components in mass fraction: 80-100% of monoether anhydride type polyimide and 0-20% of polytetrafluoroethylene molding powder.

11. A bearing, including a cage, characterized in that: The retainer is made of the porous polyimide retainer material with a gradient pore structure according to any one of claims 1 to 6.

Citation Information

Patent Citations

  • Method for preparing gradient porous Ti-Mg-based composite material

    CN102168195A

  • Method for manufacturing retainer pipe blank with fusible polyimide molding powder as base material

    CN103182761A

  • Polyimide material, polyimide retainer and preparation method of polyimide material

    CN110421866A

  • Bone tissue engineering gradient porous magnesium-based metal component body and preparation method thereof

    CN110639064A

  • Porous polyimide composite material for bearing retainer, preparation method of porous polyimide composite material and bearing retainer

    CN111763429A

Cited By

  • High-temperature-resistant PI / PET composite release film with gradient structure and preparation method of high-temperature-resistant PI / PET composite release film