Preparation method of safe and stable medical cold compress patch
By combining graphene oxide with aminated nano silica in medical cold compress patches to form a microsphere structure, combining magnesium sulfate and a variety of moisturizers to form a three-dimensional dual network structure, the existing cold compress patch has been solved by short and matching effects. The problem of skin injury has achieved rapid swelling and analgesia and long-term maintenance of hyperosmotic effects, significantly improving wound healing efficiency and skin health.
Patent Information
- Application Number
- CN202410622840.5
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-05-20
- Publication Date
- 2024-11-08
AI Technical Summary
Existing medical cold compress patches have short cold compresses and high frequency of replacement when treating wounds. They are harmful to the skin when using them for a long time. They cannot quickly repair skin tissue and promote wound healing.
Graphene oxide and aminated nanosilicon dioxide are used to form a microsphere structure, combining magnesium sulfate and a variety of moisturizers to form a cold compress patch with a three-dimensional dual network structure, and adsorb magnesium sulfate through the loose porous structure of the microsphere structure to maintain Hypersonic state achieves rapid swelling and analgesic effects and long-term maintenance.
It significantly accelerates the anti-swelling and analgesic effect, has strong and lasting effect, high safety, can effectively reduce nerve ending sensitivity, reduce vascular permeability, relieve edema symptoms, and is skin-friendly and does not easily cause dryness.
Smart Images

Figure CN118902729A_ABST
Abstract
Description
Technical Field
[0001] The present invention relates to the technical field of cold compress patches, and in particular to a method for preparing a safe and stable medical cold compress patch. Background Art
[0002] At present, traditional cold compress methods mainly use ice water, ice cubes, alcohol, etc. for cold compress, but these methods have short cold compress time, large dosage, uneven cold compress effect, easily cause local frostbite, and are inconvenient to carry and store.
[0003] At present, there is a cold compress patch on the market, which can shrink local capillaries, reduce local congestion, reduce the sensitivity of nerve endings, relieve pain, and reduce temperature and fever. The cold compress patch is improved based on the traditional cold compress method. It is generally composed of a backing layer, a gel layer and an anti-adhesive layer. It removes heat through the vaporization of water and natural cooling ingredients contained in the polymer gel to achieve local cooling and achieve the effect of cold compress to relieve pain.
[0004] For the treatment of common wounds, although medical cold compresses have a certain relief effect, the effect of treating wounds by physical cooling alone is minimal, and it cannot quickly repair skin tissue and promote wound healing. The existing method is to add certain drugs to the cold compress to treat wounds, which has a certain effect, but there are problems such as short effect and high replacement frequency. At the same time, long-term use is harmful to the skin and easily causes dry skin, which needs to be solved urgently. Summary of the invention
[0005] Based on the technical problems existing in the background technology, the present invention proposes a method for preparing a safe and stable medical cold compress patch.
[0006] A method for preparing a safe and stable medical cold compress patch comprises the following steps:
[0007] S1. Add thickener, gelatin, polyvinyl alcohol and cooling agent to water, stir at 70-80° C. for 10-30 min, and ultrasonically treat for 5-12 min to obtain premixed solution a;
[0008] S2, adding polyethylene glycol and aminated nano-silica to the graphene oxide solution, adjusting the pH value of the system to 2-4, adding toluene and stirring, adding calcium chloride, stirring at 70-80° C. for 5-15 min, cooling to room temperature, standing for 10-20 h, centrifuging, washing, and vacuum drying to obtain a silica composite;
[0009] S3, calcining the silicon dioxide composite at 200-380° C. for 1-2 h, cooling to room temperature, crushing, adding magnesium sulfate and water, stirring, adding sodium carboxymethyl cellulose, thickener, humectant, and glycerol, stirring to obtain a premixed solution b;
[0010] S4. Apply the premixed liquid b evenly on one side of the backing layer to form a first gel layer, and then apply the premixed liquid a on the other side of the backing layer to form a second gel layer. Cool to -10 to -20°C, keep for 1-2 hours, warm to room temperature, press on a polyethylene film, let stand for 1-2 hours, cut, and solidify.
[0011] Preferably, in S1, the mass ratio of thickener, gelatin, polyvinyl alcohol and cooling agent is 1-10:1-2:1-2:1-5.
[0012] Preferably, in S1, the degree of polymerization of polyvinyl alcohol is 500-600.
[0013] Preferably, in S1, the cooling agent is menthyl lactate.
[0014] Preferably, in S1, the ultrasonic frequency is 5-15kHz, and the ultrasonic power is 100-200W.
[0015] Preferably, in S2, the concentration of the graphene oxide solution is 0.2-0.6 mg / mL, and the mass ratio of the graphene oxide solution, polyethylene glycol, aminated nano-silica, toluene, and calcium chloride is 10-20:1-2:1-5:10-20:1-2.
[0016] Preferably, in S2, 0.5-1.2 mol / L hydrochloric acid is used to adjust the pH value of the system to 2-4.
[0017] Preferably, in S3, the mass ratio of the silicon dioxide composite, magnesium sulfate, sodium carboxymethyl cellulose, thickener, humectant and glycerol is 4-8:0.57-1.19:1-2:10-20:5-12:1-3.
[0018] Preferably, in S3, the thickener is at least one of propylene glycol alginate, casein, sodium polyacrylate, polyoxyethylene, and polyvinyl pyrrolidone.
[0019] Preferably, in S3, the moisturizing agent is sodium pyrrolidone carboxylate, sodium hyaluronate, hydroxyethyl urea or / and sorbitol.
[0020] Preferably, in S4, non-woven fabric or silk mask cloth is used as the backing layer.
[0021] A safe and stable medical cold compress patch is prepared by adopting the preparation method of the safe and stable medical cold compress patch.
[0022] Beneficial effects:
[0023] The present invention adopts a compound of graphene oxide and aminated nano-silicon dioxide to form a microsphere structure, reacts the carboxyl group at the edge of the graphene oxide under the action of calcium chloride, effectively stabilizes the microsphere structure, removes the internal oil phase by drying, and further calcines to remove the graphene oxide. The obtained hollow microspheres form a large number of channel structures with a large specific surface area and high adsorption activity. The loose and porous structure can effectively adsorb magnesium sulfate. During the cold compress process, as the water evaporates to a certain extent, the first gel layer of the present invention can maintain the magnesium sulfate concentration, effectively maintain its hypertonic state, and quickly relieve the inflammatory edema of the damaged tissue.
[0024] The applicant has found through experiments that adsorbing magnesium sulfate into the active microsphere structure and then adding it to the gel layer can not only accelerate the reduction of swelling, relieve pain and itching, and is 2-3 times faster than ordinary cold compresses, but also can maintain the hypertonic effect for a long time, with a strong and lasting effect, and is safe and harmless to the human body.
[0025] The present invention first applies the premixed liquid a and then compounds it with the premixed liquid b. The junction of the two layers of premixed liquid forms a three-dimensional double network structure, which not only has extremely high bonding strength, but also can play a good coagulation role, can absorb and retain a large amount of water to form a gel, and has good stability, so that the water can fully contact with the skin, and the heated part of the skin evaporates the water, and absorbs the surrounding heat during the evaporation of the water, so as to achieve the effect of cooling and heat preservation. At the same time, as the water continues to evaporate, when the water loss reaches a certain level, the magnesium sulfate concentration can be effectively guaranteed to maintain the hypertonic effect, and the effect is long-lasting.
[0026] The cold compress of the present invention can effectively reduce the sensitivity of human nerve endings, and the blood vessels will contract under the action of cold receptors, thereby reducing vascular permeability and relieving edema symptoms, thereby achieving the effect of reducing swelling and relieving pain. It has the advantages of good effect, low cost, high safety, good durability, etc. BRIEF DESCRIPTION OF THE DRAWINGS
[0027] Figure 1 This is the SEM image of the silica composite obtained in Example 5.
[0028] Figure 2 This is a comparison chart of injury degree scores of rats with acute soft tissue injury after applying the cold compress obtained in Example 5 and Comparative Examples 1-2 and the normal saline dressing.
[0029] Figure 3 This is a comparison chart of the effects of using the cold compress obtained in Example 5 and Comparative Examples 1-2 and a normal saline dressing on relieving itching caused by histamine.
[0030] Figure 4 This is a comparison chart of the tensile strength of the cold compress patches obtained in Example 5 and Comparative Examples 1-2.
[0031] Figure 5This is a comparison chart of the moisturizing performance of the cold compress patches obtained in Example 5 and Comparative Examples 1-2.
[0032] Figure 6 This is a comparison chart of the improvement of eye skin moisture after applying the cold compress obtained in Example 5 and Comparative Examples 1-2 to the outer side of the outer canthus. Figure 7 The osmotic pressure change curves of the first gel layer of the cold compress obtained in Example 5 when applied to the skin surface of the back of a volunteer's hand, at room temperature, and in a 37°C oven. DETAILED DESCRIPTION
[0033] The technical solution of the present invention is described in detail below through specific embodiments.
[0034] Example 1
[0035] A method for preparing a safe and stable medical cold compress patch comprises the following steps:
[0036] S1, add 1kg of propylene glycol alginate, 1kg of gelatin, 1kg of polyvinyl alcohol with a polymerization degree of 500, and 1kg of menthyl lactate to 20kg of purified water, stir at 70°C for 10min, stir at a speed of 50r / min, and perform ultrasonic treatment for 5min, at an ultrasonic frequency of 5kHz and an ultrasonic power of 100W, to obtain a premixed solution a;
[0037] S2, add 1kg polyethylene glycol and 1kg aminated nano-silica to 10kg of 0.2mg / mL graphene oxide solution, adjust the pH value of the system to 2-4 with 0.5mol / L hydrochloric acid, add 10kg toluene, stir at 1000r / min for 10min, add 1kg calcium chloride, stir at 70°C for 5min, cool to room temperature, stand for 10h, centrifuge, wash with deionized water, and vacuum dry to obtain a silica composite;
[0038] S3, calcine 4 kg of silicon dioxide composite at 200 ° C for 1 h, cool to room temperature, crush, add 0.57 kg of magnesium sulfate and 10 kg of purified water, stir at a speed of 1000 r / min for 5 min, reduce the speed to 50 r / min, add 1 kg of sodium carboxymethyl cellulose, 10 kg of propylene glycol alginate, 5 kg of hydroxyethyl urea, and 1 kg of glycerol, stir for 1 h to obtain a premixed solution b;
[0039] S4. Evenly apply the premixed liquid b on one side of the backing layer to form the first gel layer, and then apply the premixed liquid a on the other side of the backing layer to form the second gel layer. Cool to -10°C, keep for 1 hour, warm to room temperature, press on a polyethylene film, let stand for 1 hour, cut, and solidify.
[0040] Example 2
[0041] A method for preparing a safe and stable medical cold compress patch comprises the following steps:
[0042] S1. Add 10 kg of casein, 2 kg of gelatin, 2 kg of polyvinyl alcohol with a polymerization degree of 600, and 5 kg of menthyl lactate to 30 kg of purified water, stir at 80° C. for 30 min, at a stirring speed of 100 r / min, and perform ultrasonic treatment for 12 min at an ultrasonic frequency of 15 kHz and an ultrasonic power of 200 W to obtain a premixed solution a.
[0043] S2, add 2kg polyethylene glycol and 5kg aminated nano-silica to 20kg of 0.6mg / mL graphene oxide solution, adjust the pH value of the system to 2-4 with 1.2mol / L hydrochloric acid, add 20kg toluene, stir at 2000r / min for 30min, add 2kg calcium chloride, stir at 80°C for 15min, cool to room temperature, stand for 20h, centrifuge, wash with deionized water, and vacuum dry to obtain a silica composite;
[0044] S3, calcine 8kg of silicon dioxide composite at 380°C for 2h, cool to room temperature, crush, add 1.19kg of magnesium sulfate and 20kg of purified water, stir at 2000r / min for 12min, reduce the speed to 80r / min, add 2kg of sodium carboxymethyl cellulose, 20kg of casein, 12kg of sorbitol and 3kg of glycerol, stir for 2h to obtain premixed solution b;
[0045] S4. Evenly apply the premixed liquid b on one side of the backing layer to form a first gel layer, and then apply the premixed liquid a on the other side of the backing layer to form a second gel layer. Cool to -20°C, keep for 2 hours, warm to room temperature, press on a polyethylene film, let stand for 2 hours, cut, and solidify.
[0046] Example 3
[0047] A method for preparing a safe and stable medical cold compress patch comprises the following steps:
[0048] S1, add 3kg sodium polyacrylate, 1.8kg gelatin, 1.3kg polyvinyl alcohol with a polymerization degree of 580, and 2kg menthyl lactate to 28kg purified water, stir at 72°C for 25min, stir at a speed of 70r / min, and perform ultrasonic treatment for 10min, with an ultrasonic frequency of 6kHz and an ultrasonic power of 170W, to obtain a premixed solution a;
[0049] S2, add 1.3kg polyethylene glycol and 4kg aminated nano-silica to 13kg of 0.5mg / mL graphene oxide solution, adjust the pH value of the system to 2-4 with 0.6mol / L hydrochloric acid, add 17kg toluene, stir at 1300r / min for 25min, add 1.3kg calcium chloride, stir at 77°C for 8min, cool to room temperature, stand for 18h, centrifuge, wash with deionized water, and vacuum dry to obtain a silica composite;
[0050] S3, calcining 5 kg of silicon dioxide composite at 320 ° C for 80 min, cooling to room temperature, crushing, adding 0.8 kg of magnesium sulfate and 12 kg of purified water, stirring at a speed of 1800 r / min for 6 min, reducing the speed to 70 r / min, adding 1.3 kg of sodium carboxymethyl cellulose, 17 kg of polyethylene oxide, 6 kg of sodium pyrrolidone carboxylate, and 2.5 kg of glycerol, stirring for 80 min, and obtaining a premixed solution b;
[0051] S4. Evenly apply the premixed liquid b on one side of the backing layer to form a first gel layer, and then apply the premixed liquid a on the other side of the backing layer to form a second gel layer. Cool to -18°C, keep for 80 minutes, warm to room temperature, press on a polyethylene film, let stand for 100 minutes, cut, and solidify.
[0052] Example 4
[0053] A method for preparing a safe and stable medical cold compress patch comprises the following steps:
[0054] S1, add 7kg of polyethylene oxide, 1.2kg of gelatin, 1.7kg of polyvinyl alcohol with a degree of polymerization of 520, and 4kg of menthyl lactate to 24kg of purified water, stir at 78°C for 15min, stir at a speed of 90r / min, and perform ultrasonic treatment for 8min, with an ultrasonic frequency of 12kHz and an ultrasonic power of 130W, to obtain a premixed solution a;
[0055] S2, add 1.7kg polyethylene glycol and 2kg aminated nano-silica to 17kg of 0.3mg / mL graphene oxide solution, adjust the pH value of the system to 2-4 with 1mol / L hydrochloric acid, add 13kg toluene, stir at 1700r / min for 15min, add 1.7kg calcium chloride, stir at 73°C for 12min, cool to room temperature, stand for 12h, centrifuge, wash with deionized water, and vacuum dry to obtain a silica composite;
[0056] The silicon dioxide composite obtained in this example was scanned by electron microscope. Figure 1 shown.
[0057] S3, calcining 7kg of silicon dioxide composite at 260°C for 100min, cooling to room temperature, crushing, adding 0.93kg of magnesium sulfate and 18kg of purified water, stirring at 1200r / min for 10min, reducing the speed to 60r / min, adding 1.7kg of sodium carboxymethyl cellulose, 13kg of sodium polyacrylate, 10kg of sodium pyrrolidone carboxylate, and 1.5kg of glycerol, stirring for 100min, and obtaining premixed solution b;
[0058] S4. Evenly apply the premixed liquid b on one side of the backing layer to form the first gel layer, and then apply the premixed liquid a on the other side of the backing layer to form the second gel layer. Cool to -12°C, keep for 100 minutes, warm to room temperature, press on a polyethylene film, let stand for 80 minutes, cut, and solidify.
[0059] Example 5
[0060] A method for preparing a safe and stable medical cold compress patch comprises the following steps:
[0061] S1, add 5 kg of polyvinyl pyrrolidone, 1.5 kg of gelatin, 1.5 kg of polyvinyl alcohol with a degree of polymerization of 550, and 3 kg of menthyl lactate to 26 kg of purified water, stir at 75°C for 20 min, stir at a speed of 80 r / min, and perform ultrasonic treatment for 9 min, at an ultrasonic frequency of 9 kHz and an ultrasonic power of 150 W, to obtain a premixed solution a;
[0062] S2, add 1.5kg polyethylene glycol and 3kg aminated nano-silica to 15kg of 0.4mg / mL graphene oxide solution, adjust the pH value of the system to 2-4 with 0.8mol / L hydrochloric acid, add 15kg toluene, stir at 1500r / min for 20min, add 1.5kg calcium chloride, stir at 75°C for 10min, cool to room temperature, stand for 15h, centrifuge, wash with deionized water, and vacuum dry to obtain a silica composite;
[0063] S3, calcining 6 kg of silicon dioxide composite at 300 ° C for 90 min, cooling to room temperature, crushing, adding 0.87 kg of magnesium sulfate and 15 kg of purified water, stirring at a speed of 1500 r / min for 8 min, reducing the speed to 65 r / min, adding 1.5 kg of sodium carboxymethyl cellulose, 15 kg of polyvinyl pyrrolidone, 8 kg of sodium hyaluronate, and 2 kg of glycerol, stirring for 90 min, and obtaining a premixed solution b;
[0064] S4. Evenly apply the premixed liquid b on one side of the backing layer to form a first gel layer, and then apply the premixed liquid a on the other side of the backing layer to form a second gel layer. Cool to -15°C, keep for 90 minutes, warm to room temperature, press on a polyethylene film, let stand for 90 minutes, cut, and solidify.
[0065] Comparative Example 1
[0066] A method for preparing a cold compress patch comprises the following steps:
[0067] S1, add 5 kg of polyvinyl pyrrolidone, 1.5 kg of gelatin, 1.5 kg of polyvinyl alcohol with a degree of polymerization of 550, and 3 kg of menthyl lactate to 26 kg of purified water, stir at 75°C for 20 min, stir at a speed of 80 r / min, and perform ultrasonic treatment for 9 min, at an ultrasonic frequency of 9 kHz and an ultrasonic power of 150 W, to obtain a premixed solution a;
[0068] S2, add 6 kg of monodisperse silica microspheres (article number S2-00300, purchased from Daye (Tianjin) Technology Co., Ltd.) and 0.87 kg of magnesium sulfate to 15 kg of purified water, stir at a speed of 1500 r / min for 8 min, reduce the speed to 65 r / min, add 1.5 kg of sodium carboxymethyl cellulose, 15 kg of polyvinyl pyrrolidone, 8 kg of sodium hyaluronate, and 2 kg of glycerol, stir for 90 min to obtain a premixed solution b;
[0069] S3. Evenly apply the premixed liquid b on one side of the backing layer to form a first gel layer, and then apply the premixed liquid a on the other side of the backing layer to form a second gel layer. Cool to -15°C, keep for 90 minutes, warm to room temperature, press on a polyethylene film, let stand for 90 minutes, cut, and solidify.
[0070] Comparative Example 2
[0071] A method for preparing a cold compress patch comprises the following steps:
[0072] S1, add 5 kg of polyvinyl pyrrolidone, 1.5 kg of gelatin, 1.5 kg of polyvinyl alcohol with a degree of polymerization of 550, and 3 kg of menthyl lactate to 26 kg of purified water, stir at 75°C for 20 min, stir at a speed of 80 r / min, and perform ultrasonic treatment for 9 min, at an ultrasonic frequency of 9 kHz and an ultrasonic power of 150 W, to obtain a premixed solution a;
[0073] S2, add 1.5kg polyethylene glycol and 3kg aminated nano-silica to 15kg of 0.4mg / mL graphene oxide solution, adjust the pH value of the system to 2-4 with 0.8mol / L hydrochloric acid, add 15kg toluene, stir at 1500r / min for 20min, add 1.5kg calcium chloride, stir at 75°C for 10min, cool to room temperature, stand for 15h, centrifuge, wash with deionized water, and vacuum dry to obtain a silica composite;
[0074] S3, crush 6 kg of silicon dioxide composite, add 0.87 kg of magnesium sulfate and 15 kg of purified water, stir at a speed of 1500 r / min for 8 min, reduce the speed to 65 r / min, add 1.5 kg of sodium carboxymethyl cellulose, 15 kg of polyvinyl pyrrolidone, 8 kg of sodium hyaluronate, and 2 kg of glycerol, stir for 90 min to obtain premixed solution b;
[0075] S4. Evenly apply the premixed liquid b on one side of the backing layer to form a first gel layer, and then apply the premixed liquid a on the other side of the backing layer to form a second gel layer. Cool to -15°C, keep for 90 minutes, warm to room temperature, press on a polyethylene film, let stand for 90 minutes, cut, and solidify.
[0076] Test Example I
[0077] The cold compress obtained in Example 5 and Comparative Examples 1-2 was used to conduct an irritation test, and the specific steps are as follows:
[0078] Take the rabbit to be tested, use sterilized surgical scissors to remove the hair on its back, remove the remaining hair with an appropriate amount of depilatory cream, and wash the remaining depilatory cream and the fallen hair with warm water; place the depilated rabbit in a dry and clean breeding environment and feed it for 24 hours; take out the treated rabbit, inject 1% sodium pentobarbital into the ear vein at a dosage of 30 mg / kg, and when the rabbit is comatose, divide the two sides of its back into 6 mutually symmetrical areas, marked as the test part, the positive control part and the negative control part. Apply the cold compress obtained in Example 5 and Comparative Examples 1-2 to the test part; immerse 150 μL of a 20% sodium dodecyl sulfate aqueous solution in a gauze of appropriate size and apply it to the positive control part; immerse 150 μL of a 1×PBS solution in a gauze of appropriate size and apply it to the negative control part. The rabbits were cultured in a dry and clean environment for 4 hours, and then the gauze and experimental samples were removed. The residual substances on the back of the rabbits were carefully cleaned with warm water and the erythema and edema of the tested parts on the back of the rabbits were observed.
[0079] The positive controls all showed severe irritation, while the negative controls had no irritation, indicating that the experimental model and conditions were established in accordance with the irritation standard. The cold compresses obtained in Example 5 and Comparative Examples 1-2 did not show any irritation, indicating that the three were safe to use, non-irritating and non-allergenic, and met the requirements of medical cold compresses.
[0080] Test Example II
[0081] The cold compress obtained in Example 5 and Comparative Examples 1-2 was used to carry out a swelling reduction test, and the specific steps are as follows:
[0082] Male SPF SD rats (3 months old, weighing 225±25g) were taken. After anesthesia, a mark was made on the posterior and lateral side of the left thigh of the rat 1cm away from the popliteal fossa, and the hair at the mark was shaved. The left lower limb of the rat was straightened and fixed on the base of the impactor, and covered with gauze to avoid breaking the skin. One end of a 50cm high and 2.5cm diameter PVC tube was placed vertically on the left leg, with the tube mouth aligned with the mark; the bottom end of a 150g weight with a diameter of about 2cm was placed parallel to the top plane of the hollow tube, and it was released to allow it to fall freely from a height of 50cm and hit the soft tissue around the mark on the left lower limb of the rat, impacting a contact surface of about 1cm. 2 Repeat the above striking action 3 times, and the model is successful when obvious subcutaneous bleeding and / or swelling of the soft tissue at the striking site appears.
[0083] 52 rats with successful modeling were randomly divided into Example 5 group, Comparative Example 1 group, Comparative Example 2 group and blank control group. The Example 5 group and Comparative Example 1-2 group were applied with the cold compress obtained in Example 5 and Comparative Example 1-2 to the impacted part, respectively. The blank control group was applied with a sterile dressing soaked in physiological saline to the impacted part, and fixed and bandaged with a sanitary adhesive tape. The application was performed once a day for 4 hours each time.
[0084] The rats were evaluated in terms of pain response, redness and swelling range, and lameness after the application. No pain response was scored as 0, mild pain response as 1, and significant pain response as 2; no redness and swelling as 0, redness and swelling range of 0-2 cm as 1, and redness and swelling range of 2-4 cm as 2; no lameness as 0, mild lameness as 1, and severe lameness as 2.
[0085] like Figure 2 As shown, the cold compress obtained in Example 5 can quickly relieve acute soft tissue injuries, has the effects of reducing swelling and relieving pain, and promotes the body's self-healing.
[0086] Test Example III
[0087] Male SPF SD rats (3 months old, weighing 225±25g) were subcutaneously injected with 0.1mL of 0.001g / mL histamine solution into the back of the rats. 52 injected rats were randomly divided into Example 5 group, Comparative Example 1 group, Comparative Example 2 group and blank control group. Example 5 group and Comparative Example 1-2 group were applied with the cold compress obtained in Example 5 and Comparative Example 1-2 at the injection site, respectively. The blank control group was applied with a sterile dressing soaked in physiological saline at the injection site, and fixed and bandaged with sanitary adhesive tape.
[0088] The number of times was used as the unit of calculation. The rat scratched its head with its front paws, scratched its trunk with its hind paws, and licked various parts with its mouth, which was considered an itching episode. The total number of itching attacks within 10 minutes was recorded.
[0089] like Figure 3As shown, the number of itching in Example 5 group was significantly reduced compared with other groups (P<0.05), which confirmed that the cold compress obtained by the present invention can inhibit the itching caused by histamine solution and has a certain anti-allergic effect.
[0090] Test Example IV
[0091] The tensile strength of the cold compress obtained in Example 5 and Comparative Examples 1-2 was tested. Figure 4 As shown, the tensile strength of the cold compress obtained in Example 5 is the highest, indicating that the cold compress obtained in the present invention has the best elasticity and is not easy to tear.
[0092] Test Example V
[0093] The moisturizing performance of the cold compress obtained in Example 5 and Comparative Examples 1-2 was tested, and the specific operation was as follows: the cold compress sample was weighed to obtain a mass m1, and the mass was weighed after being fully soaked in purified water for 24 hours to obtain a mass m2. The saturated cold compress finished product was then placed in a constant temperature environment of 34°C, and the mass change of the cold compress was recorded every 0.5 hours to compare the weight of the cold compress each time it lost water.
[0094] like Figure 5 As shown, within the same period of time, the water loss weight of the cold compress obtained in Example 5 is smaller, indicating that the cold compress obtained in the present invention has better moisturizing performance.
[0095] Test Example VI
[0096] A skin moisture tester was used to measure the moisture content of the stratum corneum of the periocular skin using the capacitance method. Dynamic monitoring was performed in a constant temperature and humidity environment laboratory at a temperature of 21±1°C and a humidity of 50±10%. After the volunteers cleaned the periocular skin and waited for 30 minutes, the cold compress obtained in Example 5 and Comparative Examples 1-2 was randomly selected on the outer side of the outer canthus of the left or right eye, and the other side was used as a blank control area. The moisture content of the blank control area and the cold compress test area after the test was recorded.
[0097] The time is taken as the horizontal axis, and the difference in water content between the cold compress test area and the blank control area in each group is taken as the vertical axis. Figure 6 The cold compress of each group can continuously increase the moisture content of the eye skin, and the cold compress obtained in Example 5 has a more obvious effect, which proves that the cold compress obtained in the present invention can make moisture absorbed by the skin without damaging the stratum corneum of the skin, thereby increasing the elasticity of the skin and improving the skin condition.
[0098] Test Example VII
[0099] 36 cold compresses obtained in Example 5 were randomly divided into three groups: the experimental group (12 pieces) were flatly attached to the skin surface of the back of the hand of volunteers (normal people), the control group A (12 pieces) were placed at room temperature (20.00° C.), and the control group B (12 pieces) were placed in a 37.00° C. oven. The osmotic pressure of the first gel layer was measured and calculated at different times, and a curve was drawn.
[0100] like Figure 7 As shown, the osmotic pressure of the cold compress obtained in Example 5 increases with time under different conditions, which proves that as the water continues to evaporate, when the water loss reaches a certain level, the present invention can effectively ensure the concentration of magnesium sulfate to maintain a hypertonic effect. When the cold compress obtained in Example 5 is attached to human skin, it is still in an isotonic state (309.67mOsm / L) at 30 minutes, and then it turns into a hypertonic state.
[0101] At the same time, volunteers reported that the direct cooling sensation from the cold compress applied to the back of the hand lasted for about 4 hours.
[0102] The above description is only a preferred specific implementation manner of the present invention, but the protection scope of the present invention is not limited thereto. Any technician familiar with the technical field can make equivalent replacements or changes according to the technical scheme and inventive concept of the present invention within the technical scope disclosed by the present invention, which should be covered by the protection scope of the present invention.
Claims
1. A method for preparing a safe and stable medical cold compress patch, characterized in that: The steps include: S1. Add thickener, gelatin, polyvinyl alcohol and cooling agent to water, stir at 70-80° C. for 10-30 min, and ultrasonically treat for 5-12 min to obtain premixed solution a; S2, adding polyethylene glycol and aminated nano-silica to the graphene oxide solution, adjusting the pH value of the system to 2-4, adding toluene and stirring, adding calcium chloride, stirring at 70-80° C. for 5-15 min, cooling to room temperature, standing for 10-20 h, centrifuging, washing, and vacuum drying to obtain a silica composite; S3, calcining the silicon dioxide composite at 200-380° C. for 1-2 h, cooling to room temperature, crushing, adding magnesium sulfate and water, stirring, adding sodium carboxymethyl cellulose, thickener, humectant, and glycerol, stirring to obtain a premixed solution b; S4. Apply the premixed liquid b evenly on one side of the backing layer to form a first gel layer, and then apply the premixed liquid a on the other side of the backing layer to form a second gel layer. Cool to -10 to -20°C, keep for 1-2 hours, warm to room temperature, press on a polyethylene film, let stand for 1-2 hours, cut, and solidify.
2. The method for preparing the safe and stable medical cold compress patch according to claim 1, characterized in that: In S1, the mass ratio of thickener, gelatin, polyvinyl alcohol and cooling agent is 1-10:1-2:1-2:1-5.
3. The method for preparing the safe and stable medical cold compress patch according to claim 1, characterized in that: In S1, the degree of polymerization of polyvinyl alcohol is 500-600.
4. The method for preparing the safe and stable medical cold compress patch according to claim 1, characterized in that: In S1, the cooling agent is menthyl lactate.
5. The method for preparing the safe and stable medical cold compress patch according to claim 1, characterized in that: In S1, the ultrasonic frequency is 5-15kHz and the ultrasonic power is 100-200W.
6. The method for preparing the safe and stable medical cold compress patch according to claim 1, characterized in that: In S2, the concentration of the graphene oxide solution is 0.2-0.6 mg / mL, and the mass ratio of the graphene oxide solution, polyethylene glycol, aminated nano-silica, toluene, and calcium chloride is 10-20:1-2:1-5:10-20:1-2.
7. The method for preparing the safe and stable medical cold compress patch according to claim 1, characterized in that: In S2, the pH value of the system is adjusted to 2-4 using hydrochloric acid with a concentration of 0.5-1.2 mol / L.
8. The method for preparing the safe and stable medical cold compress patch according to claim 1, characterized in that: In S3, the mass ratio of silicon dioxide complex, magnesium sulfate, sodium carboxymethyl cellulose, thickener, humectant and glycerol is 4-8: 0.57-1.19:1-2:10-20:5-12:1-3。 9. The method for preparing the safe and stable medical cold compress patch according to claim 1, characterized in that: The thickener is at least one of propylene glycol alginate, casein, sodium polyacrylate, polyoxyethylene, and polyvinyl pyrrolidone; the moisturizer is sodium pyrrolidone carboxylate, sodium hyaluronate, hydroxyethyl urea or / and sorbitol.
10. A safe and stable medical cold compress patch, characterized in that: The safe and stable medical cold compress patch is prepared by the preparation method of any one of claims 1 to 9.