Preparation method of regenerated periodontal patch with antibacterial function

The bilayer periodontal patch prepared by layered casting and freeze-drying technology uses silk fibroin and nano-hydroxyapatite to achieve accurate sustained release of drugs and periodontal tissue regeneration, solving the instability of drug release in the existing technology and the problem of penetration difficulties improves the effectiveness and safety of periodontitis treatment.

CN118892575APending Publication Date: 2024-11-05SUZHOU UNIV
View PDF 2 Cites 0 Cited by

Patent Information

Application Number
CN202410890897.3
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-07-04
Publication Date
2024-11-05

AI Technical Summary

Technical Problem

Existing treatment methods for periodontitis are difficult to achieve the continuous and stable release of drugs and penetrate the wound site, resulting in poor treatment effects and prone to bacterial growth and infection.

Method used

The layered casting method is used to prepare silk fibroin antibacterial microneedle and silk fibroin/nanohydroxyapatite composite materials, and the precise sustained release of drugs and penetration of wounds is achieved through microneedle. Combined with ethanol fumigation treatment and freeze-drying technology, a double layer is formed. Periodontal patches are used to promote periodontal tissue regeneration.

Benefits of technology

It achieves long-term precise sustained release of the drug and continuous delivery of periodontal tissue, enhances the antibacterial effect, promotes the regeneration of periodontal bones and alveolar bones, reduces the risk of bacterial infection, and improves the therapeutic effect.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118892575A_ABST
    Figure CN118892575A_ABST
Patent Text Reader

Abstract

The invention discloses a preparation method of a regenerated periodontal patch with an antibacterial function, which comprises the following steps: firstly, preparing a silk fibroin-based antibacterial microneedle by a layered pouring method, performing ethanol fumigation treatment, and then preparing an SF / nHA composite material by a freeze drying method; finally, the microneedle and the composite material are combined through a fibroin cross-linking and freeze-drying integrated forming technology, the double-layer periodontal patch with the antibacterial / regeneration function is prepared, on one hand, local and continuous drug delivery of periodontal tissue is achieved through SF microneedle drug delivery, and the antibacterial effect is achieved; on the other hand, through the SF / nHA composite material, the function of a barrier membrane can be achieved to prevent gingival epithelial cells from invading, regeneration of alveolar bones and cementum in periodontal hard tissue can be promoted, and functional periodontal tissue regeneration is expected to be achieved. Therefore, the invention has potential application value in the technical field of oral medical instruments.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention belongs to the technical field of medical devices and relates to a method for preparing a regenerative periodontal patch with antibacterial function. Background Art

[0002] Oral diseases affect nearly 3.5 billion people worldwide, among which periodontitis is one of the most common oral diseases. Periodontitis is a common, chronic, destructive inflammatory disease that damages human tooth-supporting tissues. Currently, the clinical treatment of periodontitis mainly focuses on plaque removal and local inflammation control, such as teeth cleaning and surgical treatment. These therapies attempt to minimize symptoms and prevent disease progression, but cannot effectively restore the original periodontal tissue and attachment, and the function of the treated teeth and dentition is still impaired. Therefore, people need to design alternative regenerative strategies to restore the structure and function of periodontal tissues in patients with periodontitis.

[0003] At present, certain progress has been made in the research of periodontal regeneration technology. In the patent application with publication number CN117468171A, a method for preparing a polycaprolactone electrospun fiber membrane loaded with curcumin-nanohydroxyapatite for treating periodontitis is disclosed. Nanohydroxyapatite and curcumin are added to the spinning solution, and a nanofiber membrane is prepared by an electrospinning device for treating periodontitis. However, it is difficult for the nanofiber membrane to achieve sustained and stable release of drugs, and it is impossible to penetrate the physical barrier of the wound site. The drug stays on the wound surface, and the therapeutic effect is reduced. In the patent application with publication number CN115814170B, a method for preparing a cross-scale bionic composite restoration for guiding periodontal tissue regeneration and its application are disclosed. The material has a layer of mineral as a scaffold structure, which is conducive to inducing osteogenesis, and another layer of polylactic acid as a diaphragm structure, which can prevent gingival epithelial cells and gingival connective tissue cells from migrating to the root side, selectively allowing some cell populations to enter the wound space and reconstruct periodontal attachment on the root surface. However, unilateral periodontal regeneration can easily lead to bacterial growth and infection in the damaged area, affecting the treatment effect.

[0004] The ultimate goal of periodontal treatment is to coordinate the regeneration of periodontal tissue. Compared with traditional biomaterials or single-phase scaffolds, multiphase scaffolds can provide cells with more sufficient growth space and can release signal molecules in time to guide the regeneration of various components of periodontal structure. The application advantages in periodontal tissue regeneration are more prominent. Among scaffold materials, silk fibroin is a natural protein extracted from silkworm cocoons. It was approved as a biomaterial by the US Food and Drug Administration in 1993. It has excellent mechanical properties, biodegradability, biocompatibility and bioabsorbability, and is widely used in biological tissue engineering. Hydroxyapatite is the main inorganic component of teeth and bones. Among them, nanohydroxyapatite has unique physical and chemical properties of nanomaterials such as small grain diameter, large interface, high surface free energy and binding energy, and macroscopic quantum tunneling effect. It is widely used in the field of dentistry. Effective antibacterial and anti-inflammatory are considered to be the key to the successful treatment of periodontitis. The sustained and stable release of drugs in the periodontal pocket is crucial for the safety and effectiveness of treatment. Due to bacterial infection, saliva secretion and local adverse reactions, drug delivery in the oral cavity is still challenging.

[0005] Therefore, in order to achieve better clinical treatment effects, it is necessary to develop a periodontal patch that has both antibacterial and periodontal regeneration functions. Summary of the invention

[0006] The purpose of the present invention is to provide a method for preparing a regenerative periodontal patch with antibacterial function to solve the above problems.

[0007] The technical solution of the present invention is:

[0008] A method for preparing a regenerative periodontal patch with antibacterial function, specifically comprising:

[0009] (1) degumming raw silk from silkworms in a boiling sodium carbonate solution, washing it, and drying it in a fume hood to obtain dry silk, soaking the silk in a lithium bromide solution, dissolving it in an oven, dialyzing it in deionized water after it is dissolved, and centrifuging it to obtain a silk fibroin solution;

[0010] (2) dissolving the antibacterial drug into the silk fibroin solution and mixing the mixture thoroughly to obtain an antibacterial silk fibroin solution;

[0011] (3) using a layered casting method, first dripping the antibacterial silk fibroin solution evenly onto the microneedle template, performing a first vacuum treatment, then dripping the antibacterial silk fibroin solution evenly onto the treated surface of the microneedle template, performing a vacuum treatment for 3-5 times, and finally naturally air-drying to form, followed by ethanol fumigation treatment to obtain SF / MH antibacterial microneedles;

[0012] (4) preparing a silk fibroin / nanohydroxyapatite mixed solution, freeze-drying, and obtaining a SF / nHA composite material;

[0013] (5) The SF / MH antibacterial microneedles and the SF / nHA composite material are respectively compounded by silk cross-linking and freeze-drying to obtain a double-layer periodontal patch.

[0014] Furthermore, in step (1), the mass concentration of the sodium carbonate solution is 0.01% to 0.05%, the concentration of the lithium bromide solution is 6 to 10 mol / L, and the mass concentration of the silk fibroin solution is 6% to 10%.

[0015] Furthermore, in step (1), the temperature of the oven is 50-70° C., the dissolution time is 2-4 hours, and the dialysis time is 1-3 days.

[0016] Furthermore, in step (2), the antibacterial drug is selected from any one of minocycline hydrochloride, curcumin, and metronidazole. When minocycline hydrochloride is selected, the safe dose of minocycline hydrochloride is 0.15 mg / mL.

[0017] Furthermore, in step (3), the first vacuuming time is 10 to 20 minutes, and the natural air drying time is 2 to 3 days.

[0018] Furthermore, in step (3), the volume percentage of ethanol in the ethanol fumigation treatment is 75%, the temperature of the ethanol fumigation treatment is 40° C. to 60° C., and the time of the ethanol fumigation treatment is 2 to 4 hours.

[0019] Furthermore, in step (4), during the preparation of the silk fibroin / nano-hydroxyapatite mixed solution, the mass ratio of the silk fibroin solution to the nano-hydroxyapatite powder is 10:1-5.

[0020] Furthermore, in step (4), the freezing temperature is -45°C to -50°C, and the drying time is 2 to 3 days.

[0021] Furthermore, in step (5), the concentration of the silk cross-linking is 15-20 wt %.

[0022] Furthermore, in step (5), the freezing temperature is -45°C to -50°C, and the drying time is 2 to 3 days.

[0023] The present invention provides a method for preparing a regenerative periodontal patch with antibacterial function, which has the following advantages:

[0024] (1) Silk fibroin is used as the raw material, which has good biocompatibility and excellent mechanical properties. Antibacterial drugs have outstanding antibacterial effects on periodontal pathogens such as Porphyromonas gingivalis, and nanohydroxyapatite can effectively promote the regeneration of periodontal bone tissue;

[0025] (2) Microneedles have unique advantages in wound healing and tissue regeneration: microscale needle tips can easily penetrate the physical barriers of the wound site, microneedles can naturally provide mechanical stimulation for wound healing and tissue regeneration, microneedles can overcome the drug resistance of biofilms in wounds, the structure of microneedles allows the loading of multiple drugs, and by fumigating microneedles with ethanol, the mechanical properties of microneedles can be improved, achieving long-term and precise sustained release of antimicrobial drugs;

[0026] (3) The freeze-drying integrated molding technology ensures the stability of the product in the complex environment inside the oral cavity;

[0027] (4) The double-layer periodontal patch designed for this product, on the one hand, achieves local and continuous drug delivery to the periodontal tissue through microneedle drug delivery to achieve antibacterial effect; on the other hand, through the SF / nHA composite material, it can not only realize the barrier membrane function to prevent the invasion of gingival epithelial cells, but also promote the regeneration of alveolar bone and cementum in the periodontal hard tissue, in order to achieve functional periodontal tissue regeneration. BRIEF DESCRIPTION OF THE DRAWINGS

[0028] Figure 1 The actual image and super depth image of the antibacterial microneedle prepared in Example 1 of the method for preparing a regenerative periodontal patch with antibacterial function of the present invention, wherein (a) is the actual image of the SF / MH antibacterial microneedle and (b) is the super depth image;

[0029] Figure 2 It is a schematic diagram of the maximum bearing capacity of SF / MH microneedles and pure SF microneedles at different compression rates prepared in Example 1 of the method for preparing a regenerative periodontal patch with antibacterial function of the present invention;

[0030] Figure 3 Schematic diagram of the antibacterial effects of the antibacterial microneedles and pure SF microneedles prepared in Example 1 of the method for preparing a regenerative periodontal patch with antibacterial function of the present invention on Escherichia coli and Staphylococcus aureus, respectively, wherein A is the Escherichia coli antibacterial group, A-1 is the control group, A-2 is the pure SF microneedle group, and A-3 is the SF / MH microneedle group; B is the Staphylococcus aureus antibacterial group, B-1 is the control group, B-2 is the pure SF microneedle group, and B-3 is the SF / MH microneedle group;

[0031] Figure 4 The physical picture, SEM picture and pore size distribution picture of the SF / nHA composite material prepared in Example 2 of the method for preparing a regenerative periodontal patch with antibacterial function of the present invention, wherein (a) is a physical picture of the SF / nHA composite material, (b) is a SEM picture, and (c) is a pore size distribution picture;

[0032] Figure 5This is a comparison diagram of the mechanical properties of SF / nHA with different ratios prepared in Example 2 according to the method for preparing a regenerative periodontal patch with antibacterial function of the present invention;

[0033] Figure 6 This is a schematic diagram of the structure and function of a double-layer periodontal patch prepared in Example 3 of the method for preparing a regenerative periodontal patch with antibacterial function described in the present invention. DETAILED DESCRIPTION

[0034] The present invention provides a method for preparing a regenerative periodontal patch with antibacterial function, and the specific operation steps are as follows:

[0035] Step 1: Put the raw silk into 0.01% to 0.05% sodium carbonate (Na 2 CO 3 ) solution, and after washing, put it in a fume hood to dry. Soak the silk in a lithium bromide (LiBr) solution with a concentration of 6 to 10 mol / L, put it in a 50 to 70°C oven to dissolve for 2 to 4 hours, and then put it in deionized water for dialysis for 1 to 3 days. After centrifugation, a silk fibroin (SF) solution with a concentration of 6% to 10% (w / v) is obtained.

[0036] Step 2: Add the antibacterial drug minocycline hydrochloride (MH) to the SF solution and mix thoroughly to obtain a silk fibroin antibacterial solution. In this step, the antibacterial drug may also be curcumin, metronidazole, etc.

[0037] Step 3: Using the layered casting method, first drip the silk fibroin antibacterial solution evenly into the microneedle template, and perform the first vacuum treatment for 10 to 20 minutes. Then drip the SF solution evenly into the microneedle template and perform the vacuum treatment 3 to 5 times. Finally, air dry it naturally for 2 to 3 days to form it, and perform ethanol fumigation treatment with an ethanol concentration of 75%, a temperature of 40℃ to 60℃, and a fumigation time of 2 to 4 hours to obtain SF / MH antibacterial microneedles.

[0038] Step 4: Prepare five gradient concentration solutions of silk fibroin solution and hydroxyapatite powder according to the mass ratio of 10:1, 10:2, 10:3, 10:4, and 10:5, and ultrasonically mix for 10 to 15 minutes at an ultrasonic power of 70% to 80%. Then pre-freeze in a -20℃ refrigerator for more than 12 hours, and then freeze-dry at -45℃ to -50℃ for 2 to 3 days to prepare SF / nHA composite materials.

[0039] Step 5: The antibacterial microneedle SF / MH and SF / nHA composite materials were respectively compounded by silk cross-linking and freeze-drying, wherein the silk cross-linking concentration was 15-20wt%, the freezing temperature was -45℃--50℃, and the drying time was 2-3 days. Finally, a double-layer periodontal patch under two treatment conditions was obtained.

[0040] In order to make the above-mentioned objects, features and advantages of the present invention more clearly understood, the technical solutions of the present invention are further described below in conjunction with specific embodiments. However, the present invention is not limited to the embodiments listed, and should also include any other known changes within the scope of the rights claimed by the present invention.

[0041] The term "one embodiment" or "embodiment" as used herein refers to a specific feature, structure, or characteristic that may be included in at least one implementation of the present invention. The term "in one embodiment" that appears in different places in this specification does not necessarily refer to the same embodiment, nor does it refer to a separate or selective embodiment that is mutually exclusive with other embodiments.

[0042] Example 1

[0043] This embodiment demonstrates a method for preparing a regenerative periodontal patch with antibacterial function, and the specific steps are as follows:

[0044] (1) Add 0.05% mass fraction of Na 2 CO 3 Add to boiling water to dissolve, then boil the raw silk in boiling water for 30 minutes. After washing three times, place it in a fume hood to air dry for 24 hours. Soak the silk in 100mL of 9.3mol / L LiBr solution, then place it in a 60℃ oven, take it out after 4 hours and cool it, place it in deionized water for dialyzing for more than 36 hours, centrifuge to remove impurities, and finally obtain the silk fibroin solution, which is stored in a 4℃ refrigerator;

[0045] (2) preparing a silk fibroin solution with a concentration of 8 wt %, adding 0.15 mg / mL of the antibacterial drug minocycline hydrochloride to the silk fibroin solution, and mixing well to obtain a silk fibroin antibacterial solution;

[0046] (3) The antibacterial microneedles were prepared by the layered casting method. First, the silk fibroin antibacterial solution was evenly dripped into the microneedle template, and the first vacuum treatment was performed for 10 minutes. Then, the silk fibroin solution was evenly dripped into the microneedle template, and the vacuum treatment was performed three times. Finally, it was naturally air-dried for 2 days to obtain SF / MH antibacterial microneedles;

[0047] (4) The regenerated composite material was prepared by freeze drying, and a 6wt% silk fibroin solution and hydroxyapatite powder were mixed in a mass ratio of 10:1, and then ultrasonicated for 15 minutes at an ultrasonic power of 80%. It was then placed in a -20°C refrigerator for pre-freezing for more than 12 hours, and then freeze-dried for 3 days to prepare a SF / nHA composite material;

[0048] (5) The SF / MH antibacterial microneedles and the SF / nHA composite material were combined by silk cross-linking and naturally air-dried to obtain a SF / MH / nHA double-layer periodontal patch, wherein the silk cross-linking concentration was 15 wt % and the air-drying time was 2 days.

[0049] See also Figure 1 , Figure 1 The actual image and super depth image of the antibacterial microneedle prepared in Example 1 of the method for preparing a regenerative periodontal patch with antibacterial function of the present invention, wherein (a) is the actual image of the SF / MH antibacterial microneedle and (b) is the super depth image. Figure 1 As shown in the figure, the drugs in the SF / MH microneedles prepared by the layered casting method are mainly concentrated at the needle tip, which is conducive to the efficient release of subsequent drugs to the damaged periodontal area and improves the drug release rate. Figure 2 , Figure 2 This is a schematic diagram of the maximum bearing capacity of the SF / MH microneedles and pure SF microneedles prepared in Example 1 of the method for preparing a regenerative periodontal patch with antibacterial function of the present invention at different compression rates. Figure 2 As shown in the figure, as the compression rate increases, the stress gradually decreases. Compared with pure SF microneedles, the mechanical properties of SF / MH antibacterial microneedles are significantly improved, the maximum bearing capacity is more prominent, and they can effectively penetrate the periodontal soft tissue to release antibacterial drugs. Figure 3 , Figure 3 Schematic diagram of the antibacterial effect of the antibacterial microneedles and pure SF microneedles prepared in Example 1 of the method for preparing a regenerative periodontal patch with antibacterial function of the present invention on Escherichia coli and Staphylococcus aureus, respectively, wherein A is the Escherichia coli antibacterial group, A-1 is the control group, A-2 is the pure SF microneedle group, and A-3 is the SF / MH microneedle group; B is the Staphylococcus aureus antibacterial group, B-1 is the control group, B-2 is the pure SF microneedle group, and B-3 is the SF / MH microneedle group. Figure 3 As shown in the figure, the inhibition rate of SF / MH antibacterial microparticles against Gram-negative bacteria Escherichia coli and Gram-positive bacteria Staphylococcus aureus reached more than 99%, which has a very significant antibacterial effect and provides a suitable oral microenvironment for subsequent periodontal tissue regeneration.

[0050] Example 2

[0051] This embodiment demonstrates a method for preparing a regenerative periodontal patch with antibacterial function, and the specific steps are as follows:

[0052] (1) Add 0.05% mass fraction of Na 2 CO 3Add to boiling water to dissolve, then boil the raw silk in boiling water for 30 minutes. After washing three times, place it in a fume hood to air dry for 24 hours. Soak the silk in 100mL of 9.3mol / L LiBr solution, then place it in a 60℃ oven, take it out after 4 hours and cool it, place it in deionized water for dialyzing for more than 36 hours, centrifuge to remove impurities, and finally obtain the silk fibroin solution, which is stored in a 4℃ refrigerator;

[0053] (2) preparing a 10 wt % silk fibroin solution, adding 0.15 mg / mL of natural antibacterial drug curcumin (Cur) to the silk fibroin solution, and mixing well to obtain a silk fibroin antibacterial solution;

[0054] (3) The antibacterial microneedles were prepared by the layered casting method. First, the silk fibroin antibacterial solution was evenly dripped into the microneedle template, and the first vacuum treatment was performed for 20 minutes. Then, the silk fibroin solution was evenly dripped into the microneedle template, and the vacuum treatment was performed 4 times. The molded microneedles were naturally air-dried for 3 days. The molded microneedles were placed in a glass container with 75% ethanol solution at the bottom, and placed in a 45°C vacuum drying oven for fumigation for 12 hours. After being taken out, they were naturally air-dried for 1 day to obtain SF / Cur antibacterial microneedles;

[0055] (4) The regenerated composite material was prepared by freeze drying, and a 6wt% silk fibroin solution and hydroxyapatite powder were mixed in a mass ratio of 10 / 3, and then ultrasonicated for 20 minutes at an ultrasonic power of 80%. The mixture was then placed in a -20°C refrigerator for pre-freezing for more than 12 hours, and then freeze-dried for 3 days to prepare a SF / nHA composite material;

[0056] (5) The SF / Cur antibacterial microneedles and the SF / nHA composite material were combined by silk cross-linking and naturally air-dried to obtain a SF / Cur / nHA double-layer periodontal patch, wherein the silk cross-linking concentration was 20 wt % and the air-drying time was 2 days.

[0057] See also Figure 4 , Figure 4 The actual image, SEM image and pore size distribution diagram of the SF / nHA composite material prepared in Example 2 of the method for preparing a regenerative periodontal patch with antibacterial function of the present invention, wherein (a) is the actual image of the SF / nHA composite material, (b) is the SEM image, and (c) is the pore size distribution diagram. Figure 4 As shown in the figure, the composite material has a clear pore structure, which can improve the oxygen permeability, provide sufficient oxygen to tissue cells, and promote periodontal regeneration. Figure 5 , Figure 5 This is a comparison chart of the mechanical properties of SF / nHA with different ratios prepared in Example 2 according to the method for preparing a regenerative periodontal patch with antibacterial function of the present invention. Figure 5As shown in the figure, all prepared composite materials show typical compressive stress-strain curves. The composite material SF / nHA has better mechanical properties than pure SF material. The compressive mechanical properties of the materials obtained by the same preparation method are enhanced with the increase of nano-hydroxyapatite content.

[0058] Example 3

[0059] This embodiment demonstrates a method for preparing a regenerative periodontal patch with antibacterial function, and the specific steps are as follows:

[0060] (1) Add 0.05% mass fraction of Na 2 CO 3 Add to boiling water to dissolve, then boil the raw silk in boiling water for 30 minutes. After washing three times, place it in a fume hood to air dry for 24 hours. Soak the silk in 100mL of 9.3mol / L LiBr solution, then place it in a 60℃ oven, take it out after 4 hours and cool it, place it in deionized water for dialyzing for more than 36 hours, centrifuge to remove impurities, and finally obtain the silk fibroin solution, which is stored in a 4℃ refrigerator;

[0061] (2) preparing a 10 wt % silk fibroin solution, adding 0.15 mg / mL of a commonly used antibacterial drug metronidazole (Met) to the silk fibroin solution, and mixing the mixture thoroughly to obtain a silk fibroin antibacterial solution;

[0062] (3) The antibacterial microneedles were prepared by the layered casting method. First, the silk fibroin antibacterial solution was evenly dripped into the microneedle template, and the first vacuum treatment was performed for 30 minutes. Then, the silk fibroin solution was evenly dripped into the microneedle template, and the vacuum treatment was performed 5 times. The molded microneedles were naturally air-dried for 3 days. The molded microneedles were placed in a glass container with 75% ethanol solution at the bottom, and placed in a 60°C vacuum drying oven for fumigation for 12 hours. After being taken out, they were naturally air-dried for 1 day to obtain SF / Met antibacterial microneedles;

[0063] (4) The regenerated composite material was prepared by freeze drying, and a 6wt% silk fibroin solution and hydroxyapatite powder were mixed in a mass ratio of 10 / 5, and then ultrasonicated for 20 minutes at an ultrasonic power of 80%. The mixture was then placed in a -20°C refrigerator for pre-freezing for more than 12 hours, and then freeze-dried for 3 days to prepare a SF / nHA composite material;

[0064] (5) The SF / Met antibacterial microneedles and SF / nHA composite materials were combined by freeze-drying integrated molding technology. First, the prepared SF / nHA solution was placed in a square glass container, and the microneedles were cut into equal sizes. The base was slowly contacted with the solution, and then placed in a -20°C refrigerator for 12 hours, and then freeze-dried and naturally air-dried to obtain a SF / Met / nHA double-layer periodontal patch. The freezing temperature was -45°C and the drying time was 2 days.

[0065] See also Figure 6 , Figure 6 The structure and function diagram of the double-layer periodontal patch prepared in Example 3 of the method for preparing a regenerative periodontal patch with antibacterial function described in the present invention. Figure 6 As shown in the figure, the upper microneedles carry antibacterial drugs to remove bacteria from the periodontal infection site, providing a suitable microbial environment for periodontal regeneration; the lower SF / nHA composite material is filled into the cementum or alveolar bone defect site, releasing nanohydroxyapatite particles to promote bone regeneration. At the same time, the double-layer combination achieved through silk cross-linking or freeze-drying can effectively prevent the invasion of gingival epithelial cells on periodontal soft tissues, avoid affecting the healing effect, and ultimately achieve a one-step, two-birds-one-stone treatment effect.

[0066] In summary, the preparation method of a regenerative periodontal patch with antibacterial function described in the present invention has the characteristics of convenient molding and easy regulation of a layer of microneedles prepared with silk fibroin as raw material. The layered casting method allows the drug to be effectively concentrated in the needle tip, accurately release the drug, and improve the drug release rate; ethanol fumigation treatment can improve the mechanical properties of the microneedle, so that the needle tip can effectively penetrate the oral periodontal part and reduce the patient's discomfort; carrying different antibacterial drugs, the microneedle has significant antibacterial properties. Another layer of composite material prepared with silk fibroin and hydroxyapatite as raw materials has the characteristics of high porosity and high stability. On the one hand, this product achieves local and continuous drug delivery to periodontal tissues through SF microneedle administration to achieve antibacterial effect; on the other hand, through the SF / nHA composite material, it can not only realize the barrier membrane function to prevent the invasion of gingival epithelial cells, but also promote the regeneration of periodontal hard tissue alveolar bone and cementum, so as to achieve functional periodontal tissue regeneration. Therefore, the present invention has great development potential in the field of oral medical device technology.

[0067] It should be noted that the above embodiments are only used to illustrate the technical solutions of the present invention rather than to limit it. Although the present invention has been described in detail with reference to the preferred embodiments, those skilled in the art should understand that the technical solutions of the present invention may be modified or replaced by equivalents without departing from the spirit and scope of the technical solutions of the present invention, which should all be included in the scope of the claims of the present invention.

Claims

1. A method for preparing a regenerative periodontal patch with antibacterial function, It is characterized in that The specific steps are as follows: (1) degumming raw silk from silkworms in a boiling sodium carbonate solution, washing it, and drying it in a fume hood to obtain dry silk, soaking the silk in a lithium bromide solution, dissolving it in an oven, dialyzing it in deionized water after it is dissolved, and centrifuging it to obtain a silk fibroin solution; (2) dissolving the antibacterial drug into the silk fibroin solution and mixing the mixture thoroughly to obtain an antibacterial silk fibroin solution; (3) using a layered casting method, first dripping the antibacterial silk fibroin solution evenly onto the microneedle template, performing a first vacuum treatment, then dripping the silk fibroin solution evenly onto the treated surface of the microneedle template, performing a vacuum treatment for 3-5 times, and finally naturally air-drying to form, followed by ethanol fumigation treatment to obtain SF / MH antibacterial microneedles; (4) preparing a silk fibroin / nanohydroxyapatite mixed solution, freeze-drying, and obtaining a SF / nHA composite material; (5) The SF / MH antibacterial microneedles and the SF / nHA composite material are respectively compounded by silk cross-linking and freeze-drying to obtain a double-layer periodontal patch.

2. A method for preparing a regenerative periodontal patch with antibacterial function according to claim 1, Features: In step (1), the mass concentration of the sodium carbonate solution is 0.01% to 0.05%, the concentration of the lithium bromide solution is 6 to 10 mol / L, and the mass concentration of the silk fibroin solution is 6% to 10%.

3. The method for preparing a regenerative periodontal patch with antibacterial function according to claim 1, Features: In step (1), the temperature of the oven is 50-70° C., the dissolution time is 2-4 hours, and the dialysis time is 1-3 days.

4. The method for preparing a regenerative periodontal patch with antibacterial function according to claim 1, Features: In step (2), the antibacterial drug is selected from any one of minocycline hydrochloride, curcumin, and metronidazole. When minocycline hydrochloride is selected, the safe dose of minocycline hydrochloride is 0.15 mg / mL.

5. The method for preparing a regenerative periodontal patch with antibacterial function according to claim 1, Features: In step (3), the first vacuuming time is 10 to 20 minutes, and the natural air drying time is 2 to 3 days.

6. The method for preparing a regenerative periodontal patch with antibacterial function according to claim 1, Features: In step (3), the volume percentage of ethanol in the ethanol fumigation treatment is 75%, the temperature of the ethanol fumigation treatment is 40° C. to 60° C., and the time of the ethanol fumigation treatment is 2 to 4 hours.

7. The method for preparing a regenerative periodontal patch with antibacterial function according to claim 1, Features: In step (4), during the process of preparing the silk fibroin / nano-hydroxyapatite mixed solution, the mass ratio of the silk fibroin solution to the nano-hydroxyapatite powder is 10:1-5.

8. The method for preparing a regenerative periodontal patch with antibacterial function according to claim 1, Features: In step (4), the freezing temperature is -45°C to -50°C, and the drying time is 2 to 3 days.

9. The method for preparing a regenerative periodontal patch with antibacterial function according to claim 1, Features: In step (5), the concentration of the silk cross-linking is 15-20 wt %.

10. The method for preparing a regenerative periodontal patch with antibacterial function according to claim 1, Features: In step (5), the freezing temperature is -45°C to -50°C, and the drying time is 2 to 3 days.

Citation Information

Patent Citations

  • Preparation method and application of a cross-scale bionic composite restoration for guiding periodontal tissue regeneration

    CN115814170B

  • Preparation method of curcumin-nano-hydroxyapatite loaded PCL electrospun fibrous membrane for treating periodontitis