Ta-Ti binary hydrogen absorption transition layer of accelerator neutron source target and preparation method of Ta-Ti binary hydrogen absorption transition layer

Through magnetron cosputtering technology, the Ta-Ti binary hydrogen absorption transition layer is constructed on the surface of the neutron source target in the accelerator, which solves the cracking and shedding of the tantalum film under high stress conditions, and achieves high binding force and corrosion resistance. It also avoids waste of target materials and is suitable for industrial production.

CN118895481AActive Publication Date: 2024-11-05HUAPENG NEUTRON TECH (HANGZHOU) CO LTD

Patent Information

Application Number
CN202410441509.3
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-04-12
Publication Date
2024-11-05
Estimated Expiration
2044-04-12

AI Technical Summary

Technical Problem

The tantalum film of the existing accelerator neutron source target is prone to cracking and falling off under high stress and radiation conditions, and the preparation of multi-layer film structure requires frequent replacement of the target material, resulting in waste of resources.

Method used

Magnetically controlled cosputtering technology is used to construct a Ta-Ti binary hydrogen absorption transition layer on the substrate surface of the neutron source target. Through uniformly distributed tantalum and titanium, the residual stress of the tantalum film is reduced and the film-based binding force is improved to avoid film cracking. and fall off, and do not need to replace the target material.

Benefits of technology

The Ta-Ti binary hydrogen absorption transition layer is achieved with low residual stress and high binding force, which improves the corrosion resistance and thermal conductivity of the film, and has a simple process and high sputtering efficiency, making it suitable for industrial production.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118895481A_ABST
    Figure CN118895481A_ABST
Patent Text Reader

Abstract

The invention relates to the field of neutron source targets, and discloses a Ta-Ti binary hydrogen absorption transition layer of an accelerator neutron source target and a preparation method of the Ta-Ti binary hydrogen absorption transition layer. The Ta-Ti binary hydrogen absorption transition layer is deposited on the surface of a base body through the magnetron co-sputtering technology, and the Ta-Ti binary hydrogen absorption transition layer comprises tantalum and titanium which are evenly distributed. The mass ratio of tantalum to titanium is (80: 20)-(90: 10). The Ta-Ti binary hydrogen absorption transition layer is constructed on the surface of the matrix of the accelerator neutron source target through the magnetron co-sputtering technology, and the Ta-Ti binary hydrogen absorption transition layer is low in residual internal stress, high in binding force with the matrix and not prone to cracking and falling off; in addition, the method is simple, the target does not need to be replaced, and the sputtering efficiency is high.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the field of neutron source targets, and in particular to a Ta-Ti binary hydrogen absorption transition layer of an accelerator neutron source target and a preparation method thereof. Background Art

[0002] Boron neutron capture therapy is a rapidly developing advanced radiotherapy technology that 10 B(n,α) 7 Li nuclear reaction kills cancer cells and is a binary targeted therapy at the atomic level. To complete the above treatment, not only neutron capture drugs but also corresponding neutron sources are needed. Both are the core elements of BNCT. At present, there are two suitable sources of neutron beams in the world. One is to obtain neutron beams through reactors, and the other is to obtain them through accelerator neutron sources. The accelerator-based neutron source is a neutron produced by high-energy protons hitting targets by accelerating protons through high-energy accelerators. According to the type of accelerator, it can be divided into three categories: radio frequency linear accelerator, cyclotron accelerator and high-voltage accelerator. It has the advantages of safety, reliability, flexibility and convenience in use. In recent years, accelerator-based neutron sources have become increasingly mature and have become the preferred neutron source in clinical practice.

[0003] The neutron source target is a component that produces neutrons. For the accelerator neutron source, the target that undergoes nuclear reactions and produces neutrons is one of the most critical and most easily damaged components. Generally, the main nuclear reaction layer (target material layer) is composed of lithium or beryllium. The target must withstand severe thermomechanical, radiation and hydrogen damage conditions. Tantalum has a high hydrogen diffusion coefficient and can be used as a transition layer for neutron production targets in accelerator boron neutron capture therapy (AB-BNCT). A Ta film thickness of 20μm can effectively prevent proton deposition and hydrogen embrittlement in the Cu matrix. There are many methods for preparing Ta films, such as vacuum plasma spraying (VPS), molten salt electroplating, chemical vapor deposition (CVD) and physical vapor deposition (PVD). Magnetron sputtering is selected because of its advantages such as fast sputtering speed, formation of dense films, excellent adhesion, precise control of film formation and ability to cover large surface areas. However, the physical properties of Ta are far different from those of the copper matrix, and the film is prone to cracking and falling off when it reaches a certain thickness.

[0004] The applicant tried to design the tantalum film into a multi-layer film structure to reduce stress in the early stage. Although this method can effectively reduce the thickness of a single-layer film to prevent the film from cracking or falling off, this solution requires constant replacement of the sputtering target when constructing a multi-layer film, resulting in a waste of target materials. Therefore, it is necessary to seek more different ways to solve the above technical problems. Summary of the invention

[0005] In order to solve the above technical problems, the present invention provides a Ta-Ti binary hydrogen absorption transition layer of an accelerator neutron source target and a preparation method thereof. The present invention constructs a Ta-Ti binary hydrogen absorption transition layer on the substrate surface of the accelerator neutron source target by magnetron co-sputtering technology. The Ta-Ti binary hydrogen absorption transition layer has low residual internal stress, high bonding strength with the substrate, and is not easy to crack or fall off; in addition, the method of the present invention is simple, does not need to replace the target material, and has high sputtering efficiency.

[0006] The specific technical scheme of the present invention is: In the first aspect, the present invention provides a Ta-Ti binary hydrogen absorption transition layer for an accelerator neutron source target, which is deposited on the surface of a substrate by magnetron co-sputtering technology, wherein the Ta-Ti binary hydrogen absorption transition layer includes uniformly distributed tantalum and titanium; the mass ratio of tantalum to titanium is 80:20-90:10 (further preferably 85:15-90:10).

[0007] In the field of neutron source target systems, Ti is mainly used as a protective layer material on the surface of the target layer. The present invention finds that if it is doped into a tantalum film, at a low doping level, the titanium atom is the key position where the atomic bond angle distortion occurs, which can significantly reduce the residual stress of the tantalum film, and the present invention also finds that titanium has good adhesion to almost all substrates of material. Therefore, under the above multiple factors, if a Ti-Ta binary hydrogen absorption transition layer is deposited on the surface of the substrate, it is expected to improve the film-substrate bonding strength.

[0008] The present invention deposits a Ta-Ti binary hydrogen absorption transition layer on the substrate surface by magnetron co-sputtering. Appropriate Ti doping can promote the refinement of tantalum film grains and significantly reduce the residual internal stress of the tantalum film, thereby improving its film-base bonding strength and thermal conductivity.

[0009] In addition, the present invention finds that the ratio of Ta to Ti in the Ta-Ti binary hydrogen absorption transition layer has a significant effect on the morphology and physical phase of the coating. The appropriate doping of Ti atoms in the Ta film can refine the grains of the coating, and the physical properties of Ti and the substrate (such as Cu) are closer than Ta. The introduction of an appropriate amount of Ti atoms can effectively improve the bonding force. The difference between the co-sputtering preparation of the coating and the traditional single coating is that its atomic arrangement is more chaotic. Each element is interrupted by the second element before forming a continuous film, and only extremely small grains are formed. The higher the degree of chaos, the denser the atomic stacking. Therefore, the doping amount of Ti needs to be strictly controlled. If the Ti content is too little, the improvement effect is not obvious enough; if the Ti content is too much, excessive Ti doping will lead to an increase in the precipitation phase in the film, thereby having a negative impact on the corrosion resistance of the film.

[0010] Preferably, the thickness of the Ta-Ti binary hydrogen absorption transition layer is 1-30 microns (more preferably 20-30 microns).

[0011] After Ti is doped into the tantalum film, the transition layer can still have good bonding strength with the substrate surface even when it is thicker (usually, the thicker the transition layer, the higher the residual internal stress and the worse the bonding strength with the substrate).

[0012] In a second aspect, the present invention provides a method for preparing the above-mentioned Ta-Ti binary hydrogen absorption transition layer of the accelerator neutron source target, comprising: S1: Install the Ta target and the Ti target on two target positions of the magnetron sputtering coating machine respectively; fix the substrate on the mobile fixture trolley, pass inert gas (preferably argon) into the sputtering chamber, and close the sputtering chamber.

[0013] S2: Adjust the gas pressure in the sputtering chamber to 0.5-2Pa (further preferably 0.5-1Pa), adjust the sputtering power of the Ta target and the Ti target to 200-400W (further preferably 300-400W) and 50-200W (further preferably 100-200W), respectively, and the duty cycle to 30-90% (further preferably 60-90%), respectively, and perform magnetron co-sputtering coating, and control the mobile fixture trolley to move back and forth between the Ta target and the Ti target at a moving speed of 5-30mm / s (further preferably 15-20mm / s). After coating, a Ta-Ti binary hydrogen absorption transition layer is constructed on the surface of the substrate.

[0014] The present invention uses magnetron co-sputtering to ionize an inert gas such as argon under the action of an electric field, and the ionized argon ions bombard the surfaces of the Ta target and the Ti target, and the target material sputters a large number of target material atoms and deposits them on the surface of the substrate. The present invention regulates the atomic ratio and phase structure in the Ta-Ti binary hydrogen absorption transition layer by conditions such as sputtering power and trolley movement speed.

[0015] The base metal (such as commonly used Cu) usually has a huge difference in melting point from Ta. There is no intermetallic compound under thermal equilibrium conditions, and the difference in thermal expansion coefficient, atomic radius and electronegativity between Cu and Ta is large, which limits the solid solution diffusion capacity between the two, resulting in limited bonding between the Ta coating and the Cu substrate. The content of Ti atoms determines the quality of the film to a large extent, and there are multiple stable compounds with the change of composition. The Ti element has good corrosion resistance under various environments, which is conducive to improving the bonding performance between the coatings. The present invention finds that under the above-mentioned specific preferred sputtering conditions, during co-deposition, an ideal content of Ti can be introduced, and the introduced Ti atoms will interrupt the growth of Ta grains, thereby playing a role in fine grain strengthening, and the resulting film has a higher degree of disorder of Ti and Ta. When the degree of disorder is higher, there are more grain boundaries, and stress can also be released to a certain extent.

[0016] Preferably, in S1, the distance between the Ta target and the Ti target is 10-30 cm, and the distance between the Ta target and the sputtering chamber inlet is smaller than the distance between the Ti target and the sputtering chamber inlet.

[0017] Preferably, in S1, the reciprocating movement direction of the mobile fixture trolley is parallel to the straight line formed by the Ta target and the Ti target, and the spacing is 10-30 cm; the starting point and the end point of the reciprocating movement are flush with the Ta target and the Ti target respectively.

[0018] Preferably, the substrate is made of copper, vanadium, tungsten, gold, platinum, lead or alloys thereof.

[0019] Preferably, the electrolytic surface treatment method is: immersing the cathode and the substrate as the anode in an acid solution for electrolytic treatment; the temperature is 30-50°C, the current density is 5-50 mA·cm -2 Preferably, the electrolysis temperature is 30-40°C, and the current density is 5-20 mA·cm -2 , the time is 1 to 5 minutes. Further preferably, the acid solution is a 75 to 85 wt % phosphoric acid solution.

[0020] Preferably, the laser surface treatment method is: laser treatment of the substrate surface is performed by parallel laser scanning; the laser power is 0-20W, the pulse duration is 0-100ns, the laser line spacing is 5-30μm, and the scanning speed is 10-1000mm / s. Further preferably, the laser power is 10-20W, the pulse duration is 0-80ns, the laser line spacing is 5-20μm, and the scanning speed is 50-500mm / s.

[0021] Preferably, the Ta target and the Ti target are pre-sputtered before co-sputtering: the sputtering chamber is closed, evacuated, and then an inert gas (preferably argon) is introduced to perform pre-sputtering.

[0022] Preferably, during the pre-sputtering process, the vacuum is evacuated to a pressure of ≤5×10 -8 After Pa, an inert gas (preferably argon) is introduced to perform pre-sputtering. Preferably, Compared with the prior art, the beneficial effects of the present invention are: (1) The present invention deposits a Ta-Ti binary hydrogen absorption transition layer on the substrate surface by magnetron co-sputtering. The appropriate amount of Ti doping can promote the refinement of the tantalum film grains and significantly reduce the residual internal stress of the tantalum film, thereby improving its film-base bonding strength and thermal conductivity.

[0023] (2) The present invention utilizes magnetron co-sputtering to ensure good mechanical properties of the coating, and controls the sputtering process conditions, adjusts the Ti content, and refines the structure. The resulting Ta-Ti binary hydrogen absorption transition layer has the advantages of high density and uniform film formation.

[0024] (3) The production process of the method of the present invention has good repeatability, fast deposition speed, high process controllability, and is easy to realize industrialization. BRIEF DESCRIPTION OF THE DRAWINGS

[0025] Figure 1 The schematic diagram of the principle of magnetron co-sputtering of the present invention (the left side of the figure is a front view, and the right side of the figure is a side view); Figure 2 It is a schematic diagram of the principle of magnetron co-sputtering of the present invention (rendering); Figure 3 This is a scanning electron microscope photograph of the film after coating in Comparative Example 1 of the present invention; Figure 4 This is a scanning electron microscope photograph of the film after coating in Comparative Example 2 of the present invention; Figure 5 This is a scanning electron microscope photograph of the film after coating in Example 1 of the present invention; Figure 6 This is a scanning electron microscope photograph of the film after coating in Example 2 of the present invention; Figure 7 This is a scanning electron microscope photograph of the film after coating in Example 3 of the present invention; Figure 8 This is a scanning electron microscope photograph of the film after coating in Example 4 of the present invention; Fig. 9 This is a scanning electron microscope photograph of the film after coating in Comparative Example 3 of the present invention; Fig.10 This is a scanning electron microscope photograph of the film after coating in Example 5 of the present invention; Fig.11 This is a scanning electron microscope photograph of the film after coating in Example 6 of the present invention; Fig.12 This is a scanning electron microscope photograph of the film after coating in Example 7 of the present invention.

[0026] Reference numerals: Ta target 1, mobile fixture trolley 2, Ti target 3. DETAILED DESCRIPTION

[0027] The present invention will be further described below in conjunction with the embodiments.

[0028] Overall embodiment A Ta-Ti binary hydrogen absorption transition layer for an accelerator neutron source target is deposited on a substrate surface by magnetron co-sputtering technology. The Ta-Ti binary hydrogen absorption transition layer comprises uniformly distributed tantalum and titanium; the mass ratio of tantalum to titanium is 80:20-90:10.

[0029] In some specific embodiments, the mass ratio of tantalum to titanium is further preferably in the range of 85:15-90:10.

[0030] In some specific embodiments, the thickness of the Ta-Ti binary hydrogen absorption transition layer is in the range of 1-30 microns (more preferably 20-30 microns).

[0031] A method for preparing the above-mentioned Ta-Ti binary hydrogen absorption transition layer of the accelerator neutron source target comprises: S1: Figure 1 and Figure 2 As shown, the Ta target 1 and the Ti target 3 are respectively installed on two target positions of the magnetron sputtering coating machine; the substrate is fixed on the mobile fixture trolley 2, an inert gas (preferably argon) is passed into the sputtering chamber, and the sputtering chamber is closed.

[0032] In some specific embodiments, the substrate is made of copper, vanadium, tungsten, gold, platinum, lead or alloys thereof.

[0033] In some specific embodiments, in S1, the distance between the Ta target and the Ti target is 10-30 cm ( Figure 1 a), and the distance between the Ta target and the sputtering chamber inlet is smaller than the distance between the Ti target and the sputtering chamber inlet.

[0034] In some specific embodiments, in S1, the reciprocating movement direction of the mobile fixture trolley is parallel to the straight line formed by the Ta target and the Ti target, and the spacing is 20 cm ( Figure 1 b); the starting point and end point of the reciprocating movement are flush with the Ta target and the Ti target respectively.

[0035] S2: The gas pressure in the sputtering chamber is adjusted to 0.5-2Pa, the sputtering powers of the Ta target and the Ti target are adjusted to 200-400W and 50-200W respectively, and the duty cycle is 30-90%. Magnetron co-sputtering coating is performed, and the mobile fixture trolley is controlled to move back and forth between the Ta target and the Ti target at a moving speed of 5-30mm / s. After coating, a Ta-Ti binary hydrogen absorption transition layer is constructed on the surface of the substrate.

[0036] In some specific embodiments, in S2, the gas pressure in the sputtering chamber is adjusted to 0.5-1 Pa, the sputtering powers of the Ta target and the Ti target are adjusted to 300-400 W and 100-200 W respectively, the duty cycle is 60-90%, and the moving speed of the mobile fixture trolley is 15-20 mm / s.

[0037] In some specific embodiments, the electrolytic surface treatment method is: immersing the cathode and the substrate as the anode in an acid solution for electrolytic treatment; the temperature is 30-50°C, and the current density is 5-50 mA·cm-2 Preferably, the electrolysis temperature is 30-40°C, and the current density is 5-20 mA·cm -2 , the time is 1 to 5 minutes. Further preferably, the acid solution is a 75 to 85 wt % phosphoric acid solution.

[0038] In some specific embodiments, the laser surface treatment method is: laser treatment of the substrate surface is performed by parallel laser scanning; the laser power is 0-20W, the pulse duration is 0-100ns, the laser line spacing is 5-30μm, and the scanning speed is 10-1000mm / s. More preferably, the laser power is 10-20W, the pulse duration is 0-80ns, the laser line spacing is 5-20μm, and the scanning speed is 50-500mm / s.

[0039] In some specific embodiments, the Ta target and the Ti target are pre-sputtered before co-sputtering: the sputtering chamber is closed, evacuated, and then an inert gas is introduced to perform pre-sputtering.

[0040] In some more specific embodiments, during the pre-sputtering process, the pressure in the sputtering chamber is evacuated to ≤5×10 -8 After reaching Pa, inert gas is introduced and pre-sputtering is performed for 5-15 minutes.

[0041] Specific Examples and Comparative Examples Comparative Example 1 Substrate surface pretreatment: A 10*10*1mm copper sheet was used as the substrate, and polished with 80-grit sandpaper for 5 minutes, and then further polished with 200-grit and 400-grit sandpaper for 5 minutes each. Finally, the substrate was cleaned with acetone, alcohol and ultrapure water for 5 minutes respectively, and then dried in a vacuum drying oven for 1 hour.

[0042] Installation: The Ta target was installed on the target position of the magnetron sputtering coating machine (and the distance between the Ta target and the inlet of the sputtering chamber was 50 cm); the substrate was attached to a stainless steel plate and installed on the fixture of the magnetron sputtering equipment.

[0043] Pre-sputtering: Close the sputtering chamber and evacuate the chamber until the pressure is ≥5×10 -8 Pa, and then argon gas was introduced for pre-sputtering for 5 min.

[0044] Formal sputtering: single tantalum was deposited onto the substrate surface by magnetron sputtering (parameters: Ta target power 300 W, duty cycle 90%, sputtering pressure 0.5 Pa, sputtering time 1 hour).

[0045] Obtained by scanning electron microscopy Figure 3 It can be seen from the figure that a large area of ​​the film cracked and fell off, exposing the copper substrate.

[0046] Comparative Example 2 Substrate surface pretreatment: same as Comparative Example 1.

[0047] Installation: Install the Ta target and Ti target on the two target positions of the magnetron sputtering coating machine respectively (the distance between the Ta target and the Ti target is 20 cm, and the distances between the Ta target and the Ti target and the sampling port of the sputtering chamber are 50 cm and 70 cm respectively); stick the substrate on the stainless steel plate and fix it on the mobile fixture trolley (the reciprocating movement direction of the trolley is parallel to the straight line formed by the Ta target and the Ti target, and the distance is 20 cm; the starting point and end point of the reciprocating movement are flush with the Ta target and the Ti target respectively).

[0048] Pre-sputtering: Close the sputtering chamber and evacuate the chamber until the pressure is ≥5×10 -8 Pa, and then argon gas was introduced for pre-sputtering for 5 min.

[0049] Co-sputtering: Tantalum and titanium were co-deposited onto the substrate surface by magnetron sputtering (parameters: Ta target power 300 W, duty cycle 90%, Ti target power 50 W, duty cycle 90%, sputtering pressure 0.5 Pa, sputtering time 1 hour, trolley moving speed 15 mm / s).

[0050] Obtained by scanning electron microscopy Figure 4 It can be seen that the surface flatness is very low, a large number of particles are aggregated, and there is an island structure. At the same time, it can be seen that part of the copper matrix is ​​exposed and there are obvious cracks in the film.

[0051] Example 1 Substrate surface pretreatment: same as Comparative Example 1.

[0052] Installation: Install the Ta target and Ti target on the two target positions of the magnetron sputtering coating machine respectively (the distance between the Ta target and the Ti target is 20 cm, and the distances between the Ta target and the Ti target and the sampling port of the sputtering chamber are 50 cm and 70 cm respectively); stick the substrate on the stainless steel plate and fix it on the mobile fixture trolley (the reciprocating movement direction of the trolley is parallel to the straight line formed by the Ta target and the Ti target, and the distance is 20 cm; the starting point and end point of the reciprocating movement are flush with the Ta target and the Ti target respectively).

[0053] Pre-sputtering: Close the sputtering chamber and evacuate the chamber until the pressure is ≥5×10 -8 Pa, and then argon gas was introduced for pre-sputtering for 5 min.

[0054] Co-sputtering: Tantalum and titanium were co-deposited onto the substrate surface by magnetron sputtering (parameters: Ta target power 300 W, duty cycle 90%, Ti target power 100 W, duty cycle 90%, sputtering pressure 0.5 Pa, sputtering time 1 hour, trolley moving speed 15 mm / s).

[0055] Obtained by scanning electron microscopy Figure 5 ,As shown in the figure, it can be seen that the surface flatness is low, a lot of aggregation occurs, and the particle structure is uniform in size and dispersed.

[0056] Example 2 Substrate surface pretreatment: same as Comparative Example 1.

[0057] Installation: Install the Ta target and Ti target on the two target positions of the magnetron sputtering coating machine respectively (the distance between the Ta target and the Ti target is 20 cm, and the distances between the Ta target and the Ti target and the sampling port of the sputtering chamber are 50 cm and 70 cm respectively); stick the substrate on the stainless steel plate and fix it on the mobile fixture trolley (the reciprocating movement direction of the trolley is parallel to the straight line formed by the Ta target and the Ti target, and the distance is 20 cm; the starting point and end point of the reciprocating movement are flush with the Ta target and the Ti target respectively).

[0058] Pre-sputtering: Close the sputtering chamber and evacuate the chamber until the pressure is ≥5×10 -8 Pa, and then argon gas was introduced for pre-sputtering for 5 min.

[0059] Co-sputtering: Tantalum and titanium were co-deposited onto the substrate surface by magnetron sputtering (parameters: Ta target power 300 W, duty cycle 90%, Ti target power 150 W, duty cycle 90%, sputtering pressure 0.5 Pa, sputtering time 1 hour, trolley moving speed 15 mm / s).

[0060] Obtained by scanning electron microscopy Figure 6 It can be seen that the surface film has high flatness and few film defects.

[0061] Example 3 Substrate surface pretreatment: same as Comparative Example 1.

[0062] Installation: Install the Ta target and Ti target on the two target positions of the magnetron sputtering coating machine respectively (the distance between the Ta target and the Ti target is 20 cm, and the distances between the Ta target and the Ti target and the sampling port of the sputtering chamber are 50 cm and 70 cm respectively); stick the substrate on the stainless steel plate and fix it on the mobile fixture trolley (the reciprocating movement direction of the trolley is parallel to the straight line formed by the Ta target and the Ti target, and the distance is 20 cm; the starting point and end point of the reciprocating movement are flush with the Ta target and the Ti target respectively).

[0063] Pre-sputtering: Close the sputtering chamber and evacuate the chamber until the pressure is ≥5×10 -8 Pa, and then argon gas was introduced for pre-sputtering for 5 min.

[0064] Co-sputtering: Tantalum and titanium were co-deposited onto the substrate surface by magnetron sputtering (parameters: Ta target power 300 W, duty cycle 90%, Ti target power 200 W, duty cycle 90%, sputtering pressure 0.5 Pa, sputtering time 1 hour, trolley moving speed 15 mm / s).

[0065] Obtained by scanning electron microscopy Figure 7 , it can be seen that the surface flatness is good, and only a small amount of aggregated particles appear.

[0066] Example 4 Substrate surface pretreatment: same as Comparative Example 1.

[0067] Installation: Install the Ta target and Ti target on the two target positions of the magnetron sputtering coating machine respectively (the distance between the Ta target and the Ti target is 20 cm, and the distances between the Ta target and the Ti target and the sampling port of the sputtering chamber are 50 cm and 70 cm respectively); stick the substrate on the stainless steel plate and fix it on the mobile fixture trolley (the reciprocating movement direction of the trolley is parallel to the straight line formed by the Ta target and the Ti target, and the distance is 20 cm; the starting point and end point of the reciprocating movement are flush with the Ta target and the Ti target respectively).

[0068] Pre-sputtering: Close the sputtering chamber and evacuate the chamber until the pressure is ≥5×10 -8 Pa, and then argon gas was introduced for pre-sputtering for 5 min.

[0069] Co-sputtering: Tantalum and titanium were co-deposited onto the substrate surface by magnetron sputtering (parameters: Ta target power 300 W, duty cycle 90%, Ti target power 300 W, duty cycle 90%, sputtering pressure 0.5 Pa, sputtering time 1 hour, trolley moving speed 15 mm / s).

[0070] Obtained by scanning electron microscopy Figure 8 , it can be seen that the surface flatness is low and there are some cracks.

[0071] Comparative Example 3 Substrate surface pretreatment: same as Comparative Example 1.

[0072] Installation: Install the Ta target and Ti target on the two target positions of the magnetron sputtering coating machine respectively (the distance between the Ta target and the Ti target is 20 cm, and the distances between the Ta target and the Ti target and the sampling port of the sputtering chamber are 50 cm and 70 cm respectively); stick the substrate on the stainless steel plate and fix it on the mobile fixture trolley (the reciprocating movement direction of the trolley is parallel to the straight line formed by the Ta target and the Ti target, and the distance is 20 cm; the starting point and end point of the reciprocating movement are flush with the Ta target and the Ti target respectively).

[0073] Pre-sputtering: Close the sputtering chamber and evacuate the chamber until the pressure is ≥5×10 -8 Pa, and then argon gas was introduced for pre-sputtering for 5 min.

[0074] Co-sputtering: Tantalum and titanium were co-deposited onto the substrate surface by magnetron sputtering (parameters: Ta target power 300 W, duty cycle 90%, Ti target power 300 W, duty cycle 90%, sputtering pressure 0.5 Pa, sputtering time 1 hour, trolley moving speed 1 mm / s).

[0075] Obtained by scanning electron microscopy Fig. 9 , it can be seen that the film has obvious cracks.

[0076] Example 5 Substrate surface pretreatment: same as Comparative Example 1.

[0077] Installation: Install the Ta target and Ti target on the two target positions of the magnetron sputtering coating machine respectively (the distance between the Ta target and the Ti target is 20 cm, and the distances between the Ta target and the Ti target and the sampling port of the sputtering chamber are 50 cm and 70 cm respectively); stick the substrate on the stainless steel plate and fix it on the mobile fixture trolley (the reciprocating movement direction of the trolley is parallel to the straight line formed by the Ta target and the Ti target, and the distance is 20 cm; the starting point and end point of the reciprocating movement are flush with the Ta target and the Ti target respectively).

[0078] Pre-sputtering: Close the sputtering chamber and evacuate the chamber until the pressure is ≥5×10 -8 Pa, and then argon gas was introduced for pre-sputtering for 5 min.

[0079] Co-sputtering: Tantalum and titanium were co-deposited onto the substrate surface by magnetron sputtering (parameters: Ta target power 300 W, duty cycle 90%, Ti target power 300 W, duty cycle 90%, sputtering pressure 0.5 Pa, sputtering time 1 hour, trolley moving speed 5 mm / s).

[0080] Obtained by scanning electron microscopy Fig.10 It can be seen that the surface flatness is low, some pits appear, and the film falls off. At the same time, part of the copper substrate is exposed, and there are obvious cracks in the film.

[0081] Example 6 Substrate surface pretreatment: same as Comparative Example 1.

[0082] Installation: Install the Ta target and Ti target on the two target positions of the magnetron sputtering coating machine respectively (the distance between the Ta target and the Ti target is 20 cm, and the distances between the Ta target and the Ti target and the sampling port of the sputtering chamber are 50 cm and 70 cm respectively); stick the substrate on the stainless steel plate and fix it on the mobile fixture trolley (the reciprocating movement direction of the trolley is parallel to the straight line formed by the Ta target and the Ti target, and the distance is 20 cm; the starting point and end point of the reciprocating movement are flush with the Ta target and the Ti target respectively).

[0083] Pre-sputtering: Close the sputtering chamber and evacuate the chamber until the pressure is ≥5×10-8 Pa, and then argon gas was introduced for pre-sputtering for 5 min.

[0084] Co-sputtering: Tantalum and titanium were co-deposited onto the substrate surface by magnetron sputtering (parameters: Ta target power 300 W, duty cycle 90%, Ti target power 300 W, duty cycle 90%, sputtering pressure 0.5 Pa, sputtering time 1 hour, trolley moving speed 20 mm / s).

[0085] Obtained by scanning electron microscopy Fig.11 , it can be seen that the surface is relatively flat.

[0086] Example 7 Substrate surface pretreatment: same as Comparative Example 1.

[0087] Installation: Install the Ta target and Ti target on the two target positions of the magnetron sputtering coating machine respectively (the distance between the Ta target and the Ti target is 20 cm, and the distances between the Ta target and the Ti target and the sampling port of the sputtering chamber are 50 cm and 70 cm respectively); stick the substrate on the stainless steel plate and fix it on the mobile fixture trolley (the reciprocating movement direction of the trolley is parallel to the straight line formed by the Ta target and the Ti target, and the distance is 20 cm; the starting point and end point of the reciprocating movement are flush with the Ta target and the Ti target respectively).

[0088] Pre-sputtering: Close the sputtering chamber and evacuate the chamber until the pressure is ≥5×10 -8 Pa, and then argon gas was introduced for pre-sputtering for 5 min.

[0089] Co-sputtering: Tantalum and titanium were co-deposited onto the substrate surface by magnetron sputtering (parameters: Ta target power 300 W, duty cycle 90%, Ti target power 300 W, duty cycle 90%, sputtering pressure 0.5 Pa, sputtering time 1 hour, trolley moving speed 30 mm / s).

[0090] Obtained by scanning electron microscopy Fig.12 , it can be seen that the surface flatness is low, a large number of aggregations occur, and there are island structures. At the same time, it can be seen that part of the copper matrix is ​​exposed and there are obvious cracks in the film.

[0091] Performance Analysis The magnetron co-sputtering process conditions and performance test results of each embodiment and comparative example are shown in the following table: From the data in the above table, we can see that: In Comparative Examples 1-2 and Examples 1-4, the doping ratio of the Ti element in the film is adjusted by controlling the sputtering power of Ti palladium. By comparing the data, it can be found that Ti palladium is not sputtered in Comparative Example 1, so the resulting film is a pure tantalum film. The film stress is relatively high, and large-area cracking of the film is found. The Ti doping amount in Comparative Example 2 and Examples 1-4 is gradually increased, and it is found that the film stress is significantly lower than that in Comparative Example 1, which shows that the doping of the Ti element is beneficial to reducing the film stress. Furthermore, the effect of Examples 1-4 is better than that of Comparative Example 2, and Examples 2 and 3 are better than Examples 1 and 4, and Example 2 is the best, not only having the lowest film stress, but also having the best film appearance.

[0092] In Example 2, Comparative Example 3 and Examples 5-7, the coating quality is controlled by controlling the moving speed of the trolley. Through data comparison, it can be found that in Comparative Example 3, due to the slow moving speed of the trolley, the tantalum grains have enough time to nucleate and grow, and the number of grain boundaries is small, resulting in high film stress and poor film appearance. In Example 5, as the trolley speed increases in Example 2 and Example 6, the film stress decreases, but when Example 7 increases the speed to 30 mm / s, the film stress increases significantly. Therefore, the most preferred range is between Example 2 and Example 6.

[0093] Example 8 The difference between Example 8 and Example 3 is that the electrolytic treatment method used for substrate surface pretreatment is: (1) A 85 wt % phosphoric acid solution was used as the electrolytic solution and added into an electrolytic reactor. The electrolyte volume of the electrolytic reactor was 0.5 L.

[0094] (2) A copper sheet of 10*10*1 mm is used as an anode and a lead plate cathode of 30*30*1 mm is immersed in the electrolyte and fixed in position on the electrolytic reactor.

[0095] (3) Electrolysis pretreatment: Turn on the heating rod and observe the temperature with a thermometer. When the temperature rises to 40°C, turn on the power supply and set the current density to 20 mA cm -2 , the treatment time is 5 minutes; finally, the copper substrate is cleaned with acetone, alcohol and ultrapure water for 5 minutes respectively and then placed in a vacuum drying oven for drying for 1 hour.

[0096] After the above electrolytic pretreatment, a proper number of discrete microporous structures with a size of 3-5 microns can be constructed on the substrate surface. Compared with ordinary rough surfaces, these special discontinuous microporous structures not only increase the surface roughness of the substrate (increase the specific surface area), but more importantly, they are also conducive to the pinning effect of atomic sputtering during subsequent coating, which is more conducive to the bonding of the film substrate and also can play a better heat dissipation role during the deposition of thin films. In addition, we further found that in the later target application and service process, these microporous structures can also serve as air buffers, which is conducive to the extension of the target life. Therefore, compared with conventional surface treatment methods, electrolytic surface treatment has more advantages.

[0097] Example 9 The difference between Example 9 and Example 3 is that the laser treatment method used for substrate surface pretreatment is: A 10*10*1mm copper sheet was used as the substrate, and the laser parameters were set to laser power 15W, laser line spacing 15μm, pulse duration 50ns, scanning speed 500mm / s and laser scanning mode parallel, and then the copper sheet was surface treated.

[0098] Since the surface after laser treatment is a special surface between isotropy and anisotropy, its morphological characteristics are very different from those of traditional cutting and EDM surfaces. During the laser treatment process, the laser beam will generate high temperature while moving on the substrate surface, thereby vaporizing and melting the material, and the molten material will accumulate in the scanning direction of the laser, forming a series of parallel grooves with a width of 30 to 60 microns along the laser scanning track. In addition, we also found that the above-mentioned high-temperature melting and low-temperature solidification process will generate some irregular micropores with a size of about 5 to 30 microns on the surface of each groove. In the subsequent magnetron sputtering process, after the high-energy particles reach the parallel groove surface, the micropores on its surface can be better filled, thereby better improving the interlayer bonding between the coating and the substrate; when the neutron source target is in service for a long time, the microporous structure can also further facilitate heat diffusion and micro-area stress relief. Therefore, compared with conventional surface treatment methods, laser surface treatment has more advantages.

[0099] The raw materials and equipment used in the present invention, unless otherwise specified, are all commonly used raw materials and equipment in the art; the methods used in the present invention, unless otherwise specified, are all conventional methods in the art.

[0100] The above description is only a preferred embodiment of the present invention and does not limit the present invention in any way. Any simple modification, change and equivalent transformation made to the above embodiment based on the technical essence of the present invention still falls within the protection scope of the technical solution of the present invention.

Claims

1. A Ta-Ti binary hydrogen absorption transition layer for an accelerator neutron source target, characterized in that: The Ta-Ti binary hydrogen absorption transition layer is deposited on the substrate surface by magnetron co-sputtering technology, and includes uniformly distributed tantalum and titanium; the mass ratio of tantalum to titanium is 80:20-90:

10.

2. The Ta-Ti binary hydrogen absorption transition layer for accelerator neutron source target according to claim 1, characterized in that: The mass ratio of tantalum to titanium is 85:15-90:

10.

3. The Ta-Ti binary hydrogen absorption transition layer for accelerator neutron source target according to claim 1 or 2, characterized in that: The thickness is 1-30 microns.

4. A method for preparing a Ta-Ti binary hydrogen absorption transition layer for an accelerator neutron source target according to any one of claims 1 to 3, characterized in that include: S1: Install the Ta target and the Ti target on two target positions of the magnetron sputtering coating machine respectively; Fix the substrate on the mobile fixture trolley, pass inert gas into the sputtering chamber, and close the sputtering chamber; S2: Adjust the gas pressure in the sputtering chamber to 0.5-2Pa, adjust the sputtering power of the Ta target and the Ti target to 200-400W and 50-200W respectively, and the duty cycle to 30-90%. Perform magnetron co-sputtering coating, and control the mobile fixture trolley to move back and forth between the Ta target and the Ti target at a moving rate of 5-30mm / s. After coating, a Ta-Ti binary hydrogen absorption transition layer is constructed on the surface of the substrate.

5. The preparation method according to claim 4, characterized in that: In S2, the gas pressure in the sputtering chamber was adjusted to 0.5-1Pa, the sputtering powers of the Ta target and the Ti target were adjusted to 300-400W and 100-200W, respectively, the duty cycles were adjusted to 60-90%, and the moving speed of the mobile fixture trolley was adjusted to 15-20mm / s.

6. The preparation method according to claim 4 or 5, characterized in that: In S1, The distance between the Ta target and the Ti target is 10-30 cm, and the distance between the Ta target and the sputtering chamber inlet is smaller than the distance between the Ti target and the sputtering chamber inlet; and / or The reciprocating movement direction of the mobile fixture trolley is parallel to the straight line formed by the Ta target and the Ti target, and the spacing is 10-30 cm; the starting point and the end point of the reciprocating movement are flush with the Ta target and the Ti target respectively.

7. The preparation method according to claim 4, characterized in that: The material of the substrate is copper, vanadium, tungsten, gold, platinum, lead or an alloy thereof.

8. The preparation method according to claim 4, characterized in that: The substrate is subjected to surface pretreatment: the substrate is surface treated, cleaned, dried and then used for later use.

9. The preparation method according to claim 8, characterized in that: The surface treatment method is electrolytic surface treatment or laser surface treatment.

10. The preparation method according to claim 9, characterized in that: The electrolytic surface treatment method comprises: immersing the cathode and the substrate as the anode in an acid solution for electrolytic treatment; the temperature is 30-50° C., the current density is 5-50 mA·cm -2 , time is 1~10min.

11. The preparation method according to claim 9, characterized in that: The laser surface treatment method comprises: performing laser treatment on the substrate surface by parallel laser scanning; the laser power is 0-20W, the pulse duration is 0-100ns, the laser line spacing is 5-30μm, and the scanning speed is 10-1000mm / s.

12. The preparation method according to claim 4, characterized in that: The Ta target and the Ti target are pre-sputtered before co-sputtering: the sputtering chamber is closed, evacuated, and then an inert gas is introduced to perform pre-sputtering.

13. The preparation method according to claim 12, characterized in that: During the pre-sputtering process, the vacuum is evacuated to a pressure of ≤5×10 -8 After 30 0.5 Pa, inert gas is introduced for pre-sputtering.

Citation Information

Patent Citations

  • Electric conductor and process for its production

    CN101978431A

  • Method for efficiently preparing Ti-Ta high-temperature memory alloy thin film

    CN104388904A

  • A medical porous titanium-tantalum composite material

    CN109172862A

  • Low-stress film

    CN111763016A

  • Al2O3 / CrN composite insulating coating for high-frequency electrotome and preparation method thereof

    CN113737144A

Cited By

  • Method for improving bonding strength of tantalum coating on surface of biomedical peek material

    CN119615095A

  • Accelerator neutron source target composite transition layer and hydrothermal-magnetron sputtering preparation method thereof

    CN120026290A

  • Neutron source target substrate surface structure and laser surface treatment construction method thereof

    CN120129136A

  • Neutron source target substrate surface structure and its laser surface treatment construction method