Composite flexible resistive film and preparation method and application thereof
By using materials such as polyimide, nanosilver wires, and nanocellulose in composite flexible resistive films, combined with sophisticated preparation processes, the problems of insufficient conductivity and flexibility in the existing technology are solved, and high-performance composite films are achieved. Membrane preparation for high-precision sound sensors and other electronic components.
Patent Information
- Application Number
- CN202410974530.X
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-07-19
- Publication Date
- 2024-10-29
- Estimated Expiration
- Not applicable · inactive patent
AI Technical Summary
Existing composite flexible resistive films have deficiencies in conductivity, flexibility and material dispersion, making it difficult to meet the needs of high-performance flexible electronic products, especially in applications in the field of sound sensors, which are difficult to meet the requirements for sound sensitivity and flexibility.
Polyimide is used as the base material, nanosilver wire is used as the conductive material, nanocellulose is used as the reinforcing material, ethanol and polyvinylpyrrolene are used as the solvent and dispersant, and plant-based epoxy resin and isocyanate are used as the cross-linking agent and curing agent. Composite flexible resistive films are prepared through steps such as stirring, ultrasonic dispersion, coating, cross-linking and curing, and process parameters are carefully controlled to optimize performance.
The composite flexible resistive film achieves low resistivity, high conductivity, excellent flexibility and mechanical strength, meets the needs of high-precision electronic components, and broadens the range of sensitive response to external stimuli such as sound and pressure.
Smart Images

Figure CN118866431A_ABST
Abstract
Description
Technical Field
[0001] The present invention belongs to the technical field of resistor films, and in particular relates to a composite flexible resistor film and a preparation method and application thereof. Background Art
[0002] As an important electronic material, resistor film has a wide range of applications in sensors, touch screens, electronic tags and other fields. Especially in the field of sound sensors, traditional rigid resistor films are difficult to meet the requirements of sound sensitivity and flexibility. Therefore, the development of a composite flexible resistor film that has both good mechanical properties and sound sensitivity has important application value.
[0003] In a Chinese patent with publication number CN107474293B, a friction-sensitive composite flexible resistor film, its preparation method and a friction sensor are mentioned. The preparation method includes: mixing graphene, a pore-forming agent and water to obtain a suspension; heating and evaporating the suspension to obtain a crystalline powder; mixing carbon nanotubes and a dispersant to obtain a dispersion; mixing a polydimethylsiloxane prepolymer and a curing agent to form a wet film on a carrier, coating the crystalline powder on the surface of the wet film, and then curing to obtain a cured film, washing and drying the cured film to obtain a flexible film layer; and soaking the flexible film layer in the dispersion, taking it out and drying it to obtain the composite flexible resistor film. The process of the present invention is simple, and the composite flexible resistor film obtained can sense friction with high sensitivity.
[0004] However, the composite flexible resistor film produced by the above technical solution can sense friction with high sensitivity. This device can sense friction with high sensitivity, but the preparation process of the composite flexible resistor film is relatively simple, lacks fine control over the dispersion and uniformity of the material, and has deficiencies in conductivity and flexibility. It is difficult to meet the needs of high-performance flexible electronic products, so staff need to improve it. Summary of the invention
[0005] The object of the present invention is to provide a composite flexible resistor film and a preparation method and application thereof, so as to solve the problems raised in the above background technology.
[0006] To achieve the above object, the present invention provides the following technical solutions:
[0007] A composite flexible resistor film, comprising the following materials:
[0008] Base materials, conductive materials, reinforcing materials, solvents and dispersants, and cross-linking agents and curing agents;
[0009] The base material is polyimide, the conductive material is nano silver wire, the reinforcing material is nano cellulose, the solvent and dispersant are selected to be suitable for the conductive material, namely ethanol and the dispersant is polyvinyl pyrrolidone, and the crosslinking agent and curing agent are selected to be plant-based epoxy resin and isocyanate.
[0010] A method for preparing a composite flexible resistor film comprises the following steps:
[0011] S1. Preparation of conductive material dispersion: adding conductive material nanosilver wires into a solvent and adding an appropriate amount of dispersant, and preparing a uniform conductive material dispersion by stirring and ultrasonic dispersion treatment;
[0012] S2. Pretreatment of substrate materials: cleaning, drying and surface modification of the substrate materials;
[0013] S3. Conductive layer coating: Use one of the following equipment: a coater, a spin coater, or a spray coater to evenly coat the conductive material dispersion on the pretreated base material, and control the coating thickness and speed;
[0014] S4. Addition of reinforcing materials: During and after the coating of the conductive layer, an appropriate amount of reinforcing materials is added, and the reinforcing materials are evenly distributed in the conductive layer by stirring or spraying;
[0015] S5, cross-linking and curing: placing the base material coated with the conductive layer and the reinforcing material in a UV curing device for cross-linking and curing, and controlling the temperature, time and atmosphere conditions of the cross-linking and curing;
[0016] S6. Post-processing and testing: The cured composite film is cleaned and dried to remove residual solvents and impurities, and tests including but not limited to mechanical properties test, electrical conductivity test and resistance characteristic test are carried out to verify whether the performance indicators of the composite film meet the requirements.
[0017] Preferably, in step S1, after the ultrasonic dispersion is completed, a small amount of the dispersion liquid is dropped on a glass slide, and the dispersion of the conductive material is observed using a microscope to ensure that there is no obvious agglomeration.
[0018] Preferably, in step S3, after coating, a scanning electron microscope (SEM) is used to check the uniformity and thickness of the conductive layer.
[0019] Preferably, in step S5, after curing is completed, the composite film is taken out to observe its surface state and color change, and a preliminary performance test, such as a peel strength test, is performed if necessary to evaluate the cross-linking and curing effects.
[0020] An application of the above composite flexible resistor film in a sound sensor.
[0021] Compared with the prior art, the present invention has the following beneficial effects:
[0022] (1) As a high-performance conductive material, nanosilver wire ensures that the composite flexible resistor film has low resistivity and high conductivity, which is suitable for the preparation of high-precision electronic components.
[0023] (2) The use of flexible substrate materials and nano-reinforced materials ensures that the composite film has excellent flexibility and bendability while maintaining excellent conductive properties, meeting the design requirements of the sound sensor.
[0024] (3) The addition of nanocellulose reinforcement significantly improves the mechanical strength and durability of the composite membrane, enabling it to maintain stable performance in complex usage environments.
[0025] (4) The composite flexible resistor film not only has the basic conductive function, but also can adjust the material formula and preparation process according to needs to achieve sensitive response to external stimuli such as sound and pressure, thus broadening its application scope in sensors, wearable devices and other fields.
[0026] (5) By finely controlling the process parameters and conditions of each step, the performance of the composite membrane can be precisely regulated and optimized to meet the needs of different application scenarios. BRIEF DESCRIPTION OF THE DRAWINGS
[0027] Figure 1 It is a preparation flow chart of the present invention. DETAILED DESCRIPTION
[0028] The following will be combined with the drawings in the embodiments of the present invention to clearly and completely describe the technical solutions in the embodiments of the present invention. Obviously, the described embodiments are only part of the embodiments of the present invention, not all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.
[0029] Embodiment 1:
[0030] See also Figure 1 As shown, a composite flexible resistive film includes the following materials:
[0031] Base materials, conductive materials, reinforcing materials, solvents and dispersants, and cross-linking agents and curing agents;
[0032] The base material is polyimide, the conductive material is nano silver wire, the reinforcing material is nano cellulose, the solvent and dispersant are selected to be suitable for the conductive material, namely ethanol and the dispersant is polyvinyl pyrrolidone, and the crosslinking agent and curing agent are selected to be plant-based epoxy resin and isocyanate.
[0033] Polyimide (PI) is selected as the substrate material because it has good flexibility and chemical stability and is suitable as a supporting substrate for electronic components.
[0034] The conductive material uses silver nanowires (AgNWs) as the conductive material. Silver nanowires have extremely high conductivity and can form a uniform conductive network on a flexible substrate, ensuring low resistivity and high conductivity of the resistor film.
[0035] Reinforcement material Nanocellulose (NFC) is added as a reinforcement material to improve the mechanical strength and durability of the composite membrane. Nanocellulose has excellent mechanical properties and biocompatibility, and can effectively enhance the overall performance of the composite membrane.
[0036] Among the solvents and dispersants, ethanol is selected as the solvent and polyvinyl pyrrolidone (PVP) is selected as the dispersant to prepare a uniform conductive material dispersion.
[0037] Plant-based epoxy resin is used as a cross-linking agent and isocyanate is used as a curing agent to achieve a firm bond between the conductive layer and the base material and to improve the weather resistance and stability of the composite film.
[0038] A method for preparing a composite flexible resistor film comprises the following steps:
[0039] S1. Preparation of conductive material dispersion: adding conductive material nanosilver wires into a solvent and adding an appropriate amount of dispersant, and preparing a uniform conductive material dispersion by stirring and ultrasonic dispersion treatment;
[0040] S2. Pretreatment of substrate materials: cleaning, drying and surface modification of the substrate materials;
[0041] S3. Conductive layer coating: Use one of the following equipment: a coater, a spin coater, or a spray coater to evenly coat the conductive material dispersion on the pretreated base material, and control the coating thickness and speed;
[0042] S4. Addition of reinforcing materials: During and after the coating of the conductive layer, an appropriate amount of reinforcing materials is added, and the reinforcing materials are evenly distributed in the conductive layer by stirring or spraying;
[0043] S5, cross-linking and curing: placing the base material coated with the conductive layer and the reinforcing material in a UV curing device for cross-linking and curing, and controlling the temperature, time and atmosphere conditions of the cross-linking and curing;
[0044] S6. Post-processing and testing: The cured composite film is cleaned and dried to remove residual solvents and impurities, and tests including but not limited to mechanical properties test, electrical conductivity test and resistance characteristic test are carried out to verify whether the performance indicators of the composite film meet the requirements.
[0045] In step S1, after the ultrasonic dispersion is completed, a small amount of dispersion liquid is dropped on a glass slide, and the dispersion of the conductive material is observed using a microscope to ensure that there is no obvious agglomeration.
[0046] In step S3, after coating, the uniformity and thickness of the conductive layer are checked using a scanning electron microscope (SEM).
[0047] In step S5, after the curing is completed, the composite film is taken out, and its surface state and color change are observed. If necessary, a preliminary performance test, such as a peel strength test, is performed to evaluate the cross-linking and curing effects.
[0048] Conductive material dispersion is prepared as follows:
[0049] Step 1: Material preparation;
[0050] Accurately weigh the required amount of silver nanowires (AgNWs), as well as appropriate amounts of solvent (ethanol) and dispersant (polyvinyl pyrrolidone).
[0051] Step 2: Preliminary mixing;
[0052] The conductive material was slowly added to the solvent while stirring at a low speed with a magnetic stirrer to prevent the material from agglomerating.
[0053] Step 3: ultrasonic dispersion;
[0054] The preliminarily mixed solution is transferred to an ultrasonic cleaner, and appropriate ultrasonic power and time (such as 200 W power and 30 minutes time) are set for ultrasonic dispersion treatment, during which stirring can be stopped from time to time to prevent overheating.
[0055] Step 4: Check the dispersion effect;
[0056] After the ultrasonic dispersion is completed, a small amount of the dispersion is dropped on a glass slide and the dispersion of the conductive material is observed under a microscope to ensure that there is no obvious agglomeration.
[0057] Substrate material pretreatment as follows:
[0058] Step 1: Cleaning;
[0059] Place the base material (such as PI) in a cleaning solution (such as deionized water plus a small amount of detergent), and gently wipe the surface with a soft cloth to remove dust and oil.
[0060] Then rinse with plenty of deionized water and clean again with ethanol or isopropanol to ensure a clean surface.
[0061] Step 2 drying;
[0062] The cleaned substrate material is placed in a drying oven, and an appropriate temperature (such as 60° C.) and time (such as 30 minutes) are set for drying.
[0063] Step 3: surface modification;
[0064] Select appropriate surface modification methods according to needs. For example, use plasma treatment equipment to bombard the surface of the substrate material to increase surface roughness and hydrophilicity; or use chemical etching to form micro-nano structures on the surface of the substrate material to improve adhesion.
[0065] The conductive layer is applied as follows:
[0066] Step 1: Preparation of coating equipment;
[0067] Select a suitable coater, spin coater or spray coater according to laboratory conditions and adjust it to the predetermined working state.
[0068] Step 2 coating operation;
[0069] Fix the pretreated base material on the coating machine and adjust the distance and angle between the coating head and the base material.
[0070] Pour the conductive material dispersion into the coating machine's trough and start the machine for coating. Adjust the coating speed, pressure and number of times according to the type of conductive material and the required thickness.
[0071] Step 3: Uniformity check;
[0072] After coating, the uniformity and thickness of the conductive layer are checked using an optical microscope or a scanning electron microscope (SEM).
[0073] Reinforcement materials are added as follows:
[0074] Step 1: prepare reinforcement materials;
[0075] The required amount of nanocellulose (NFC) is accurately weighed and dispersed in a small amount of solvent to form a uniform suspension.
[0076] Step 2: Add method selection;
[0077] According to the experimental design, the reinforcing material can be added simultaneously during the coating process of the conductive layer, or added by spraying or dipping after the conductive layer is coated and initially dried.
[0078] Step 3: even distribution;
[0079] Regardless of the addition method used, it is necessary to ensure that the reinforcing material can be evenly distributed in the conductive layer without forming agglomerates or affecting the conductive properties.
[0080] Crosslinking and curing are as follows:
[0081] Step 1: Equipment preparation;
[0082] According to the selected cross-linking and curing method (oven curing or UV curing), prepare the corresponding equipment and set the parameters such as temperature, time and atmosphere.
[0083] Step 2: cross-linking and curing;
[0084] Place the base material coated with the conductive layer and the reinforcing material in an oven or UV curing device for crosslinking and curing according to the preset parameters. During this period, pay attention to the changes in the material to prevent overheating or insufficient curing.
[0085] Step 3: Check the curing effect;
[0086] After curing, take out the composite film and observe its surface state and color change. If necessary, preliminary performance tests such as peel strength tests can be carried out to evaluate the cross-linking and curing effects.
[0087] Post-processing and detection are as follows:
[0088] Step 1: cleaning and drying;
[0089] The cured composite film is cleaned to remove residual solvents and impurities on the surface, and then placed in a drying oven for drying to ensure that moisture is completely removed.
[0090] Step 2: Performance test;
[0091] Conduct mechanical property tests (such as tensile strength, elongation at break), electrical conductivity tests (such as resistivity, conductivity) and resistance characteristic tests (such as temperature coefficient, stability) and other test items. Each test must be carried out in accordance with relevant standards or experimental plans to ensure the accuracy and reliability of the data.
[0092] Step 3: Data analysis and evaluation;
[0093] The test data is collated and analyzed to evaluate whether the performance indicators of the composite membrane meet the expected requirements. If necessary, the preparation process can be improved according to the test results.
[0094] An application of the above composite flexible resistor film in a sound sensor.
[0095] The above-mentioned composite flexible resistor film is particularly suitable for the preparation of high-precision electronic components such as sound sensors due to its excellent conductive properties and flexibility. In the sound sensor, the composite flexible resistor film can accurately sense the resistance change caused by sound vibration, thereby realizing the collection and conversion of sound signals. The composite flexible resistor film has lower resistivity, higher conductivity and better flexibility, which can meet the requirements of sound sensors for high precision, high sensitivity and high stability.
[0096] Although embodiments of the present invention have been shown and described, it will be appreciated by those skilled in the art that various changes, modifications, substitutions and variations may be made to the embodiments without departing from the principles and spirit of the present invention, and that the scope of the present invention is defined by the appended claims and their equivalents.
[0097] The standard parts used in the present invention can all be purchased from the market, and the special-shaped parts can be customized according to the description and the drawings. The specific connection methods of each part adopt conventional means such as mature bolts, rivets, welding, etc. in the prior art. The machinery, parts and equipment all adopt conventional models in the prior art, and the circuit connection adopts the conventional connection method in the prior art, which will not be described in detail here. The contents not described in detail in this specification belong to the prior art known to professional and technical personnel in this field.
[0098] In the description of the present invention, the terms "first" and "second" are used for descriptive purposes only and should not be understood as indicating or implying relative importance or implicitly indicating the number of the indicated technical features. Therefore, the features defined as "first" and "second" may explicitly or implicitly include one or more of the features. "Multiple" means two or more, unless otherwise clearly and specifically defined.
[0099] In the present invention, unless otherwise clearly specified and limited, the terms "installed", "connected", "connected", "fixed" and the like should be understood in a broad sense, for example, it can be a fixed connection, a detachable connection, or an integral connection; it can be a mechanical connection or an electrical connection; it can be a direct connection or an indirect connection through an intermediate medium, it can be the internal connection of two elements or the interaction relationship between two elements. For ordinary technicians in this field, the specific meanings of the above terms in the present invention can be understood according to specific circumstances.
[0100] In the present invention, unless otherwise clearly specified and limited, a first feature being "above" or "below" a second feature may mean that the first and second features are in direct contact, or the first and second features are in indirect contact through an intermediate medium. Moreover, a first feature being "above", "above" or "above" a second feature may mean that the first feature is directly above or obliquely above the second feature, or simply means that the first feature is higher in level than the second feature. A first feature being "below", "below" or "below" a second feature may mean that the first feature is directly below or obliquely below the second feature, or simply means that the first feature is lower in level than the second feature.
[0101] In the description of this specification, the description with reference to the terms "one embodiment", "some embodiments", "example", "specific example" or "some examples" etc. means that the specific features, structures, materials or characteristics described in conjunction with the embodiment or example are included in at least one embodiment or example of the present invention. In this specification, the schematic representations of the above terms do not necessarily refer to the same embodiment or example. Moreover, the specific features, structures, materials or characteristics described may be combined in any one or more embodiments or examples in a suitable manner. In addition, those skilled in the art may combine and combine the different embodiments or examples described in this specification and the features of the different embodiments or examples, unless they are contradictory.
[0102] In the drawings of the embodiments disclosed in the present invention, only the structures related to the embodiments disclosed in the present invention are involved, and other structures can refer to the general design. In the absence of conflict, the same embodiment and different embodiments of the present invention can be combined with each other.
[0103] Although the present invention has been described in detail with reference to the aforementioned embodiments, it is still possible for those skilled in the art to modify the technical solutions described in the aforementioned embodiments, or to make equivalent substitutions for some of the technical features therein. Any modifications, equivalent substitutions, improvements, etc. made within the spirit and principles of the present invention should be included in the protection scope of the present invention.
Claims
1. A composite flexible resistor film, characterized in that: Includes the following materials: Base materials, conductive materials, reinforcing materials, solvents and dispersants, and cross-linking agents and curing agents; The base material is polyimide, the conductive material is nano silver wire, the reinforcing material is nano cellulose, the solvent and dispersant are selected to be suitable for the conductive material, namely ethanol and the dispersant is polyvinyl pyrrolidone, and the crosslinking agent and curing agent are selected to be plant-based epoxy resin and isocyanate.
2. A method for preparing a composite flexible resistor film, applicable to the composite flexible resistor film according to claim 1, characterized in that: The following steps are involved: S1. Preparation of conductive material dispersion: adding conductive material nanosilver wires into a solvent and adding an appropriate amount of dispersant, and preparing a uniform conductive material dispersion by stirring and ultrasonic dispersion treatment; S2. Pretreatment of substrate materials: cleaning, drying and surface modification of the substrate materials; S3. Conductive layer coating: Use one of the following equipment: a coater, a spin coater, or a spray coater to evenly coat the conductive material dispersion on the pretreated base material, and control the coating thickness and speed; S4. Addition of reinforcing materials: During and after the coating of the conductive layer, an appropriate amount of reinforcing materials is added, and the reinforcing materials are evenly distributed in the conductive layer by stirring or spraying; S5, cross-linking and curing: placing the base material coated with the conductive layer and the reinforcing material in a UV curing device for cross-linking and curing, and controlling the temperature, time and atmosphere conditions of the cross-linking and curing; S6. Post-processing and testing: The cured composite film is cleaned and dried to remove residual solvents and impurities, and tests including but not limited to mechanical properties test, electrical conductivity test and resistance characteristic test are carried out to verify whether the performance indicators of the composite film meet the requirements.
3. The method for preparing a composite flexible resistor film according to claim 2, characterized in that: In step S1, after the ultrasonic dispersion is completed, a small amount of dispersion liquid is dropped on a glass slide, and the dispersion of the conductive material is observed using a microscope to ensure that there is no obvious agglomeration.
4. The method for preparing a composite flexible resistor film according to claim 2, characterized in that: In step S3, after coating, the uniformity and thickness of the conductive layer are checked using a scanning electron microscope (SEM).
5. The method for preparing a composite flexible resistor film according to claim 2, characterized in that: In step S5, after the curing is completed, the composite film is taken out, and its surface state and color change are observed. If necessary, a preliminary performance test, such as a peel strength test, is performed to evaluate the cross-linking and curing effects.
6. Use of the composite flexible resistor film according to claim 1 in a sound sensor.