Analysis method for rapidly identifying dispersion degree of filler in sizing material
By establishing a linear regression equation using dispersion testing and tensile testing in rubber, we can quickly identify the degree of dispersion of fillers in rubber materials, solve the problems of limited test conditions and large number of samples in the existing technology, and achieve fast and simple filler dispersion. Dispersion degree analysis is suitable for optimization of rubber processing technology in industrial production.
Patent Information
- Application Number
- CN202410979250.8
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-07-22
- Publication Date
- 2024-10-29
AI Technical Summary
The existing methods for analyzing the dispersion degree of fillers in rubber have problems such as limited application range of test conditions, high sample quality requirements, and large quantity, making it difficult to meet the rapid inspection needs in industrial production.
Adopt an analytical method to quickly identify the degree of filler dispersion in the rubber compound, establish a linear regression equation through dispersion testing and tensile test testing, and use the tensile test results to quickly identify the degree of filler dispersion, simplify operations, reduce the number of samples, and is suitable for industry Production.
It realizes fast, simple and low-cost analysis of filler dispersion degree, reduces human labor and environmental pollution, improves the accuracy and versatility of analysis, and is suitable for optimization of rubber processing technology in industrial production.
Smart Images

Figure CN118858604A_ABST
Abstract
Description
Technical Field
[0001] The invention belongs to the technical field of filler dispersion analysis in rubber materials, and in particular relates to an analysis method for quickly identifying the filler dispersion in rubber materials. Background Art
[0002] Filler is a very important component of rubber materials. The dispersibility of filler is one of the important factors affecting the mechanical properties of rubber materials. Good dispersibility helps to improve the performance of rubber materials. At present, the analysis methods for the dispersion degree of fillers in rubber products mainly include: first, qualitative analysis method. The evaluation method of carbon black dispersion is specified in ASTM D2663 A method. This method uses a magnifying glass and a low-magnification binocular microscope to observe the fresh torn section of the rubber compound, and compares the surface state of the sample with the standard dispersion section photo to determine the dispersion grade; second, quantitative analysis method, which is a quantitative analysis method formed by standardizing several analysis methods such as microscopes. This method uses an electron microscope or a high-magnification microscope for testing, and its accuracy is higher than the method of judging by the naked eye; third, the stylus type surface roughness measuring instrument analysis method. The principle of this method is to use the stylus of the stylus type surface roughness measuring instrument to horizontally scan the cut surface of the sample and draw the scanning trajectory curve of the stylus. After the trajectory curve is further processed by a computer, the roughness index of the cross section is calculated based on the peak frequency and average value height of the deviation from the horizontal center line on the scanning curve. This method can quantitatively determine the dispersion degree of carbon black in the rubber compound and can be applied to various rubber compounds.
[0003] Although the above three methods can analyze and determine the dispersion degree of fillers in rubber, they have the following shortcomings: the test results of qualitative analysis will be affected by human factors and have poor accuracy; the quantitative analysis method requires very high-quality slicing technology, and the analysis results are closely related to the slicing quality, which is not suitable for rapid inspection in industrial production; the stylus type surface roughness measuring instrument analysis method requires a large number of samples, otherwise the samples will have large errors, and the popularity of this equipment method is low.
[0004] Therefore, how to provide an analytical method for identifying the dispersion degree of fillers in rubber materials, which is simple and quick, requires a small number of samples and has high versatility, is an urgent problem to be solved by those skilled in the art. Summary of the invention
[0005] The present invention aims at the technical problems of the existing analytical methods for the dispersion degree of fillers in rubber, such as limited application range of test conditions, high sample quality requirements and large number of samples, and proposes an analytical method for quickly identifying the dispersion degree of fillers in rubber with simple procedures, no need for complex equipment and short test cycle, which is of great significance for optimizing rubber processing parameters.
[0006] In order to achieve the above-mentioned purpose, the technical solution adopted by the present invention is: an analytical method for quickly identifying the dispersion degree of fillers in rubber, comprising the following steps: performing dispersion test and tensile test on rubber samples with different dispersion degrees respectively, establishing a linear regression equation based on the obtained dispersion value and the dispersion index determined by the tensile test result, and quickly identifying the dispersion degree of fillers in the rubber by the dispersion index obtained by the tensile test of the tested rubber and the linear regression equation; wherein the linear coefficient of the linear regression equation is greater than 0.96.
[0007] Preferably, the tensile test includes a ML test of a low strain tensile stress and a MH test of a high strain tensile stress. ML reflects the interaction between particles, while MH reflects the interaction between rubber materials.
[0008] Preferably, the low strain range of the elongation stress ML under low strain is 5%-50%. If the strain is less than 5%, the elongation stress will not change much, but the error of the elongation stress may be large. By selecting the range under low strain of 5%-50%, the influence of the error can be overcome.
[0009] Preferably, the high strain range of the tensile stress MH under high strain is 200%-300%. When the range under high strain of 200%-300% is selected, the tensile stress does not change much, and it can be basically considered that the stress belongs to the force between rubbers.
[0010] As a preferred method, the dispersion index MD is determined according to the formula MD=MH / ML. According to the stress curve of the rubber under different strains, the rubber with poor dispersion has higher stress under low strain and high strain than the rubber with good dispersion, but the amplitude of the high stress is different. The stress amplitude under low strain is higher, and using low strain as the denominator can effectively amplify the effect of low strain, and its accuracy and discrimination are improved.
[0011] Preferably, rubber samples with different dispersion degrees are prepared by using the same formula but different mixing processes.
[0012] Preferably, the filler in the rubber material is an inorganic filler.
[0013] Preferably, the rubber sample is a masterbatch, final mix or vulcanized rubber sample including at least one of styrene-butadiene rubber and isoprene rubber.
[0014] Preferably, before the steps of performing dispersion and tensile tests on the rubber samples with different dispersion degrees, the step of performing plate vulcanization on the rubber samples is also included. The purpose of performing dispersion and tensile tests on the rubber samples after vulcanization is to retain the dispersion state of the rubber to the greatest extent. After vulcanization, the rubber performs overall bonding inside under the action of sulfur, which can better reflect the relationship between dispersion and tensile test.
[0015] Preferably, the dispersion test adopts one of the following methods: scanning with a carbon black dispersion analyzer, strain scanning of the rubber material with an RPA, and analysis by a stylus-type surface roughness measuring instrument.
[0016] Compared with the prior art, the advantages and positive effects of the present invention are:
[0017] Compared with the complicated operation of directly measuring the dispersion degree of fillers in rubber materials, the analytical method for quickly identifying the dispersion degree of fillers in rubber materials of the present invention is simpler to operate, requires a small number of samples, saves the sample preparation process of filler dispersion test, saves rubber materials, has a short test cycle, reduces a lot of manpower, and does not generate waste gas and waste liquid in the sample preparation process, has little pollution to the environment, and has low requirements on the quality of samples. General operators can master the sample preparation method, and no operator with professional ability is required.
[0018] Compared with the existing filler dispersion detection method, the sample is prepared by high-quality slicing technology after the rubber is vulcanized, and the dispersion degree is evaluated by observation and comparison through an electron microscope or a high-magnification microscope, and the sampling points are extremely random. The present invention uses tensile testing to more comprehensively display the filling performance of the filler in the rubber, and by establishing a correlation equation with the filler dispersion, the dispersion of the rubber can be evaluated by tensile performance detection means, which is of great significance for optimizing the rubber processing parameters. BRIEF DESCRIPTION OF THE DRAWINGS
[0019] Figure 1 This is a correlation curve between the dispersion degree of the filler in the rubber compound provided in the embodiment of the present invention and the MH300% / ML50% dispersion index. DETAILED DESCRIPTION
[0020] In order to be able to understand the characteristics and technical contents of the embodiments of the present invention in more detail, the technical solutions in the embodiments of the present invention will be clearly and completely described below. Obviously, the embodiments described below are only part of the embodiments of the present invention, rather than all the embodiments of the present invention. In the following technical description, for the convenience of explanation, a full understanding of the disclosed embodiments is provided through multiple details. However, one or more embodiments can still be implemented without these details. Based on the embodiments in the present invention, all other embodiments obtained by ordinary technicians in this field without making creative work belong to the scope of protection requested by the present invention.
[0021] The embodiment of the present invention provides an analytical method for quickly identifying the dispersion degree of fillers in rubber materials. The dispersion degree test and tensile test are respectively performed on rubber samples with different dispersion degrees. A linear regression equation is established based on the obtained dispersion value and the dispersion index determined by the tensile test result. The dispersion degree of fillers in the rubber materials is determined by the dispersion index obtained by the tensile test of the rubber materials to be tested and the linear regression equation. The analytical method for quickly identifying the dispersion degree of fillers in rubber materials of the present invention has a small number of tests and a simple process. It is particularly suitable for analyzing the dispersion degree of fillers in rubber materials prepared from rubber species whose molecular chains are not severely broken during the mixing process, and is of great significance for optimizing rubber material processing parameters.
[0022] At present, tensile test is only used to evaluate the physical properties of rubber. The present invention establishes a correlation between the tensile performance test results and the filler dispersion, and can evaluate the dispersion of the rubber by daily pulling test means, so as to better evaluate the rubber and achieve the purpose of "one test, multiple performance evaluation". The reason why the dispersion of fillers in rubber has a good linear relationship with the dispersion index is that in the stretching process, the tensile stress has the effect between fillers and fillers, the effect between fillers and rubber, and the effect between rubber and rubber. When the filler is unevenly dispersed, the filler will aggregate, and the aggregates will generate attraction. This intermolecular force increases the force between the filler and the rubber; when the filler is evenly dispersed, the filler cannot aggregate, and this intermolecular force is not generated; therefore, when the dispersion between fillers is poorer under low strain, the tensile stress is higher. As the strain increases, the forces between fillers and fillers and between fillers and rubber continue to weaken. When the strain is high, the tensile stress gradually tends to the effect between rubber and rubber. Therefore, the dispersibility index of the rubber compound has a high correlation with the dispersion degree of the filler in the rubber compound, so the dispersibility index can be used to evaluate the dispersion degree of the filler in the rubber compound.
[0023] The analytical method for quickly identifying the dispersion degree of fillers in a rubber material according to an embodiment of the present invention specifically comprises the following steps:
[0024] Prepare rubber samples with different dispersion degrees, wherein the raw material formula includes fillers of the same type and the same amount, and the preparation method adopts different mixing process conditions; the mixing method adopts industry standards or other recognized schemes, including ingredients, preparation of masterbatch, preparation of final mix, plate vulcanization, cutting and other steps, wherein the masterbatch is prepared by raw rubber plasticizing, filler mixing, small material mixing, constant temperature mixing, and rubber removal, and the final mix is prepared by raw rubber plasticizing, small material mixing, constant temperature mixing, and rubber removal; the rubber sample is a masterbatch, final mix or vulcanized rubber sample of at least one of styrene-butadiene rubber and isoprene rubber; the filler in the rubber sample is an inorganic filler, preferably carbon black or white carbon black;
[0025] After vulcanization of rubber samples with different dispersion degrees, dispersion and tensile tests are performed respectively, and the dispersion, tensile stress ML under low strain and tensile stress MH under high strain of each rubber are measured and recorded; wherein, the dispersion of fillers can be measured by an index that can characterize the dispersion degree of rubber, not limited to the dispersion of fillers obtained by scanning with a carbon black dispersion analyzer, strain scanning of rubber using RPA, dispersion of fillers in rubber obtained by stylus surface roughness measuring instrument analysis, etc.; the tensile test can more comprehensively display the filling performance of fillers in rubber, and the low strain value range of tensile stress ML under low strain is 5%-50%; the high strain value range of tensile stress MH under high strain is 200%-300%; by vulcanizing the rubber samples, the dispersion of the rubber is greatly retained through vulcanization cross-linking, and the force between the filler and the rubber is reflected through the stress of the tensile test;
[0026] Determine the dispersion index, the dispersion index MD is the ratio of the modulus stress MH under high strain to the modulus stress ML under low strain, that is, MD = MH / ML;
[0027] Conduct linear correlation analysis on the dispersion index and the dispersion degree, draw a standard curve with the dispersion degree as the horizontal coordinate and the dispersion index as the vertical coordinate, and obtain the linear regression equation of the standard curve;
[0028] The tensile test is carried out on the rubber sample to be tested, and the obtained dispersion index is substituted into the linear regression equation to obtain the predicted dispersion degree, so as to quickly identify the dispersion degree of fillers in the rubber.
[0029] In order to more clearly and in detail introduce the analytical method for quickly identifying the dispersion degree of fillers in rubber provided by the embodiments of the present invention, it will be described in combination with specific embodiments below. In the following embodiments, the fillers are carbon black of the same type and amount, the mixing process adopts the same mixing method, and the masterbatch mixing time is different. The prepared rubber samples are tested to obtain samples with different dispersion degrees. Unless otherwise specified, the reagents and equipment used are commercially available; if the specific processing conditions and processing methods are not clearly described in the embodiments, the conditions and methods known in the art can be used for processing.
[0030] Example 1
[0031] Raw material formula: by weight, 100 parts of styrene-butadiene rubber, 60 parts of medium-super wear-resistant carbon black, 3 parts of zinc oxide, 2 parts of stearic acid, 4 parts of antioxidant, 1.2 parts of sulfur, and 1.3 parts of accelerator CZ;
[0032] Main test equipment: electronic universal material testing machine, Instron, USA; carbon black dispersion analyzer, Alpha Technology, USA; flat vulcanizer, Hubei Dongfang; laboratory small internal mixer, Kobelco, Japan;
[0033] The analytical method for quickly identifying the dispersion degree of fillers in the rubber material of this embodiment comprises the following steps:
[0034] Sample preparation: a masterbatch is prepared by the steps of raw rubber plasticizing, filler mixing, small material mixing, constant temperature mixing, and rubber discharge, wherein the initial temperature of the masterbatch is 60°C, the rotor speed is 90r / min, and the mixing time is 80s; a final rubber mix is prepared by the steps of raw rubber plasticizing, small material mixing, constant temperature mixing, and rubber discharge, and then thinned on an open mixer, sheeted, and flat-plate vulcanized to obtain a vulcanized rubber sample, wherein the final rubber mix is mixed in an internal mixer, and the process conditions of the final rubber mix are a starting temperature of 60°C, 50r / min, an upper push bolt pressure of 1MPa, and mixing up and down 3 times, with mixing times of 30s, 30s, and 45s, respectively, and vulcanization conditions of 161°C×15min, a pressure of 12MPa, and a 5mm thick tensile sheet is made;
[0035] Sample test: Referring to the GB / T 528 method, the vulcanized rubber sample was repeatedly tested by an electronic universal material testing machine to determine its tensile properties and characterize the tensile stress under different deformations. The tensile stress ML under low strain of 5%, 25%, and 50% and the tensile stress MH under high strain of 200%, 250%, and 300% were recorded. The test results are shown in Table 1.
[0036] Referring to the ASTMD7723 standard, the cross section of the vulcanized rubber sample was scanned with a carbon black dispersion analyzer, and the Z value in ASTMD7723 was used to characterize the dispersion of the filler in the rubber, as shown in Table 1, where the dispersion formula is as follows:
[0037]
[0038] Where S1 represents the area percentage of undispersed particles;
[0039] Determine the dispersion index: Determine different dispersion indexes MD according to the formula MD = MH / ML. The specific results are shown in Table 2.
[0040] Example 2
[0041] Raw material formula: by weight, 100 parts of styrene-butadiene rubber, 60 parts of medium-super wear-resistant carbon black, 3 parts of zinc oxide, 2 parts of stearic acid, 4 parts of antioxidant, 1.2 parts of sulfur, and 1.3 parts of accelerator CZ;
[0042] Main test equipment: electronic universal material testing machine, Instron, USA; carbon black dispersion analyzer, Alpha Technology, USA; flat vulcanizer, Hubei Dongfang; laboratory small internal mixer, Kobelco, Japan;
[0043] The analytical method for quickly identifying the dispersion degree of fillers in the rubber material of this embodiment comprises the following steps:
[0044] Sample preparation: a masterbatch is prepared by the steps of raw rubber plasticizing, filler mixing, small material mixing, constant temperature mixing, and rubber discharge, wherein the initial temperature of the masterbatch is 60°C, the rotor speed is 90r / min, and the mixing time is 90s; a final rubber mix is prepared by the steps of raw rubber plasticizing, small material mixing, constant temperature mixing, and rubber discharge, and then thinned on an open mixer, sheeted, and flat-plate vulcanized to obtain a vulcanized rubber sample, wherein the final rubber mix is mixed in an internal mixer, and the process conditions of the final rubber mix are a starting temperature of 60°C, 50r / min, an upper push bolt pressure of 1MPa, and mixing up and down 3 times, with mixing times of 30s, 30s, and 45s, respectively, and vulcanization conditions of 161°C×15min, a pressure of 12MPa, and a 5mm thick tensile sheet is made;
[0045] Sample test: Referring to the GB / T 528 method, the vulcanized rubber sample was repeatedly tested by an electronic universal material testing machine to determine its tensile properties and characterize the tensile stress under different deformations. The tensile stress ML under low strain of 5%, 25%, and 50% and the tensile stress MH under high strain of 200%, 250%, and 300% were recorded. The test results are shown in Table 1.
[0046] Referring to the ASTMD7723 standard, the cross section of the vulcanized rubber sample was scanned with a carbon black dispersion analyzer, and the Z value in ASTMD7723 was used to characterize the dispersion of the filler in the rubber, as shown in Table 1, where the dispersion formula is as follows:
[0047]
[0048] Where S1 represents the area percentage of undispersed particles;
[0049] Determine the dispersion index: Determine different dispersion indexes MD according to the formula MD = MH / ML. The specific results are shown in Table 2.
[0050] Example 3
[0051] Raw material formula: by weight, 100 parts of styrene-butadiene rubber, 60 parts of medium-super wear-resistant carbon black, 3 parts of zinc oxide, 2 parts of stearic acid, 4 parts of antioxidant, 1.2 parts of sulfur, and 1.3 parts of accelerator CZ;
[0052] Main test equipment: electronic universal material testing machine, Instron, USA; carbon black dispersion analyzer, Alpha Technology, USA; flat vulcanizer, Hubei Dongfang; laboratory small internal mixer, Kobelco, Japan;
[0053] The analytical method for quickly identifying the dispersion degree of fillers in the rubber material of this embodiment comprises the following steps:
[0054] Sample preparation: a masterbatch is prepared by the steps of raw rubber plasticizing, filler mixing, small material mixing, constant temperature mixing, and rubber discharge, wherein the initial temperature of the masterbatch is 60°C, the rotor speed is 90r / min, and the mixing time is 110s; a final rubber mix is prepared by the steps of raw rubber plasticizing, small material mixing, constant temperature mixing, and rubber discharge, and then thinned on an open mixer, sheeted, and flat-plate vulcanized to obtain a vulcanized rubber sample, wherein the final rubber mix is mixed in an internal mixer, and the process conditions of the final rubber mix are a starting temperature of 60°C, 50r / min, an upper push bolt pressure of 1MPa, and mixing up and down 3 times, with mixing times of 30s, 30s, and 45s, respectively, and vulcanization conditions of 161°C×15min, a pressure of 12MPa, and a 5mm thick tensile sheet is made;
[0055] Sample test: Referring to the GB / T 528 method, the vulcanized rubber sample was repeatedly tested by an electronic universal material testing machine to determine its tensile properties and characterize the tensile stress under different deformations. The tensile stress ML under low strain of 5%, 25%, and 50% and the tensile stress MH under high strain of 200%, 250%, and 300% were recorded. The test results are shown in Table 1.
[0056] Referring to the ASTMD7723 standard, the cross section of the vulcanized rubber sample was scanned with a carbon black dispersion analyzer, and the Z value in ASTMD7723 was used to characterize the dispersion of the filler in the rubber, as shown in Table 1, where the dispersion formula is as follows:
[0057]
[0058] Where S1 represents the area percentage of undispersed particles;
[0059] Determine the dispersion index: Determine different dispersion indexes MD according to the formula MD = MH / ML. The specific results are shown in Table 2.
[0060] Example 4
[0061] Raw material formula: by weight, 100 parts of styrene-butadiene rubber, 60 parts of medium-super wear-resistant carbon black, 3 parts of zinc oxide, 2 parts of stearic acid, 4 parts of antioxidant, 1.2 parts of sulfur, and 1.3 parts of accelerator CZ;
[0062] Main test equipment: electronic universal material testing machine, Instron, USA; carbon black dispersion analyzer, Alpha Technology, USA; flat vulcanizer, Hubei Dongfang; laboratory small internal mixer, Kobelco, Japan;
[0063] The analytical method for quickly identifying the dispersion degree of fillers in the rubber material of this embodiment comprises the following steps:
[0064] Sample preparation: a masterbatch is prepared by the steps of raw rubber plasticizing, filler mixing, small material mixing, constant temperature mixing, and rubber discharge, wherein the initial temperature of the masterbatch is 60°C, the rotor speed is 90r / min, and the mixing time is 130s; a final rubber mix is prepared by the steps of raw rubber plasticizing, small material mixing, constant temperature mixing, and rubber discharge, and then thinned on an open mixer, sheeted, and flat-plate vulcanized to obtain a vulcanized rubber sample, wherein the final rubber mix is mixed in an internal mixer, and the process conditions of the final rubber mix are a starting temperature of 60°C, 50r / min, an upper push bolt pressure of 1MPa, and mixing up and down 3 times, with mixing times of 30s, 30s, and 45s, respectively, and vulcanization conditions of 161°C×15min, a pressure of 12MPa, and a 5mm thick tensile sheet is made;
[0065] Sample test: Referring to the GB / T 528 method, the vulcanized rubber sample was repeatedly tested by an electronic universal material testing machine to determine its tensile properties and characterize the tensile stress under different deformations. The tensile stress ML under low strain of 5%, 25%, and 50% and the tensile stress MH under high strain of 200%, 250%, and 300% were recorded. The test results are shown in Table 1.
[0066] Referring to the ASTMD7723 standard, the cross section of the vulcanized rubber sample was scanned with a carbon black dispersion analyzer, and the Z value in ASTMD7723 was used to characterize the dispersion of the filler in the rubber, as shown in Table 1, where the dispersion formula is as follows:
[0067]
[0068] Where S1 represents the area percentage of undispersed particles;
[0069] Determine the dispersion index: According to the formula MD = MH / ML, different dispersion indexes MD are determined. The specific results are shown in Table 2.
[0070] Example 1-4 Correlation analysis between dispersion degree and dispersion index
[0071] The dispersions measured in Examples 1-4 were subjected to a linear correlation analysis with the dispersion index obtained based on the tensile stress at different strains. The specific analysis results are shown in Table 2.
[0072] Table 1 Filler dispersion in the rubber materials of Examples 1-4 and tensile stress under different deformations
[0073] performance Example 1 Example 2 Example 3 Example 4 Dispersion / % 55.3 66.3 78.6 87.9 ML5% / MPa 0.87 0.55 0.31 0.21 ML25% / MPa 4.35 2.83 1.63 1.20 ML50% / MPa 5.58 3.72 2.12 1.60 MH200% / MPa 12.58 12.42 12.31 12.29 MH250% / MPa 13.49 13.38 13.30 13.28 MH300% / MPa 13.98 13.95 13.85 13.82
[0074] Table 2 Linear correlation coefficients between filler dispersion and different dispersion indexes in the rubber materials of Examples 1-4
[0075]
[0076]
[0077] As shown in Table 2, the dispersion of fillers in the rubber compound is linearly correlated with the dispersion index MD, and the linear coefficient R 2 greater than 0.96, among which MH300% / ML50% had the highest linear correlation coefficient, and the linear coefficient R 2 =0.9804, so this index is preferred as the dispersion evaluation index of the filler dispersion in the rubber compound. When the dispersion index MH300% / ML50% is used, the dispersion degree (%) of the filler in the rubber compound and the dispersion index are plotted into a correlation curve, as shown in the attached figure. Figure 1 As shown, the linear regression equation of the standard curve is y=0.192x-8.4742.
[0078] Application examples of filler dispersion in rubber compounds
[0079] Four kinds of rubber samples were prepared by adopting the same formula as Example 1 but different mixing processes. The rubber samples were tensile tested after vulcanization, and the tensile stress at 50% low strain and 300% high strain was measured respectively to obtain the dispersion index of MH300% / ML50%. The dispersion index obtained above was substituted into the linear regression equation y=0.192x-8.4742 to obtain the dispersion degree of the filler in the corresponding rubber. Then, the real dispersion degree of the filler in the four kinds of rubber was measured by using a carbon black dispersion analyzer. The measurement results of the actual application case are shown in Table 3.
[0080] Table 3 Application analysis case of filler dispersion in rubber compound
[0081]
[0082] From the above, it can be seen that the comparison between the dispersion prediction analysis results in Table 3 and the actual measured results shows that there is little difference, indicating that by establishing a correlation equation between the dispersion degree of fillers in the rubber and the dispersibility index, the dispersion degree of fillers in the rubber is analyzed and judged using the correlation equation, and the judgment result has a high accuracy rate, which is of great significance for improving the processing parameters of the rubber.
[0083] In summary, the analytical method for rapidly identifying the dispersion degree of fillers in rubber materials of the present invention is applicable to the analysis and determination of the dispersion degree of fillers in rubber materials such as masterbatch, final mix and vulcanized rubber of styrene-butadiene rubber and isoprene rubber; when using this method, it is necessary to establish a correlation equation for the dispersion degree of the rubber material and the dispersion index of the filler in the rubber material, and there is a good correlation; the above embodiment of the present method provides a dispersion index, and in practical applications, the specific dispersion index can be selected according to the physical properties of the rubber material, and is not limited to the dispersion index in the above experimental method of the present invention. In the analytical method for rapidly identifying the dispersion degree of fillers in rubber materials of the present invention, the evaluation index is simple, and it is only necessary to establish a correlation equation between the dispersion index and the dispersion degree in the early stage, and the dispersion degree of the filler in the rubber material can be quickly evaluated by measuring the dispersion index in the later stage; and the dispersion index in the analytical method of the present invention can be obtained by testing the conventional physical property index of the rubber material, realizing the purpose of "one test, multiple performance evaluation".
[0084] Finally, it should be noted that the present invention is not limited to the above-mentioned embodiments. The above-mentioned embodiments are only the preferred feasible embodiments of the present invention, and the above-mentioned embodiments are only used to illustrate the technical scheme of the present invention, and are not intended to limit the scope of the present invention. Without departing from the design spirit of the present invention, various deformations, modifications, evolutions and improvements made by ordinary technicians in this field to the technical scheme of the present invention should all fall within the protection scope determined by the claims of the present invention.
Claims
1. A method for quickly identifying the dispersion degree of fillers in rubber materials, characterized in that: The following steps are involved: Dispersion test and tensile test are respectively carried out on rubber samples with different dispersion degrees. A linear regression equation is established based on the obtained dispersion value and the dispersion index determined by the tensile test result. The dispersion degree of fillers in the rubber is quickly identified by the dispersion index obtained by the tensile test of the tested rubber and the linear regression equation. Among them, the linear coefficient of the linear regression equation is greater than 0.
96.
2. The method for rapidly identifying the dispersion degree of fillers in rubber materials according to claim 1, characterized in that: The tensile test includes the ML test of the tensile stress at low strain and the MH test of the tensile stress at high strain.
3. The method for rapidly identifying the dispersion degree of fillers in rubber materials according to claim 2, characterized in that: The low strain range of the low strain modulus stress ML is 5%-50%.
4. The method for rapidly identifying the dispersion degree of fillers in rubber materials according to claim 2, characterized in that: The high strain range of the high strain modulus stress MH is 200%-300%.
5. The method for rapidly identifying the dispersion degree of fillers in rubber materials according to claim 2, characterized in that: The dispersion index MD is determined according to the formula MD=MH / ML.
6. The method for rapidly identifying the dispersion degree of fillers in rubber materials according to claim 1, characterized in that: Rubber samples with different dispersion degrees were prepared using the same formula but different mixing processes.
7. The method for rapidly identifying the dispersion degree of fillers in rubber materials according to claim 1, characterized in that: The filler in the rubber compound is an inorganic filler.
8. The method for rapidly identifying the dispersion degree of fillers in rubber materials according to claim 1, characterized in that: The rubber sample is a masterbatch, a final mix or a vulcanized rubber including at least one of styrene-butadiene rubber and isoprene rubber.
9. The method for rapidly identifying the dispersion degree of fillers in rubber materials according to claim 1, characterized in that: Before respectively carrying out dispersion and tensile test steps on rubber samples with different dispersion degrees, the step of flat plate vulcanization of the rubber samples is also included.
10. The method for rapidly identifying the dispersion degree of fillers in rubber materials according to claim 1, characterized in that: The dispersion test adopts one of the following methods: scanning with a carbon black dispersion analyzer, strain scanning of the rubber compound by RPA, and analysis by a stylus-type surface roughness measuring instrument.