Semiconductor oxide film and preparation method thereof

By introducing a multi-layer structure into the semiconductor oxide film, including a metal oxide layer of In and/or Sn, a second metal oxide layer and a third rare earth metal oxide layer, ALD technology is used to control the carrier concentration and microstructure. , solves the problem of poor thermal stability and photostability of TFT devices in the existing technology, and achieves high mobility and excellent photothermal stability.

CN118872065APending Publication Date: 2024-10-29SOUTH CHINA UNIV OF TECH
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202480001821.9
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-03-06
Publication Date
2024-10-29

AI Technical Summary

Technical Problem

Existing metal oxide TFT devices have problems with poor thermal stability and photostability, making it difficult to achieve high mobility and excellent photothermal stability using semiconductor oxide film deposition methods.

Method used

A multi-layer metal oxide film structure is adopted, including a metal oxide layer of In and/or Sn, two second metal oxide layers with different functions and a third rare earth metal oxide layer, through atomic layer deposition (ALD) deposition, regulating carrier concentration and microstructure to improve photothermal stability.

Benefits of technology

A semiconductor oxide film with high mobility and excellent photothermal stability is achieved, which is suitable for active layer materials of thin film transistors and ensures the density and uniformity of composition distribution of the material.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure BDA0005029909560000121
    Figure BDA0005029909560000121
  • Figure BDA0005029909560000131
    Figure BDA0005029909560000131
  • Figure BDA0005029909560000132
    Figure BDA0005029909560000132
Patent Text Reader

Abstract

The invention provides a semiconductor oxide thin film and a preparation method thereof. The semiconductor oxide thin film comprises a plurality of metal oxide layers, the composition general formula of the multiple metal oxide layers is AO [alpha] BO [beta] RO [gamma], wherein [alpha], [beta] and [gamma] are cycle times of the AO layer, the BO layer and the RO layer respectively; aO is an oxide layer of the first metal, BO is an oxide layer of the second metal, and RO is an oxide layer of the third rare earth metal. According to the semiconductor oxide film, the second metal oxide layer and the third rare earth metal oxide layer which have different functions are introduced into the metal oxide layer of In and / or Sn at the same time through regulation and control of components and the structure, so that the photo-thermal stability of the semiconductor oxide film is improved. According to the preparation method, related parameters of the ALD deposition process are controlled, so that the prepared semiconductor oxide thin film is extremely high in density, uniform in component microcell distribution, easy to accurately control and excellent in surface appearance coverage.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present application belongs to the technical field of semiconductor materials and devices, and relates to a semiconductor oxide film and a preparation method thereof. Background Art

[0002] The core technology of the new flat panel display industry is the thin film transistor (TFT) backplane technology. Metal oxide TFT (MO-TFT) not only has high mobility, but also has a relatively simple and diverse manufacturing process, is compatible with the current a-Si process, has low manufacturing costs, and has excellent large-area uniformity. Therefore, MO-TFT technology has attracted much attention from the industry since its birth.

[0003] There are many types of inorganic metal oxide semiconductor materials and preparation methods currently in use. The commercial semiconductor oxide thin film production method is mainly based on vacuum sputtering technology (such as physical vapor deposition PVD). Although the sputtering method has the advantage of rapid film formation, in terms of raw material formulation and target material preparation, the high-mobility multi-component rare earth doping formula design and large-area target material sintering face many difficulties, including: target material nodule problem, poor target material density, poor target material uniformity, etc. Therefore, in terms of semiconductor thin film deposition methods, atomic layer deposition (ALD) is a very potential thin film preparation method that may compete with the sputtering process.

[0004] ALD can achieve good composition control using simple raw materials and can deposit high-quality nano-scale oxide films. In addition, since ALD is an atomic-level deposition process, it has obvious advantages in achieving precise doping of trace elements, and the self-limiting deposition mechanism of ALD makes it have good three-dimensional conformality, which can be well deposited on three-dimensional or porous materials. In addition, low-temperature growth (<250°C) is also a major advantage of ALD.

[0005] However, TFT devices currently made of metal oxides have poor thermal stability and photostability. Therefore, developing a semiconductor oxide film with excellent photostability is of extraordinary significance for the industrial application of oxide thin film transistors. Summary of the invention

[0006] The following is a summary of the subject matter described in detail herein. This summary is not intended to limit the scope of the claims.

[0007] The purpose of the present application is to provide a semiconductor oxide thin film and a method for preparing the same. The semiconductor oxide thin film achieves a higher mobility while introducing two second metal oxide layers and a third rare earth metal oxide layer with different functions to obtain a semiconductor oxide thin film with excellent photothermal stability, which can be used as an active layer material for a thin film transistor.

[0008] To achieve this goal, this application adopts the following technical solutions:

[0009] In a first aspect, the present application provides a semiconductor oxide film, wherein the semiconductor oxide film comprises a plurality of metal oxide layers;

[0010] The composition formula of the multi-layer metal oxide layer is AO α BO β RO γ , where α, β, and γ are the number of cycles of AO layer, BO layer, and RO layer, respectively; AO is the oxide layer of the first metal, BO is the oxide layer of the second metal, and RO is the oxide layer of the third rare earth metal.

[0011] The semiconductor oxide film described in the present application has extremely high density, uniform and easy to accurately control the micro-region distribution of components, and excellent surface morphology coverage. In addition, the semiconductor oxide film is composed of three metal oxide layers of different materials, and two second metal oxide layers and a third rare earth metal oxide layer with different functions are simultaneously introduced into the metal oxide layer of In and / or Sn, thereby improving the light and heat stability of the semiconductor oxide film.

[0012] It is worth noting that the oxide layer of the first metal in the semiconductor oxide film described in the present application is mainly the source of carriers and determines the upper limit of the mobility of the oxide material; the oxide layer of the second metal is mainly to adjust the microstructure of the oxide film, such as the crystal state of the material (crystalline and amorphous), and can also inhibit the formation of oxygen vacancies and improve the controllability of the carrier transport process; the third rare earth metal oxide layer is mainly rare earth doping to improve the photothermal stability of the material. Rare earth elements are doped into the oxide system, which can induce shallow energy level defect states in the oxide system. The defect states can serve as recombination centers for photogenerated carriers and holes, thereby improving the optical bias stability of materials and devices. The main mechanism is that the rare earth elements doped into the oxide substrate can induce shallow energy level "acceptor defects" near the Fermi level, which can act as oxygen vacancies Vo. 2+ The recombination center with electrons can improve the light bias stability problem caused by oxygen vacancies in the device.

[0013] As an optional technical solution of the present application, the first metal includes In and / or Sn.

[0014] In one embodiment, the second metal includes any one of Zn, Ga, Ta, W, Bi, Hf, Zr, Ti, Mo or Ge, or a combination of at least two of them, wherein the combination is typical but not limiting. The combination includes: a combination of Zn and Ga, a combination of Ta and W, a combination of Bi and Hf, or a combination of Zr and Ti, etc.

[0015] In one embodiment, the third rare earth metal includes any one of Sc, Y, Ce, Pr, Tb, Dy or Yb, or a combination of at least two of them, wherein the combinations are typical but not limiting: a combination of Sc and Y, a combination of Ce and Pr, a combination of Tb and Dy, or a combination of Yb and Dy, etc.

[0016] As an optional technical solution of the present application, the ratio of α and β in the multi-layer metal oxide layer is (1-20):1, for example, it can be 2:1, 4:1, 5:1, 7:1, 9:1, 10:1, 12:1, 14:1, 15:1, 17:1 or 19:1, but is not limited to the listed values, and other unlisted values ​​within the numerical range are also applicable.

[0017] In one embodiment, the ratio of α to γ ​​in the multilayer metal oxide layer is (10-100):1, for example, it can be 20:1, 30:1, 40:1, 50:1, 60:1, 70:1, 80:1 or 90:1, but is not limited to the listed values, and other unlisted values ​​within the numerical range are also applicable.

[0018] It is worth noting that the AO material layer is mainly used as a transport channel layer, and the more layers it has, the higher the mobility. However, as the AO layer increases, its corresponding film is easier to crystallize. Due to the scattering effect of the grain boundary, the mobility will be reduced. At the same time, since the AO material itself has a low AO bond energy and there are many defects in the film, the increase of the AO layer will usually also lead to the decline of the photothermal stability of the final device; the present application mainly controls the microstructure of the oxide material system film by regulating the layer ratio of the AO layer and the BO layer in the multilayer metal oxide layer to (1-20): 1, and then regulates the carrier concentration and mobility. And the layer ratio of the AO layer and the RO layer in the multilayer metal oxide layer is regulated to (10-100): 1, mainly through the doping amount of rare earth elements, thereby adjusting the photothermal stability of the device; the lower the layer ratio, the better the stability, but the mobility is also at risk of decreasing. Therefore, it is necessary to comprehensively consider the layer ratio relationship of AO / BO / RO to ensure the high mobility, high controllability and high stability of the semiconductor oxide film.

[0019] As an optional technical solution of the present application, the thickness of the semiconductor oxide film is For example it could be or etc., but not limited to the listed values. Other values ​​not listed in the numerical range are also applicable and can be selected as

[0020]

[0021] In one embodiment, the carrier concentration of the semiconductor oxide film is 10 14 -10 21 cm -3 , for example, it can be 10 15 cm -3 , 10 16 cm -3 , 10 17 cm -3 , 10 18 cm -3 , 10 19 cm -3 or 10 19 cm -3 etc., but not limited to the listed values. Other values ​​not listed in the numerical range are also applicable, and can be selected as 10 16 -10 20 cm -3 .

[0022] It is worth noting that the carrier concentration determines the upper limit of the mobility of the oxide material. By organically regulating the carrier concentration, a high-mobility TFT device can be obtained. Generally speaking, the higher the carrier concentration, the higher the mobility. This is determined by the carrier transport mechanism of the oxide material system, which is called the percolation threshold theory. However, too high a carrier concentration will lead to a scattering effect between particles, and there is a risk of decreased mobility. Therefore, this application controls the carrier concentration of the semiconductor oxide film to 10 14 -10 21 cm -3 range, resulting in a higher mobility.

[0023] In this application, it is necessary to strictly and accurately control the element type, film thickness parameters, film microstructure and carrier concentration parameters of the semiconductor oxide film to match, so as to achieve a semiconductor oxide thin film transistor with high mobility and high stability.

[0024] In a second aspect, the present application provides a method for preparing a semiconductor oxide thin film as described in the first aspect, the preparation method comprising:

[0025] Cyclic deposition of AO on substrate using atomic layer deposition α / n BO β / n RO γ / n , to obtain the semiconductor oxide film; wherein n is the number of cyclic deposition times.

[0026] In the present application, a sub-cycle of deposition (AO layer+BO layer+RO layer) is first performed, and then n sub-cycles are deposited in a cycle to obtain a semiconductor oxide thin film.

[0027] As an optional technical solution of the present application, the preparation method specifically includes:

[0028] The substrate is placed in an atomic layer deposition reaction device, and a first metal source precursor, an inert gas and an oxygen source are introduced into the reaction device in sequence to deposit an α / n AO layer; then a second metal source precursor, an inert gas and an oxygen source are introduced into the reaction device in sequence to deposit a β / n BO layer; then a third rare earth metal source precursor, an inert gas and an oxygen source are introduced into the reaction device in sequence to deposit a γ / n RO layer; finally, the semiconductor oxide film is obtained through cyclic deposition.

[0029] As an optional technical solution of the present application, the number of cyclic deposition is 10-200, for example, it can be 20, 30, 50, 70, 90, 100, 120, 140, 150, 170 or 190, but is not limited to the listed values, and other unlisted values ​​within the numerical range are also applicable.

[0030] In one embodiment, the first metal source precursor includes an In source and / or a Sn source.

[0031] In the present application, the In source includes any one of trimethylindium (TMIn), dimethylethylindium (DMEI), cyclopentadienylindium (InCp), [3-(dimethylamino)propyl]dimethylindium (DADI) or (N,N-dimethylbutylamine)trimethylindium (DATI) or a combination of at least two thereof.

[0032] In the present application, the Sn source includes any one of SnCl4, tetra(dimethylamine)tin (TDMASn) or bis(N,N'-di-iso-propylacetamidine)tin(II)Sn(iPr-MeAMD)2 or a combination of at least two thereof.

[0033] In one embodiment, the pulse time of the first metal source precursor is 0.03-2s, for example, it can be 0.05s, 0.07s, 0.1s, 0.3s, 0.5s, 0.7s, 0.9s, 1s, 1.1s, 1.3s, 1.5s, 1.7s or 1.9s, but is not limited to the listed values, and other unlisted values ​​within the numerical range are also applicable.

[0034] In one embodiment, the flow rate of the first metal source precursor is 10-500sccm, for example, it can be 30sccm, 50sccm, 70sccm, 100sccm, 150sccm, 200sccm, 250sccm, 300sccm, 350sccm, 400sccm or 450sccm, but is not limited to the listed values, and other unlisted values ​​within the numerical range are also applicable.

[0035] In one embodiment, the chemical source temperature of the first metal source precursor is 50-130°C, for example, it can be 60°C, 70°C, 80°C, 90°C, 100°C, 110°C or 120°C, but is not limited to the listed values, and other unlisted values ​​within the numerical range are also applicable.

[0036] In one embodiment, the thin film deposition temperature of the first metal source precursor is 150-300°C, for example, it can be 160°C, 170°C, 200°C, 220°C, 240°C, 250°C, 270°C or 290°C, but is not limited to the listed values, and other unlisted values ​​within the numerical range are also applicable.

[0037] In one embodiment, the plasma power for depositing the AO layer is 50-300 W, for example, 60 W, 70 W, 90 W, 100 W, 120 W, 150 W, 170 W, 200 W, 220 W, 250 W, 270 W or 290 W, but is not limited to the listed values, and other unlisted values ​​within the numerical range are also applicable.

[0038] As an optional technical solution of the present application, the second metal source precursor includes any one of Zn source, Ga source, Ta source, W source, Bi source, Hf source, Zr source, Ti source, Mo source or Ge source, or a combination of at least two of them.

[0039] In the present application, the Zn source includes diethyl zinc (DEZ); the Ga source includes trimethyl gallium (TMGa) and / or triethyl gallium (TEGa); the Ta source includes any one of tert-butylamine tri(diethylamine) tantalum (TBTDEAT), tert-butylamine tri(ethylmethylamine) tantalum (TBTEMAT) or penta(dimethylamine) tantalum (PDMAT) or a combination of at least two thereof; the W source includes di-tert-butylamine bis(dimethylamine) tungsten (BTBMW) and / or WF6; the Bi source includes bismuth heptanedione (Bi(thd)2); the Hf source includes tetra(dimethylamine) hafnium (TDMAHf), tetra(ethylamine) The Zr source includes any one of tetrakis(dimethylamino)zirconium (TDMAZr), tetrakis(ethylmethylamino)zirconium (TEMAZr) or cyclopentadienyl zirconium (CpZr) or a combination of at least two of them; the Ti source includes any one of TiCl4, tetrakis(ethylmethylamino)titanium (TDMATi) or titanium tetraisopropoxide (TTIP) or a combination of at least two of them; the Mo source includes bis(tert-butylimino)bis(dimethylamino)molybdenum(VI); and the Ge source includes tetrakis(dimethylamino)germanium.

[0040] In one embodiment, the pulse time of the second metal source precursor is 0.01-1.5s, for example, it can be 0.03s, 0.05s, 0.07s, 0.1s, 0.3s, 0.5s, 0.7s, 0.9s, 1s, 1.1s, 1.3s or 1.4s, but is not limited to the listed values, and other unlisted values ​​within the numerical range are also applicable.

[0041] In one embodiment, the flow rate of the second metal source precursor is 20-300sccm, for example, it can be 30sccm, 50sccm, 70sccm, 90sccm, 100sccm, 120sccm, 150sccm, 170sccm, 200sccm, 220sccm, 250sccm, 270sccm or 290sccm, but is not limited to the listed values, and other unlisted values ​​within the numerical range are also applicable.

[0042] In one embodiment, the chemical source temperature of the second metal source precursor is 20-100°C, for example, it can be 30°C, 40°C, 50°C, 60°C, 70°C, 80°C or 90°C, but is not limited to the listed values, and other unlisted values ​​within the numerical range are also applicable.

[0043] In one embodiment, the thin film deposition temperature of the second metal source precursor is 150-300°C, for example, it can be 160°C, 170°C, 200°C, 220°C, 240°C, 250°C, 270°C or 290°C, but is not limited to the listed values, and other unlisted values ​​within the numerical range are also applicable.

[0044] In one embodiment, the plasma power for depositing the BO layer is 50-200 W, for example, 60 W, 70 W, 80 W, 100 W, 120 W, 140 W, 150 W, 170 W or 190 W, but is not limited to the listed values, and other unlisted values ​​within the numerical range are also applicable.

[0045] As a preferred technical solution of the present application, the third rare earth metal source precursor includes any one of a Sc source, a Y source, a Ce source, a Pr source, a Tb source, a Dy source or a Yb source, or a combination of at least two thereof.

[0046] In the present application, the Sc source includes tris(2,2,6,6-tetramethyl-3,5-heptanedione)scandium Sc(thd)3; the Y source includes tris(2,2,6,6-tetramethyl-3,5-heptanedione)yttrium Y(thd)3 and / or tris(cyclopentadienyl)yttrium (MeCp)3Y; the Ce source includes tetra(2,2,6,6-tetramethyl-3,5-heptanedione)cerium Ce(thd)4; the Pr source includes tris(2,2,6,6-tetramethyl-3,5-heptanedione)praseodymium Pr(thd)3 and / or triisopropylcyclopentadienylpraseodymium ( The invention relates to a novel terbium source comprising tris(2,2,6,6-tetramethyl-3,5-heptanedione)terbium Tb(thd)3 and / or triisopropylcyclopentadienylterbium (iPCp)3Tb; the dyne source comprises tris(2,2,6,6-tetramethyl-3,5-heptanedione)dysprosium Dy(thd)3 and / or triisopropylcyclopentadienyldysprosium (iPCp)3Dy; the yb source comprises tris(2,2,6,6-tetramethyl-3,5-heptanedione)ytterbium Yb(thd)3 and / or triisopropylcyclopentadienylytterbium (iPCp)3Yb.

[0047] In one embodiment, the pulse time of the third rare earth metal source precursor is 0.05-3s, for example, it can be 0.07s, 0.1s, 0.3s, 0.5s, 0.7s, 0.9s, 1s, 1.1s, 1.3s, 1.5s, 1.7s, 2s, 2.1s, 2.3s, 2.5s, 2.7s or 2.9s, but is not limited to the listed values, and other unlisted values ​​within the numerical range are also applicable.

[0048] In one embodiment, the flow rate of the third rare earth metal source precursor is 50-500sccm, for example, it can be 100sccm, 150sccm, 200sccm, 250sccm, 300sccm, 350sccm, 400sccm or 450sccm, but is not limited to the listed values, and other unlisted values ​​within the numerical range are also applicable.

[0049] In one embodiment, the chemical source temperature of the third rare earth metal source precursor is 60-150°C, for example, it can be 70°C, 80°C, 90°C, 100°C, 110°C, 120°C, 130°C or 140°C, but is not limited to the listed values, and other unlisted values ​​within the numerical range are also applicable.

[0050] In one embodiment, the thin film deposition temperature of the third rare earth metal source precursor is 150-300°C, for example, it can be 160°C, 170°C, 200°C, 220°C, 240°C, 250°C, 270°C or 290°C, but is not limited to the listed values, and other unlisted values ​​within the numerical range are also applicable.

[0051] In one embodiment, the plasma power for depositing the RO layer is 100-500 W, for example, 150 W, 200 W, 250 W, 300 W, 350 W, 400 W or 450 W, but is not limited to the listed values, and other values ​​not listed within the numerical range are also applicable.

[0052] As an optional technical solution of the present application, the purge time of the inert gas is 5-30s, for example, it can be 7s, 9s, 10s, 12s, 15s, 17s, 19s, 20s, 22s, 25s, 27s or 29s, but is not limited to the listed values, and other unlisted values ​​within the numerical range are also applicable.

[0053] In the present application, the inert gas includes nitrogen.

[0054] In one embodiment, the oxygen source includes any one of O2, H2O, H2O2, O3 or oxygen plasma, or a combination of at least two of them, wherein the combination is typically but not limited to: a combination of O2 and H2O, a combination of H2O and H2O2, or a combination of oxygen plasma and O3, etc.

[0055] In one embodiment, the pulse time of the oxygen source is 0.2-50 s, for example, 0.5 s, 1 s, 3 s, 5 s, 7 s, 9 s, 10 s, 15 s, 20 s, 25 s, 30 s, 35 s, 40 s or 45 s, but is not limited to the listed values, and other values ​​not listed within the numerical range are also applicable.

[0056] In the present application, when depositing different metal oxide layers, the flow rate and pulse time of the oxygen source are not the same, and no specific limitation is made here, as long as the introduced oxygen source reacts with the metal source precursor substance to generate the corresponding metal oxide molecular layer.

[0057] The numerical range described in this application includes not only the point values ​​listed above, but also any point values ​​between the above numerical ranges that are not listed. Due to limited space and for the sake of brevity, this application no longer exhaustively lists the specific point values ​​included in the range.

[0058] Compared with the prior art, this application has the following beneficial effects:

[0059] (1) The semiconductor oxide film provided by the present application is composed of three metal oxide layers of different materials at the atomic layer thickness level through the regulation of composition and structure. In the metal oxide layer of In and / or Sn, two second metal oxide layers and a third rare earth metal oxide layer with different functions are simultaneously introduced, thereby improving the light and heat stability of the semiconductor oxide film;

[0060] (2) The preparation method provided in the present application controls the relevant parameters of the ALD deposition process, so that the obtained semiconductor oxide film has extremely high density, uniform and easy to accurately control the micro-region distribution of components, and excellent surface morphology coverage.

[0061] Still other aspects will be apparent upon reading and understanding the detailed description. DETAILED DESCRIPTION

[0062] The technical solution of the present application is further described below through specific implementation methods. Those skilled in the art should understand that the embodiments are only to help understand the present application and should not be regarded as specific limitations of the present application.

[0063] The semiconductor oxide thin films prepared in the following examples and comparative examples were tested for thickness and carrier concentration. The semiconductor oxide thin films were deposited on Si wafer substrates and the thickness was tested using an ellipsometer; the semiconductor oxide thin films were deposited on glass substrates with a thickness of The semiconductor oxide film is tested with a Hall tester to measure the carrier concentration of the film.

[0064] The semiconductor oxide thin films prepared in the following examples and comparative examples were made into TFT devices and subjected to a light thermal stability (NBITS) test. The drift (ΔVth) of the threshold voltage Vth of the TFT device was measured when the TFT device was under a negative gate bias (negative bias, Vgs = -30V) and the device was heated (temperature, 60°C) and illuminated (illumination, 15000nits).

[0065] The manufacturing process of the TFT device includes the following steps:

[0066] (1) Depositing a buffer layer SiO2 on a glass substrate;

[0067] (2) ALD preparation of oxide active layer thin film material; patterning etching; annealing treatment;

[0068] (3) depositing an insulating layer SiO2 and a metal gate Mo; performing patterning and self-aligned dry etching to form an SD contact area;

[0069] (4) depositing an interlayer insulating layer SiO2; performing patterning etching;

[0070] (5) Depositing source / drain electrodes S / D; performing patterning etching;

[0071] (6) Deposit a protective layer of SiO2; perform patterning etching.

[0072] Example 1

[0073] This embodiment provides a semiconductor oxide film and a preparation method thereof, wherein the semiconductor oxide film comprises a plurality of metal oxide layers; the composition formula of the plurality of metal oxide layers is (In2O3) 300 (ZnO) 30 (Sc2O3) 10 ;

[0074] The method for preparing the semiconductor oxide thin film comprises the following steps:

[0075] (1) The substrate was placed in an atomic layer deposition reactor, and a TMIn pulse was introduced into the reactor at a flow rate of 240 sccm for 1 s, and then nitrogen was introduced for 20 s to remove excess TMIn from the chamber, and then an oxygen plasma pulse was introduced at a flow rate of 240 sccm for 20 s to perform 30 In2O3 layer depositions;

[0076] The temperature of the chemical source for introducing TMIn is 50°C; the temperature of the In2O3 layer deposition is 200°C and the plasma power is 230W;

[0077] (2) After the oxygen plasma pulse in step (1) is completed, a DEZ pulse is introduced into the reaction device at a flow rate of 150 sccm for 0.8 s, and then nitrogen is introduced for 20 s to remove excess DEZ material from the cavity, and then an oxygen plasma pulse is introduced at a flow rate of 100 sccm for 10 s to perform three ZnO layer depositions;

[0078] The temperature of the chemical source introduced into DEZ is 25°C; the temperature of the ZnO layer deposition is 200°C and the plasma power is 120W;

[0079] (3) After the oxygen plasma pulse in step (2) is completed, a Sc(thd)3 pulse is introduced into the reaction device at a flow rate of 240 sccm for 1.5 s, and then nitrogen is introduced for 20 s to remove excess Sc(thd)3 from the cavity. Thereafter, an oxygen plasma pulse is introduced at a flow rate of 240 sccm for 30 s to perform one Sc2O3 layer deposition;

[0080] The temperature of the chemical source for introducing Sc(thd)3 is 100°C; the temperature of the Sc2O3 layer deposition is 200°C and the plasma power is 300W;

[0081] (4) The operation from step (1) to step (3) is regarded as a large cycle, and the large cycle is repeated 10 times to obtain the semiconductor oxide film.

[0082] Example 2-11

[0083] The types of metal oxides in each layer and the chemical source temperature parameters of the precursor were changed, as shown in Table 1. Other conditions were the same as those in Example 1. The film performance test results are shown in Table 1.

[0084] Table 1

[0085]

[0086]

[0087] It can be seen from Table 1 that the semiconductor oxide thin film and its preparation method provided in the present application, while achieving higher mobility, a semiconductor oxide thin film with excellent photothermal stability is obtained by introducing two second metal oxide layers and a third rare earth metal oxide layer with different functions and controlling the carrier concentration, and can be used as an active layer material for thin film transistors.

[0088] Examples 12-14

[0089] The layer ratio parameters of the AO / BO layer and the AO / RO layer were changed as shown in Table 2. The other conditions were the same as those in Example 1. The film performance test results are shown in Table 2.

[0090] Table 2

[0091]

[0092] It can be seen from Table 2 that: when the layer ratio of the AO layer and the BO layer is too small, the content of the AO layer (In or Sn) as the main source of carriers is relatively reduced, which makes the growth rate of the obtained semiconductor oxide thin film significantly increased, resulting in a decrease in the carrier concentration of the film and improved photothermal stability; when the layer ratio of the AO layer and the BO layer is too large, the content of the AO layer (In or Sn) as the main source of carriers is relatively increased, so that the growth rate of the obtained semiconductor oxide thin film is slightly decreased, and at the same time, due to the increase in the carrier concentration of the film, the photothermal stability is significantly deteriorated; when the layer ratio of the AO layer and the RO layer is too small, the content of the RO layer as a carrier inhibitor is relatively increased, so that the growth rate of the obtained semiconductor oxide thin film is slightly increased, resulting in a decrease in the carrier concentration of the film and improved photothermal stability.

[0093] Examples 15-16

[0094] The chemical source temperature parameters of the first metal source precursor were changed as shown in Table 3. The other conditions were the same as those in Example 1. The film performance test results are shown in Table 3.

[0095] Table 3

[0096]

[0097] It can be seen from Table 3 that: when the chemical source temperature of the first metal source precursor is too low, the precursor cannot effectively enter the chamber for adsorption-reaction because the vapor pressure temperature of the precursor is too low, which causes the growth rate of the obtained semiconductor oxide film to drop significantly, and the film thickness decreases, but the carrier concentration and photothermal stability are not much different; when the chemical source of the first metal source precursor is too high, because the vapor pressure of the precursor has reached the saturated vapor pressure of the material itself, the growth rate of the obtained semiconductor oxide film does not change much, and the carrier concentration and photothermal stability are also not much different, but the production cost is increased.

[0098] Examples 17-19

[0099] The plasma power parameters of the AO layer deposition were changed as shown in Table 4. The other conditions were the same as those in Example 1. The film performance test results are shown in Table 4.

[0100] Table 4

[0101]

[0102] It can be seen from Table 4 that: when the power of AO layer deposition is too low, due to the low power density of plasma, the precursor reaction activity of film growth is reduced, the precursor site reaction is incomplete, the growth rate of the obtained semiconductor oxide film is significantly reduced, the carrier concentration of the film is significantly reduced, and the photothermal stability does not change significantly; when the power of AO layer deposition is too high, due to the high power density of plasma, the precursor reaction activity of film growth is reduced, the precursor site reaction is complete, the growth rate of the obtained semiconductor oxide film is significantly increased, the carrier concentration of the film does not change significantly, but due to the increase in the content of AO layer, the photothermal stability is significantly deteriorated. And as the AO layer deposition power continues to increase, due to the self-etching effect of plasma itself, that is, the two processes of film growth and film etching occur simultaneously, excessive power will cause the film etching effect to become more obvious, resulting in a slight decrease in the thickness of the film.

[0103] Embodiment 20

[0104] This embodiment provides a semiconductor oxide film and a preparation method thereof, wherein the semiconductor oxide film comprises a plurality of metal oxide layers; the composition formula of the plurality of metal oxide layers is (In2O3) 300 (TiO2) 30 (Sc2O3) 10 ;

[0105] The method for preparing the semiconductor oxide film is the same as that in Example 1, except that step (2) is adjusted as follows: after the oxygen plasma pulse in step (1) ends, a TDMATi pulse is introduced into the reaction device at a flow rate of 150 sccm for 0.3 s, and then nitrogen is introduced for 15 s to remove excess TDMATi material from the cavity, and then an oxygen plasma pulse is introduced at a flow rate of 150 sccm for 15 s to perform three TDMATi layer depositions; other conditions are the same as those in Example 1.

[0106] Examples 21-23

[0107] The layer ratio parameters of the AO / BO layer were changed as shown in Table 5. The other conditions were the same as those in Example 20. The film performance test results are shown in Table 5.

[0108] Table 5

[0109]

[0110] It can be seen from Table 5 that: when the layer ratio of the AO layer and the BO layer is too large, the content of the BO layer as the main source of carrier inhibitors is relatively reduced, so that the growth rate of the obtained semiconductor oxide film is slightly decreased, and at the same time, the carrier concentration of the film increases, but the photothermal stability is seriously deteriorated; when the layer ratio of the AO layer and the BO layer is too small, the content of the BO layer as the main source of carrier inhibitors is relatively increased, so that the growth rate of the obtained semiconductor oxide film is slightly increased, but the carrier concentration of the film decreases, and the photothermal stability is significantly improved; when the BO layer content is further increased (AO / BO=300 / 150), the BO layer is difficult to play the role of carrier suppression of the AO layer due to its own crystallization phenomenon, and the photothermal stability will be deteriorated to a certain extent.

[0111] Examples 24-25

[0112] The plasma power parameters of BO layer deposition were changed as shown in Table 6. Other conditions were the same as those in Example 1. The film performance test results are shown in Table 6.

[0113] Table 6

[0114]

[0115] It can be seen from Table 6 that: when the power of BO layer deposition is too low, due to the low power density of plasma, the reaction activity of the precursor for film growth is reduced, the site reaction of the precursor is incomplete, and the growth rate of the obtained semiconductor oxide film is significantly reduced; in addition, the content of the BO layer as a carrier inhibitor is reduced, the carrier concentration of the film will increase, and there is a risk of deterioration of the photothermal stability; when the power of BO layer deposition is too high, although the power density of plasma is high, the site reaction of the precursor is basically complete, resulting in the film growth rate change is not obvious, the carrier concentration of the film does not change significantly, and the photothermal stability does not change significantly.

[0116] Examples 26-27

[0117] The chemical source temperature parameters of the third rare earth metal source precursor were changed as shown in Table 7. The other conditions were the same as those in Example 1. The film performance test results are shown in Table 7.

[0118] Table 7

[0119]

[0120]

[0121] It can be seen from Table 7 that: when the chemical source temperature of the third metal source precursor is too low, the precursor cannot effectively enter the chamber for adsorption-reaction because the vapor pressure temperature of the precursor is too low, which causes the RO layer content of the obtained semiconductor oxide film to decrease significantly, and the carrier concentration to increase, but the photothermal stability to deteriorate significantly; when the chemical source temperature of the third metal source precursor is too high, because the vapor pressure of the precursor has reached the saturated vapor pressure of the material itself, the growth rate of the obtained semiconductor oxide film does not change much, but the RO layer can be fully bonded with the AO layer, resulting in a decrease in the carrier concentration and a significant improvement in the photothermal stability.

[0122] Examples 28-29

[0123] The plasma power parameters of the RO layer deposition were changed as shown in Table 8. The other conditions were the same as those in Example 1. The film performance test results are shown in Table 8.

[0124] Table 8

[0125]

[0126] It can be seen from Table 8 that: when the power of RO layer deposition is too low, due to the low power density of plasma, the reaction activity of the precursor for film growth is reduced, and the site reaction of the precursor is incomplete, which makes the RO layer content of the obtained semiconductor oxide film significantly reduced, and the carrier concentration is significantly reduced, resulting in a significant deterioration of the photothermal stability; when the power of RO layer deposition is too high, although the power density of plasma is high, the site reaction of the precursor is basically complete, resulting in the film growth rate change is not obvious, the carrier concentration of the film does not change significantly, and the photothermal stability does not change significantly.

[0127] Comparative Examples 1-3

[0128] The composition parameters of the semiconductor oxide film were changed as shown in Table 9. The other conditions were the same as those in Example 1. The film performance test results are shown in Table 9.

[0129] Table 9

[0130]

[0131] It can be seen from Table 9 that: when the BO layer is not deposited, due to the lack of carrier inhibitors and film growth crystal control agents, the carrier concentration of the obtained semiconductor oxide film is relatively high, the TFT device is difficult to control the switching performance, and the photothermal stability is significantly deteriorated; when the RO layer is not deposited, due to the lack of passivation and inhibition of oxygen vacancy defects in the film, the carrier concentration of the obtained semiconductor oxide film is relatively high, the TFT device is difficult to control the switching performance, and the photothermal stability is significantly deteriorated; when the semiconductor oxide film is a single-layer metal oxide layer, that is, all metal oxides are mixed and deposited, because each layer of material cannot use its own sites to react with the oxidant for oxidation, the growth rate of the film is significantly reduced, so that the carrier concentration of the obtained semiconductor oxide film is reduced (especially the AO layer), and at the same time, since the BO / RO layers fail to form films and bonds effectively, the photothermal stability will be significantly reduced.

Claims

1. A semiconductor oxide film, the composition of which includes multiple metal oxide layers; The composition formula of the multi-layer metal oxide layer is AO α BO β RO γ , where α, β, and γ are the number of cycles of AO layer, BO layer, and RO layer, respectively; AO is the oxide layer of the first metal, BO is the oxide layer of the second metal, and RO is the oxide layer of the third rare earth metal.

2. The semiconductor oxide thin film according to claim 1, wherein The first metal includes In and / or Sn; Optionally, the second metal includes any one or a combination of at least two of Zn, Ga, Ta, W, Bi, Hf, Zr, Ti, Mo or Ge; Optionally, the third rare earth metal includes any one of Sc, Y, Ce, Pr, Tb, Dy or Yb, or a combination of at least two of them.

3. The semiconductor oxide thin film according to claim 1 or 2, wherein: The ratio of α to β in the multi-layer metal oxide layer is (1-20):1; Optionally, the ratio of α to γ ​​in the multi-layer metal oxide layer is (10-100):

1.

4. The semiconductor oxide thin film according to any one of claims 1 to 3, wherein: The thickness of the semiconductor oxide film is Further optional Optionally, the carrier concentration of the semiconductor oxide film is 10 14 -10 21 cm -3 , further optional to 10 16 -10 20 cm -3 .

5. A method for preparing a semiconductor oxide thin film according to any one of claims 1 to 4, comprising: Cyclic deposition of AO on substrate using atomic layer deposition α / n BO β / n RO γ / n , to obtain the semiconductor oxide film; wherein n is the number of cyclic deposition times.

6. The preparation method according to claim 5, wherein: The preparation method specifically comprises: The substrate is placed in an atomic layer deposition reaction device, and a first metal source precursor, an inert gas and an oxygen source are introduced into the reaction device in sequence to deposit an α / n AO layer; then a second metal source precursor, an inert gas and an oxygen source are introduced into the reaction device in sequence to deposit a β / n BO layer; then a third rare earth metal source precursor, an inert gas and an oxygen source are introduced into the reaction device in sequence to deposit a γ / n RO layer; finally, the semiconductor oxide film is obtained through cyclic deposition.

7. The preparation method according to claim 6, wherein: The number of cyclic deposition is 10-200; Optionally, the first metal source precursor includes an In source and / or a Sn source; Optionally, the pulse time of the first metal source precursor is 0.03-2s; Optionally, the inlet flow rate of the first metal source precursor is 10-500 sccm; Optionally, the chemical source temperature of the first metal source precursor is 50-130°C; Optionally, the AO layer is deposited at a temperature of 150-300°C; Optionally, the plasma power for depositing the AO layer is 50-300W.

8. The preparation method according to claim 6 or 7, wherein: The second metal source precursor includes any one of a Zn source, a Ga source, a Ta source, a W source, a Bi source, a Hf source, a Zr source, a Ti source, a Mo source or a Ge source, or a combination of at least two thereof; Optionally, the pulse time of the second metal source precursor is 0.01-1.5s; Optionally, the flow rate of the second metal source precursor is 20-300 sccm; Optionally, the chemical source temperature of the second metal source precursor is 25-100°C; Optionally, the thin film deposition temperature of the second metal source precursor is 150-300°C; Optionally, the plasma power for depositing the BO layer is 50-200W.

9. The preparation method according to any one of claims 6 to 8, wherein: The third rare earth metal source precursor includes any one of a Sc source, a Y source, a Ce source, a Pr source, a Tb source, a Dy source or a Yb source, or a combination of at least two thereof; Optionally, the pulse time of the third rare earth metal source precursor is 0.05-3s; Optionally, the inlet flow rate of the third rare earth metal source precursor is 50-500 sccm; Optionally, the chemical source temperature of the third rare earth metal source precursor is 60-150°C; Optionally, the thin film deposition temperature of the third rare earth metal source precursor is 150-300° C.; Optionally, the plasma power for depositing the RO layer is 100-500W.

10. The preparation method according to any one of claims 6 to 9, wherein: The purge time of the inert gas is 5-30s; Optionally, the oxygen source includes any one of O2, H2O, H2O2, O3 or oxygen plasma or a combination of at least two thereof; Optionally, the pulse time of the oxygen source is 0.2-50s.