Nano-porous B-site high-entropy perovskite oxide electro-catalytic material as well as preparation method and application of nano-porous B-site high-entropy perovskite oxide electro-catalytic material

By preparing nanoporous B-site high-entropy perovskite oxide electrocatalytic materials, the problems of low availability of precious metal catalysts and high energy consumption in preparation have been solved, achieving low-cost and high-efficiency electrocatalytic hydrogen evolution and water splitting performance, with excellent electrocatalytic activity and broad application prospects.

CN118908301APending Publication Date: 2024-11-08QILU UNIVERSITY OF TECHNOLOGY (SHANDONG ACADEMY OF SCIENCES)

Patent Information

Application Number
CN202410960804.X
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-07-17
Publication Date
2024-11-08

AI Technical Summary

Technical Problem

The existing precious metal catalysts used in water electrolysis for hydrogen production are in short supply and expensive, and traditional preparation methods are energy-intensive, failing to effectively replace non-precious metal electrocatalysts and affecting the efficiency of the electrocatalytic hydrogen evolution reaction.

Method used

LaBO3 nanoporous structures were prepared by using nanoporous B-site high-entropy perovskite oxide electrocatalytic materials through melting, spinning, dealloying and annealing. The B-site elements were Fe, Co, Cr, Mn, Ni or Ru. Combined with alloy design and annealing methods, materials with high electrocatalytic activity were prepared.

Benefits of technology

We have achieved low-cost and high-efficiency preparation of nanoporous B-site high-entropy perovskite oxide electrocatalytic materials, which improves the electrocatalytic hydrogen evolution reaction rate and overall water splitting performance, solves the problem of precious metal scarcity, and has broad application prospects.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure HDA0004950208670000011
    Figure HDA0004950208670000011
  • Figure HDA0004950208670000021
    Figure HDA0004950208670000021
  • Figure HDA0004950208670000022
    Figure HDA0004950208670000022
Patent Text Reader

Abstract

The invention provides a nano-porous B-site high-entropy perovskite oxide electro-catalytic material as well as a preparation method and application of the nano-porous B-site high-entropy perovskite oxide electro-catalytic material. The preparation method of the nano-porous B-site high-entropy perovskite oxide electro-catalytic material comprises the following steps: mixing metal Al, Sr and La with B-site metal, and carrying out smelting and melt-spinning to obtain an alloy strip; the B-site metal is a mixture of any five metals of Fe, Co, Cr, Mn, Ni or Ru according to an equal molar ratio; and carrying out dealloying treatment on the alloy strip, and then carrying out annealing treatment to obtain the nano-porous B-site high-entropy perovskite oxide electro-catalytic material. The method is simple and easy to implement, high in practicability and easy to popularize. The nano-porous B-site high-entropy perovskite oxide electro-catalytic material prepared by the preparation method disclosed by the invention has excellent HER activity and relatively high overall water decomposition performance.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention belongs to the technical field of electrocatalytic materials, and in particular relates to a nanoporous B-site high entropy perovskite oxide electrocatalytic material and a preparation method and application thereof. Background Art

[0002] With the acceleration of industrialization, traditional energy sources that humans rely on for survival are becoming increasingly depleted. Hydrogen energy is expected to become one of the most promising future energy sources due to its advantages such as high calorific value, low pollution, wide sources and flexible conversion. At present, hydrogen energy is mainly produced through traditional fossil energy reforming, biomass cracking, industrial by-product gas, etc., but these methods still have problems such as greenhouse gas emissions, high energy consumption, and environmental pollution. Recently, water electrolysis using renewable energy as raw materials has attracted much attention from all walks of life due to its high product purity, pollution-free, and flexible production. The water electrolysis process consists of two half reactions, hydrogen evolution reaction (HER) and oxygen evolution reaction (OER). The slow kinetic process makes the actual decomposition pressure of water higher than the theoretical decomposition pressure. The appropriate use of catalysts in the water electrolysis process is one of the effective ways to reduce the reaction overpotential and increase the reaction rate. At present, the most widely used HER and OER catalysts are precious metal catalysts such as Pt / C and RuO2 / IrO2, respectively. However, their low inventory and high price limit their commercial application, so it is urgent to find alternative non-precious metal electrocatalysts.

[0003] In recent years, perovskite oxides have received extensive attention in various fields due to their advantages such as structural stability and element diversity. The chemical formula of perovskite oxides is ABO3, in which both A and B positions can be replaced by other elements while maintaining the crystal structure unchanged. In recent years, high-entropy materials have shown many excellent properties due to their thermodynamic high-entropy effect, kinetic slow diffusion effect, structural lattice distortion effect and performance cocktail effect. Due to the unique crystal structure stability of perovskite oxides, high-entropy perovskite oxides are possible. Studies have found that they exhibit many excellent properties that traditional materials cannot match, such as high strength, high hardness, corrosion resistance, high oxidation activity and excellent electromagnetic properties. On the other hand, the microscopic morphology also plays a very important role in the performance of the catalyst. The increase in active sites can significantly improve its electrocatalytic activity. Therefore, the development of nanoscale high-entropy perovskite oxides for electrocatalysis has important research significance.

[0004] Recently, there have been a few studies on the use of perovskite oxides or high entropy perovskite oxides in the field of electrocatalysis. For example, Chinese patent document CN109759077A discloses a perovskite oxide and its preparation method and application. In the perovskite oxide, A is selected from one of Sr, La, Ca, Na, K or Ba, and B is selected from two or more of Nb, Ti, Co, Mn, Fe, Ni, Al, Mo, Cu, Sc or Cr. The perovskite oxide of the invention can be prepared by traditional sol-gel method, solid phase method and other processes, and the method is simple, but the invention does not involve the preparation of high entropy perovskite oxide, and its electrocatalytic hydrogen evolution performance is not analyzed. Chinese patent document CN116177627A discloses a high-entropy perovskite oxide and its preparation method and application. It uses strontium carbonate, titanium oxide, zirconium oxide, hafnium oxide, tin oxide and ruthenium oxide as raw materials, and is prepared through processes such as high-speed ball milling, drying and roasting. The prepared Sr(Ti / Zr / Hf / Sn / Ru)O3 high-entropy perovskite oxide has abundant active sites and a stable structure, but its preparation method may have the problem of high energy consumption, and the patent is mainly used in the field of electrocatalytic nitrogen oxidation to prepare nitrate, and does not involve research on electrocatalytic hydrogen evolution performance.

[0005] Therefore, it is worth further exploring how to design a method to efficiently prepare nanoscale high-entropy perovskite oxides and apply them in the field of electrocatalysis. Summary of the invention

[0006] In view of the shortcomings of the prior art, the present invention proposes a nanoporous B-site high entropy perovskite oxide electrocatalytic material and a preparation method and application thereof. The method of the present invention is simple and easy to implement, highly practical, and easy to popularize. The nanoporous B-site high entropy perovskite oxide electrocatalytic material prepared by the present invention has excellent HER activity and high overall water decomposition performance.

[0007] Terminology Note:

[0008] Room temperature: 25℃±5℃.

[0009] To achieve the above object, the present invention adopts the following technical solution:

[0010] A nanoporous B-site high-entropy perovskite oxide electrocatalytic material, wherein the chemical formula of the high-entropy perovskite oxide electrocatalytic material is LaBO3, wherein the B-site elements are selected from any five elements of Fe, Co, Cr, Mn, Ni or Ru, and are composed in an equimolar ratio.

[0011] Preferably according to the present invention, the microstructure of the high entropy perovskite oxide electrocatalytic material is a nanoporous structure with a pore size between 8-200 nm.

[0012] The method for preparing the above-mentioned nanoporous B-site high entropy perovskite oxide electrocatalytic material comprises the steps of:

[0013] (1) mixing metals Al, Sr, La and B-site metals, smelting and spinning to obtain alloy strips; the B-site metals are any five metals selected from Fe, Co, Cr, Mn, Ni or Ru mixed in an equal molar ratio;

[0014] (2) The alloy strips are dealloyed and then annealed to obtain nanoporous B-site high entropy perovskite oxide electrocatalytic materials.

[0015] Preferably according to the present invention, in step (1), the atomic ratio of metals Al, Sr, La and B-site metal is 85-90:1-2:4-5:4-5, preferably 88:2:5:5.

[0016] Preferably, in step (1), smelting is carried out in a vacuum arc furnace; the smelting atmosphere is nitrogen or argon, the induced current during the smelting process is between 300 and 370 A, and the alloy is cooled to room temperature after smelting for 0.5 to 1 min; and the above smelting steps are repeated 4 to 7 times to obtain a uniform alloy ingot.

[0017] According to the preferred embodiment of the present invention, in step (1), the width of the alloy strip is 1-10 mm, the thickness is 10-100 μm, and the length is different. The strip spinning process can be carried out according to the existing method; preferably, the strip spinning is carried out in a vacuum strip spinning machine with a vacuum degree of 3×10 -3 -5×10 -3 Pa, the induced current of the belt spinning process is between 300 and 370A, the pressure difference between the quartz tube and the vacuum belt spinning machine furnace is 0.03-0.05MPa, preferably 0.05MPa, and the rotation speed of the copper roller is 2000-3500rpm, preferably 2865rpm. The specific steps are as follows: crush the alloy ingot obtained by smelting, and place a part of the crushed alloy ingot as the master alloy in the quartz tube of the vacuum belt spinning machine; adjust the vacuum degree of the vacuum belt spinning machine furnace to 3×10 -3 -5×10 -3 Pa, start the stepless speed regulating motor, when the speed of the copper roller reaches the set speed, turn on the power of the induction coil to melt it, melt the master alloy in the quartz tube to obtain the alloy melt; fill the quartz tube with high-purity argon gas instantly, so as to establish a preset pressure difference of 0.03-0.05MPa, preferably 0.05MPa, in the furnace chamber of the quartz tube and the vacuum belt spinning machine, under the action of the set pressure difference, the alloy melt is ejected from the quartz tube nozzle, sprayed onto the surface of the copper roller, and quickly cooled into an alloy strip. The preset speed of the copper roller is 2000-3500rpm, preferably 2865rpm.

[0018] Preferably according to the present invention, in step (1), the B-site metal is an equimolar mixture of Fe, Co, Mn, Ni, and Ru, an equimolar mixture of Fe, Co, Cr, Mn, and Ru, an equimolar mixture of Fe, Co, Cr, Ni, and Ru, an equimolar mixture of Fe, Cr, Mn, Ni, and Ru, an equimolar mixture of Co, Cr, Mn, Ni, and Ru, or an equimolar mixture of Fe, Co, Cr, Mn, Ni, and Ni; preferably, the B-site metal is an equimolar mixture of Fe, Co, Mn, Ni, and Ru.

[0019] Preferably, in step (2) of the present invention, the dealloying treatment is performed as follows: immersing the alloy strip in a NaOH aqueous solution, allowing it to stand at room temperature until no bubbles are generated, and then washing and drying to obtain a dealloyed alloy strip.

[0020] Preferably, the concentration of the NaOH aqueous solution is 2-5 mol / L; and the standing time is 10-15 h.

[0021] Preferably, the washing is performed using ultrapure water and anhydrous ethanol 5-6 times each.

[0022] Preferably, the drying is vacuum drying, the drying temperature is 40-80° C., and the drying time is 10-14 h.

[0023] Preferably, in step (2), the annealing treatment conditions are: in an air atmosphere, heating to 800-900°C at a heating rate of 3-5°C / min, keeping at 800-900°C for 2-4h, and then cooling to room temperature at a cooling rate of 3-5°C / min.

[0024] The above-mentioned nanoporous B-site high entropy perovskite oxide electrocatalytic material is applied to electrocatalytic hydrogen evolution reaction or electrocatalytic water decomposition.

[0025] Preferably according to the present invention, the anode for electrocatalytic water decomposition is an electrode made of nanoporous B-site high entropy perovskite oxide electrocatalytic material, and the cathode is an electrode made of RuO2; the electrolyte is a 0.5-5 mol / L KOH aqueous solution; the preparation method of the electrode comprises the steps of: mixing nanoporous B-site high entropy perovskite oxide electrocatalytic material or RuO2: acetylene black: PVDF = 6-10:1:1 in a mass ratio, then adding N-methylpyrrolidone (NMP), fully grinding and mixing to obtain a coating liquid; coating the coating liquid on the surface of a nickel sheet, drying, and pressing to obtain an anode or a cathode.

[0026] The technical features and beneficial effects of the present invention are as follows:

[0027] 1. The present invention provides a nanoporous B-site high entropy perovskite oxide electrocatalytic material, wherein the A-site is La, and the B-site is composed of any five elements of Fe, Co, Cr, Mn, Ni, and Ru in equal moles. The advantage of the preparation method is that the alloy design, dealloying and annealing methods are combined. First, smelting is performed to obtain an alloy ingot with uniform composition, and then the alloy strip is obtained after stripping. Then, the active metal elements are removed by dealloying, and finally annealing is performed to obtain a nanoporous B-site high entropy perovskite oxide electrocatalytic material. The preparation method of the present invention is simple and efficient, low in cost, safe and environmentally friendly, easy to operate, can be mass-produced, and has good application prospects.

[0028] 2. The LaBO3 electrocatalytic material prepared by the present invention is a high-entropy perovskite oxide material with a nanoporous structure. It has the advantages of small pores, uniform pore distribution, high specific surface area, and abundant active sites. It can effectively improve the electrocatalytic reaction rate and has good application prospects in electrocatalytic hydrogen evolution and overall water decomposition.

[0029] 3. The nanoporous LaBO3 high entropy perovskite oxide electrocatalytic material prepared by the present invention has excellent HER electrocatalytic activity and exhibits good performance in overall water decomposition, and can be applied to the current more urgent field of electrocatalytic water decomposition and hydrogen production. The nanoporous B-site high entropy perovskite oxide prepared by the present invention improves the electrocatalytic activity by adjusting the type of B-site elements, which can solve the problem of precious metal scarcity and has certain advantages and broad application prospects.

[0030] 4. The nanoporous LaBO3 high entropy perovskite oxide electrocatalytic material prepared by the present invention obtains a series of different high entropy perovskite oxides by regulating the types of B-site cations in the perovskite material, and systematically explores the effects of different element types on crystal structure, physicochemical properties and electrocatalytic performance. The type and quantity of B-site elements significantly affect the HER electrocatalytic performance. Among them, La(Fe 0.2 Co 0.2 Mn 0.2 Ni 0.2 Ru 0.2 )O3 has the best activity in electrocatalytic HER as well as overall water splitting. BRIEF DESCRIPTION OF THE DRAWINGS

[0031] Figure 1 X-ray diffraction patterns of the nanoporous B-site high entropy perovskite oxide electrocatalyst materials prepared in Examples 1-6 of the present invention and the low / medium entropy perovskite oxide electrocatalyst materials prepared in Comparative Examples 1 and 2.

[0032] Figure 2This is a scanning electron microscope photograph of the nanoporous B-site high entropy perovskite oxide electrocatalytic material prepared in Examples 1-6 of the present invention.

[0033] Figure 3 These are scanning electron microscope photographs of the low / medium entropy perovskite oxide electrocatalytic materials prepared in Comparative Examples 1 and 2 of the present invention.

[0034] Figure 4 HER polarization curves of the nanoporous B-site high entropy perovskite oxide electrocatalytic material prepared in Examples 1-6 of the present invention in a N2-saturated 1M KOH solution at a scanning rate of 10 mV / s.

[0035] Figure 5 This is a graph showing the overall water decomposition performance of the nanoporous B-site high entropy perovskite oxide electrocatalytic material prepared in Example 1 of the present invention.

[0036] Figure 6 This is a diagram of the specific surface area of ​​the nanoporous B-site high entropy perovskite oxide electrocatalytic material prepared in Examples 1-6 of the present invention. DETAILED DESCRIPTION

[0037] Hereinafter, the present invention will be described in detail. Before describing, it should be understood that the terms used in this specification and the appended claims should not be interpreted as being limited to the general meaning and dictionary meaning, but should be interpreted according to the meaning and concept corresponding to the technical aspects of the present invention on the basis of the principle that the inventor is allowed to appropriately define the terms for the best interpretation. Therefore, the descriptions presented here are only preferred examples for illustrative purposes and are not intended to limit the scope of the present invention, so that it should be understood that other equivalents or improvements can be obtained therefrom without departing from the spirit and scope of the present invention.

[0038] The following examples are only listed as examples of embodiments of the present invention and do not constitute any limitation to the present invention. It can be understood by those skilled in the art that modifications within the scope of the essence and concept of the present invention fall within the protection scope of the present invention. Unless otherwise specified, the reagents and instruments used in the following examples and comparative examples are commercially available products.

[0039] Example 1

[0040] A nanoporous La(Fe 0.2 Co 0.2 Mn 0.2 Ni 0.2 Ru 0.2 )O3 high entropy perovskite oxide electrocatalytic material is prepared by the following method:

[0041] (1) raw metals Al, Sr, La, Fe, Co, Mn, Ni, and Ru with a purity greater than 99.9% are mixed according to the following atomic ratio: 88:2:5:1:1:1:1:1;

[0042] (2) melting the above raw metal in a vacuum arc furnace;

[0043] The specific steps are as follows:

[0044] The prepared raw metals are placed in a graphite crucible, and the graphite crucible is then placed in a smelting pit of a vacuum arc furnace;

[0045] The air is exhausted by combining mechanical pump rough pumping and molecular pump fine pumping: First, the mechanical pump roughly pumps to make the vacuum degree reach 1×10 -1 Pa, high-purity argon gas was injected; the second rough pumping to 1×10 -1 Pa, inject high-purity argon gas; the third vacuum pumping to 1×10 -1 Pa, turn on the molecular pump to make the vacuum degree reach 4×10 -3 Pa, and high-purity argon gas is injected again;

[0046] Under the protection of high-purity argon, the induction coil current was adjusted to 350A, and the mixture was melted at this temperature for 0.5 min and then cooled to room temperature. The above melting steps were repeated 6 times to obtain an alloy ingot.

[0047] (3) placing the obtained alloy ingot in a vacuum belt spinning machine for belt spinning to obtain alloy strips;

[0048] The specific steps are as follows:

[0049] The alloy ingot is physically crushed, and the alloy ingot of suitable size is selected as the master alloy and placed in the quartz tube of the vacuum belt spinning machine (the nozzle is a small round hole with a diameter of 0.6-0.7 mm);

[0050] When the vacuum degree of the vacuum belt spinning machine chamber reaches 4×10 -3 After Pa, start the stepless speed regulating motor, and after the copper roller speed reaches 2865rpm (surface linear speed is about 30m / s), connect the induction coil power supply, and adjust the induction coil current to 320A to completely melt the master alloy in the quartz tube;

[0051] High-purity argon gas is immediately injected into the quartz tube, and the pressure difference (0.05MPa) between the quartz tube and the furnace is used to spray the molten liquid onto the surface of the high-speed rotating copper roller, causing it to cool rapidly to obtain an alloy strip with a width of about 2-4mm and a thickness of about 20-50μm.

[0052] (4) performing dealloying treatment on the alloy strip;

[0053] The specific steps are as follows:

[0054] Place the alloy strip in a 150 mL beaker, then pour in 120 mL of 2 M NaOH aqueous solution and let stand at 25 °C for 12 h. When no bubbles appear in the beaker, pour out the supernatant and wash with ultrapure water and anhydrous ethanol for 7 times each to remove impurities.

[0055] (5) vacuum drying the cleaned sample;

[0056] The specific steps are as follows:

[0057] The cleaned alloy was placed in a vacuum drying oven, the temperature was set to 60°C, and the air in the vacuum drying oven was evacuated with a vacuum pump. The drying time was 14 hours.

[0058] (6) The dried sample was placed in a muffle furnace for annealing to obtain nanoporous La(Fe 0.2 Co 0.2 Mn 0.2 Ni 0.2 Ru 0.2 )O3 high entropy perovskite oxide electrocatalytic materials.

[0059] The specific steps are as follows:

[0060] The dried sample was ground in a mortar and then fired in a porcelain boat in a muffle furnace. The temperature of the muffle furnace was set to rise from room temperature to 850°C at a heating rate of 3°C / min, kept at 850°C for 3h, and then cooled to room temperature at a cooling rate of 4°C / min. The annealing atmosphere was air. 0.2 Co 0.2 Mn 0.2 Ni 0.2 Ru 0.2 )O3 high entropy perovskite electrocatalytic materials.

[0061] After testing, the XRD pattern of the catalytic material prepared in this Example 1 is as follows: Figure 1 As shown in the figure, it is consistent with the lattice structure of perovskite oxide; the SEM results of the catalytic material prepared in this Example 1 are as follows Figure 2 As shown in a, the figure shows that it presents a nanoporous structure.

[0062] The performance test method of HER is:

[0063] The high entropy perovskite oxide electrocatalytic material prepared in Example 1 of the present invention was mixed with carbon powder XC-72 in a mass ratio of 5:2, and then 0.8 mL of Nafion dilution solution (Nafion dilution solution is prepared by mixing anhydrous ethanol with a volume fraction of 90% and Nafion solution with a volume fraction of 10%) and 1.2 mL of isopropanol solution were added, and ultrasonicated in an ultrasonicator for 30 minutes to obtain a mixed solution. A certain amount of the mixed solution was coated (coating amount was 15 μL) on a 5 mm glassy carbon electrode (electrode area was 0.196 cm 2 ), and dried in a vacuum dish for more than 3 hours to obtain a glassy carbon electrode.

[0064] A three-electrode system was used, with the sample-coated glassy carbon electrode as the working electrode, the graphite rod as the counter electrode, and the Hg / HgO electrode as the reference electrode. The electrolyte used was 1M KOH aqueous solution. High-purity N2 was introduced for 30 minutes before the test to saturate the electrolyte with N2, and the scanning speed was 10mV / s.

[0065] HER polarization curve is as follows Figure 4 As shown. Figure 4 It can be seen that the current density is -10mAcm -2 The hydrogen evolution overpotential under the condition of 51mV; the nanoporous La(Fe 0.2 Co 0.2 Mn 0.2 Ni 0.2 Ru 0.2 )O3 high entropy perovskite oxide electrocatalytic material has the best hydrogen evolution performance.

[0066] The specific surface area of ​​the catalytic material prepared in this example is as follows Figure 6 As shown in a, it reaches 17.4m 2 ·g -1 .

[0067] Example 2

[0068] A nanoporous La(Fe 0.2 Co 0.2 Cr 0.2 Mn 0.2 Ru 0.2 )O3 high entropy perovskite oxide electrocatalytic material is prepared by the following method:

[0069] (1) raw metals Al, Sr, La, Fe, Co, Cr, Mn, and Ru with a purity greater than 99.9% are mixed according to the following atomic ratio: 88:2:5:1:1:1:1:1;

[0070] (2) melting the above raw metal in a vacuum arc furnace;

[0071] The specific steps are as follows:

[0072] The prepared raw metals are placed in a graphite crucible, and the graphite crucible is then placed in a smelting pit of a vacuum arc furnace;

[0073] The air is exhausted by combining mechanical pump rough pumping and molecular pump fine pumping: First, the mechanical pump roughly pumps to make the vacuum degree reach 1×10 -1 Pa, high-purity argon gas was injected; the second rough pumping to 1×10 -1 Pa, inject high-purity argon gas; the third vacuum pumping to 1×10 -1 Pa, turn on the molecular pump to make the vacuum degree reach 4×10 -3 Pa, and high-purity argon gas is injected again;

[0074] Under the protection of high-purity argon, the induction coil current was adjusted to 350A, and the mixture was melted at this temperature for 0.5 min and then cooled to room temperature. The above melting steps were repeated 6 times to obtain an alloy ingot.

[0075] (3) placing the obtained alloy ingot in a vacuum belt spinning machine for belt spinning to obtain alloy strips;

[0076] The specific steps are as follows:

[0077] The alloy ingot is physically crushed, and the alloy ingot of suitable size is selected as the master alloy and placed in the quartz tube of the vacuum belt spinning machine (the nozzle is a small round hole with a diameter of 0.6-0.7 mm);

[0078] When the vacuum degree of the vacuum belt spinning machine chamber reaches 4×10 -3 After Pa, start the stepless speed regulating motor, and after the copper roller speed reaches 2865rpm (surface linear speed is about 30m / s), turn on the induction coil current and adjust the induction coil current to 320A to completely melt the master alloy in the quartz tube;

[0079] High-purity argon gas is immediately injected into the quartz tube, and the pressure difference (0.05MPa) between the quartz tube and the furnace is used to spray the molten liquid onto the surface of the high-speed rotating copper roller, causing it to cool rapidly to obtain an alloy strip with a width of about 2-4mm and a thickness of about 20-50μm.

[0080] (4) performing dealloying treatment on the alloy strip;

[0081] The specific steps are as follows:

[0082] Place the alloy strip in a 150 mL beaker, then pour in 120 mL of 2 M NaOH aqueous solution and let stand at 25 °C for 12 h. When no bubbles appear in the beaker, pour out the supernatant and wash with ultrapure water and anhydrous ethanol for 7 times each to remove impurities.

[0083] (5) vacuum drying the cleaned sample;

[0084] The specific steps are as follows:

[0085] The cleaned alloy was placed in a vacuum drying oven, the temperature was set to 60°C, and the air in the vacuum drying oven was evacuated with a vacuum pump. The drying time was 14 hours.

[0086] (6) The dried sample was placed in a muffle furnace for annealing to obtain nanoporous La(Fe 0.2 Co 0.2 Cr 0.2 Mn 0.2 Ru 0.2 )O3 high entropy perovskite oxide electrocatalytic materials.

[0087] The specific steps are as follows:

[0088] The dried sample was ground in a mortar and then fired in a porcelain boat in a muffle furnace. The temperature of the muffle furnace was set to rise from room temperature to 850°C at a heating rate of 3°C / min, kept at 850°C for 3h, and then cooled to room temperature at a cooling rate of 4°C / min. The annealing atmosphere was air. 0.2 Co 0.2 Cr 0.2 Mn 0.2 Ru 0.2 )O3 high entropy perovskite electrocatalytic materials.

[0089] After testing, the XRD spectrum of the catalytic material prepared in this Example 2 is as follows: Figure 1 As shown in the figure, it is consistent with the lattice structure of perovskite oxide; the SEM results of the catalytic material prepared in Example 2 are as follows Figure 2 As shown in b, the figure shows that it presents a uniformly distributed nanoporous structure.

[0090] The HER performance of the catalytic material was tested according to the method of Example 1. The HER polarization curve is shown in Figure 4 As shown. The current density is -10mA cm -2 The overpotential for hydrogen evolution is 75 mV.

[0091] The specific surface area of ​​the catalytic material prepared in this example is as follows Figure 6 As shown in b, it reaches 15.5m 2 ·g -1 .

[0092] Example 3

[0093] A nanoporous La(Fe 0.2 Co 0.2 Cr0.2 Ni 0.2 Ru 0.2 )O3 high entropy perovskite oxide electrocatalytic material is prepared by the following method:

[0094] (1) raw metals Al, Sr, La, Fe, Co, Cr, Ni, and Ru with a purity greater than 99.9% are mixed according to the following atomic ratio: 88:2:5:1:1:1:1:1;

[0095] (2) melting the above raw metal in a vacuum arc furnace;

[0096] The specific steps are as follows:

[0097] The prepared raw metals are placed in a graphite crucible, and the graphite crucible is then placed in a smelting pit of a vacuum arc furnace;

[0098] The air is exhausted by combining mechanical pump rough pumping and molecular pump fine pumping: First, the mechanical pump roughly pumps to make the vacuum degree reach 1×10 -1 Pa, high-purity argon gas was injected; the second rough pumping to 1×10 -1 Pa, inject high-purity argon gas; the third vacuum pumping to 1×10 -1 Pa, turn on the molecular pump to make the vacuum degree reach 4×10 -3 Pa, and high-purity argon gas is injected again;

[0099] Under the protection of high-purity argon, the induction coil current was adjusted to 350A, and the mixture was melted at this temperature for 0.5 min and then cooled to room temperature. The above melting steps were repeated 6 times to obtain an alloy ingot.

[0100] (3) placing the obtained alloy ingot in a vacuum belt spinning machine for belt spinning to obtain alloy strips;

[0101] The specific steps are as follows:

[0102] The alloy ingot is physically crushed, and the alloy ingot of suitable size is selected as the master alloy and placed in the quartz tube of the vacuum belt spinning machine (the nozzle is a small round hole with a diameter of 0.6-0.7 mm);

[0103] When the vacuum degree of the vacuum belt spinning machine chamber reaches 4×10 -3 After Pa, start the stepless speed regulating motor, and after the copper roller speed reaches 2865rpm (surface linear speed is about 30m / s), connect the induction coil, and adjust the induction coil current to 320A to completely melt the master alloy in the quartz tube;

[0104] High-purity argon gas is immediately injected into the quartz tube, and the pressure difference (0.05MPa) between the quartz tube and the furnace is used to spray the molten liquid onto the surface of the high-speed rotating copper roller, causing it to cool rapidly to obtain an alloy strip with a width of about 2-4mm and a thickness of about 20-50μm.

[0105] (4) performing dealloying treatment on the alloy strip;

[0106] The specific steps are as follows:

[0107] Place the alloy strip in a 150 mL beaker, then pour in 120 mL of 2 M NaOH aqueous solution and let stand at 25 °C for 12 h. When no bubbles appear in the beaker, pour out the supernatant and wash with ultrapure water and anhydrous ethanol for 7 times each to remove impurities.

[0108] (5) vacuum drying the cleaned sample;

[0109] The specific steps are as follows:

[0110] The cleaned alloy was placed in a vacuum drying oven, the temperature was set to 60°C, and the air in the vacuum drying oven was evacuated with a vacuum pump. The drying time was 14 hours.

[0111] (6) The dried sample was placed in a muffle furnace for annealing to obtain nanoporous La(Fe 0.2 Co 0.2 Cr 0.2 Ni 0.2 Ru 0.2 )O3 high entropy perovskite oxide electrocatalytic materials.

[0112] The specific steps are as follows:

[0113] The dried sample was ground in a mortar and then fired in a porcelain boat in a muffle furnace. The temperature of the muffle furnace was set to rise from room temperature to 850°C at a heating rate of 3°C / min, kept at 850°C for 3h, and then cooled to room temperature at a cooling rate of 4°C / min. The annealing atmosphere was air. 0.2 Co 0.2 Cr 0.2 Ni 0.2 Ru 0.2 )O3 high entropy perovskite electrocatalytic materials.

[0114] After testing, the XRD pattern of the catalytic material prepared in Example 3 is as follows: Figure 1 As shown in the figure, it is consistent with the lattice structure of perovskite oxide; the SEM results of the catalytic material prepared in Example 3 are as follows Figure 2 As shown in c, the figure shows that it presents a uniformly distributed nanoporous structure.

[0115] The HER performance of the catalytic material was tested according to the method of Example 1. The HER polarization curve is shown in Figure 4 As shown. The current density is -10mAcm -2 The overpotential for hydrogen evolution is 84 mV.

[0116] The specific surface area of ​​the catalytic material prepared in this example is as follows Figure 6 As shown in c, it reached 12.9m 2 ·g -1 .

[0117] Example 4

[0118] A nanoporous La(Fe 0.2 Cr 0.2 Mn 0.2 Ni 0.2 Ru 0.2 )O3 high entropy perovskite oxide electrocatalytic material is prepared by the following method:

[0119] (1) raw metals Al, Sr, La, Fe, Cr, Mn, Ni, and Ru with a purity greater than 99.9% are mixed according to the following atomic ratio: 88:2:5:1:1:1:1:1;

[0120] (2) melting the above raw metal in a vacuum arc furnace;

[0121] The specific steps are as follows:

[0122] The prepared raw metals are placed in a graphite crucible, and the graphite crucible is then placed in a smelting pit of a vacuum arc furnace;

[0123] The air is exhausted by combining mechanical pump rough pumping and molecular pump fine pumping: First, the mechanical pump roughly pumps to make the vacuum degree reach 1×10 -1 Pa, high-purity argon gas was injected; the second rough pumping to 1×10 -1 Pa, inject high-purity argon gas; the third vacuum pumping to 1×10 -1 Pa, turn on the molecular pump to make the vacuum degree reach 4×10 -3 Pa, and high-purity argon gas is injected again;

[0124] Under the protection of high-purity argon, the induction coil current was adjusted to 350A, and the mixture was melted at this temperature for 0.5 min and then cooled to room temperature. The above melting steps were repeated 6 times to obtain an alloy ingot.

[0125] (3) placing the obtained alloy ingot in a vacuum belt spinning machine for belt spinning to obtain alloy strips;

[0126] The specific steps are as follows:

[0127] The alloy ingot is physically crushed, and the alloy ingot of suitable size is selected as the master alloy and placed in the quartz tube of the vacuum belt spinning machine (the nozzle is a small round hole with a diameter of 0.6-0.7 mm);

[0128] When the vacuum degree of the vacuum belt spinning machine chamber reaches 4×10 -3 After Pa, start the stepless speed regulating motor, and after the copper roller speed reaches 2865rpm (surface linear speed is about 30m / s), connect the induction coil power supply, and adjust the induction coil current to 320A to completely melt the master alloy in the quartz tube;

[0129] High-purity argon gas is immediately injected into the quartz tube, and the pressure difference (0.05MPa) between the quartz tube and the furnace is used to spray the molten liquid onto the surface of the high-speed rotating copper roller, causing it to cool rapidly to obtain an alloy strip with a width of about 2-4mm and a thickness of about 20-50μm.

[0130] (4) performing dealloying treatment on the alloy strip;

[0131] The specific steps are as follows:

[0132] Place the alloy strip in a 150 mL beaker, then pour in 120 mL of 2 M NaOH aqueous solution and let stand at 25 °C for 12 h. When no bubbles appear in the beaker, pour out the supernatant and wash with ultrapure water and anhydrous ethanol for 7 times each to remove impurities.

[0133] (5) vacuum drying the cleaned sample;

[0134] The specific steps are as follows:

[0135] The cleaned alloy was placed in a vacuum drying oven, the temperature was set to 60°C, and the air in the vacuum drying oven was evacuated with a vacuum pump. The drying time was 14 hours.

[0136] (6) The dried sample was placed in a muffle furnace for annealing to obtain nanoporous La(Fe 0.2 Cr 0.2 Mn 0.2 Ni 0.2 Ru 0.2 )O3 high entropy perovskite oxide electrocatalytic materials.

[0137] The specific steps are as follows:

[0138] The dried sample was ground in a mortar and then fired in a porcelain boat in a muffle furnace. The temperature of the muffle furnace was set to rise from room temperature to 850°C at a heating rate of 3°C / min, kept at 850°C for 3h, and then cooled to room temperature at a cooling rate of 4°C / min. The annealing atmosphere was air. 0.2 Cr0.2 Mn 0.2 Ni 0.2 Ru 0.2 )O3 high entropy perovskite electrocatalytic materials.

[0139] After testing, the XRD pattern of the catalytic material prepared in this Example 4 is as follows: Figure 1 As shown in the figure, it is consistent with the lattice structure of perovskite oxide; the SEM results of the catalytic material prepared in Example 4 are as follows Figure 2 As shown in d, the figure shows that it presents a uniformly distributed nanoporous structure.

[0140] The HER performance of the catalytic material was tested according to the method of Example 1. The HER polarization curve is shown in Figure 4 As shown. The current density is -10mA cm -2 The overpotential for hydrogen evolution is 126 mV.

[0141] The specific surface area of ​​the catalytic material prepared in this example is as follows Figure 6 As shown in d, it reaches 12.5m 2 ·g -1 .

[0142] Example 5

[0143] A nanoporous La(Co 0.2 Cr 0.2 Mn 0.2 Ni 0.2 Ru 0.2 )O3 high entropy perovskite oxide electrocatalytic material is prepared by the following method:

[0144] (1) raw metals Al, Sr, La, Co, Cr, Mn, Ni, and Ru with a purity greater than 99.9% are mixed according to the following atomic ratio: 88:2:5:1:1:1:1:1;

[0145] (2) melting the above raw metal in a vacuum arc furnace;

[0146] The specific steps are as follows:

[0147] The prepared raw metals are placed in a graphite crucible, and the graphite crucible is then placed in a smelting pit of a vacuum arc furnace;

[0148] The air is exhausted by combining mechanical pump rough pumping and molecular pump fine pumping: First, the mechanical pump roughly pumps to make the vacuum degree reach 1×10 -1 Pa, high-purity argon gas was injected; the second rough pumping to 1×10 -1 Pa, inject high-purity argon gas; the third vacuum pumping to 1×10 -1 Pa, turn on the molecular pump to make the vacuum degree reach 4×10-3 Pa, and high-purity argon gas is injected again;

[0149] Under the protection of high-purity argon, the induction coil current was adjusted to 350A, and the mixture was melted at this temperature for 0.5 min and then cooled to room temperature. The above melting steps were repeated 6 times to obtain an alloy ingot.

[0150] (3) placing the obtained alloy ingot in a vacuum belt spinning machine for belt spinning to obtain alloy strips;

[0151] The specific steps are as follows:

[0152] The alloy ingot is physically crushed, and the alloy ingot of suitable size is selected as the master alloy and placed in the quartz tube of the vacuum belt spinning machine (the nozzle is a small round hole with a diameter of 0.6-0.7 mm);

[0153] When the vacuum degree of the vacuum belt spinning machine chamber reaches 4×10 -3 After Pa, start the stepless speed regulating motor, and after the copper roller speed reaches 2865rpm (surface linear speed is about 30m / s), connect the induction coil power supply, and adjust the induction coil current to 320A to completely melt the master alloy in the quartz tube;

[0154] High-purity argon gas is immediately injected into the quartz tube, and the pressure difference (0.05MPa) between the quartz tube and the furnace is used to spray the molten liquid onto the surface of the high-speed rotating copper roller, causing it to cool rapidly to obtain an alloy strip with a width of about 2-4mm and a thickness of about 20-50μm.

[0155] (4) performing dealloying treatment on the alloy strip;

[0156] The specific steps are as follows:

[0157] Place the alloy strip in a 150 mL beaker, then pour in 120 mL of 2 M NaOH aqueous solution and let stand at 25 °C for 12 h. When no bubbles appear in the beaker, pour out the supernatant and wash with ultrapure water and anhydrous ethanol for 7 times each to remove impurities.

[0158] (5) vacuum drying the cleaned sample;

[0159] The specific steps are as follows:

[0160] The cleaned alloy was placed in a vacuum drying oven, the temperature was set to 60°C, and the air in the vacuum drying oven was evacuated with a vacuum pump. The drying time was 14 hours.

[0161] (6) The dried sample was placed in a muffle furnace for annealing to obtain nanoporous La(Co 0.2 Cr 0.2 Mn 0.2 Ni 0.2 Ru0.2 )O3 high entropy perovskite oxide electrocatalytic materials.

[0162] The specific steps are as follows:

[0163] The dried sample was ground in a mortar and then fired in a porcelain boat in a muffle furnace. The temperature of the muffle furnace was set to rise from room temperature to 850°C at a heating rate of 3°C / min, kept at 850°C for 3h, and then cooled to room temperature at a cooling rate of 4°C / min. The annealing atmosphere was air. 0.2 Cr 0.2 Mn 0.2 Ni 0.2 Ru 0.2 )O3 high entropy perovskite electrocatalytic materials.

[0164] After testing, the XRD pattern of the catalytic material prepared in this Example 5 is as follows: Figure 1 As shown in the figure, it is consistent with the lattice structure of perovskite oxide; the SEM results of the catalytic material prepared in Example 5 are as follows Figure 2 As shown in e, the figure shows that it presents a uniformly distributed nanoporous structure.

[0165] The HER performance of the catalytic material was tested according to the method of Example 1. The HER polarization curve is shown in Figure 4 As shown. The current density is -10mA cm -2 The overpotential for hydrogen evolution is 123 mV.

[0166] The specific surface area of ​​the catalytic material prepared in this example is as follows Figure 6 As shown in e, it reaches 11.6m 2 ·g -1 .

[0167] Example 6

[0168] A nanoporous La(Fe 0.2 Co 0.2 Cr 0.2 Mn 0.2 Ni 0.2 )O3 high entropy perovskite oxide electrocatalytic material is prepared by the following method:

[0169] (1) raw metal elements Al, Sr, La, Fe, Co, Cr, Mn, and Ni with a purity greater than 99.9% are mixed according to the following atomic ratio: 88:2:5:1:1:1:1:1;

[0170] (2) melting the above raw metal in a vacuum arc furnace;

[0171] The specific steps are as follows:

[0172] The prepared raw metals are placed in a graphite crucible, and the graphite crucible is then placed in a smelting pit of a vacuum arc furnace;

[0173] The air is exhausted by combining mechanical pump rough pumping and molecular pump fine pumping: First, the mechanical pump roughly pumps to make the vacuum degree reach 1×10 -1 Pa, high-purity argon gas was injected; the second rough pumping to 1×10 -1 Pa, inject high-purity argon gas; the third vacuum pumping to 1×10 -1 Pa, turn on the molecular pump to make the vacuum degree reach 4×10 -3 Pa, and high-purity argon gas is injected again;

[0174] Under the protection of high-purity argon, the induction coil current was adjusted to 350A, and the mixture was melted at this temperature for 0.5 min and then cooled to room temperature. The above melting steps were repeated 6 times to obtain an alloy ingot.

[0175] (3) placing the obtained alloy ingot in a vacuum belt spinning machine for belt spinning to obtain alloy strips;

[0176] The specific steps are as follows:

[0177] The alloy ingot is physically crushed, and the alloy ingot of suitable size is selected as the master alloy and placed in the quartz tube of the vacuum belt spinning machine (the nozzle is a small round hole with a diameter of 0.6-0.7 mm);

[0178] When the vacuum degree of the vacuum belt spinning machine chamber reaches 4×10 -3 After Pa, start the stepless speed regulating motor, and after the copper roller speed reaches 2865rpm (surface linear speed is about 30m / s), connect the induction coil power supply, and adjust the induction coil current to 320A to completely melt the master alloy in the quartz tube;

[0179] High-purity argon gas is immediately injected into the quartz tube, and the pressure difference (0.05MPa) between the quartz tube and the furnace is used to spray the molten liquid onto the surface of the high-speed rotating copper roller, causing it to cool rapidly to obtain an alloy strip with a width of about 2-4mm and a thickness of about 20-50μm.

[0180] (4) performing dealloying treatment on the alloy strip;

[0181] The specific steps are as follows:

[0182] Place the alloy strip in a 150 mL beaker, then pour in 120 mL of 2 M NaOH aqueous solution and let stand at 25 °C for 12 h. When no bubbles appear in the beaker, pour out the supernatant and wash with ultrapure water and anhydrous ethanol for 7 times each to remove impurities.

[0183] (5) vacuum drying the cleaned sample;

[0184] The specific steps are as follows:

[0185] The cleaned alloy was placed in a vacuum drying oven, the temperature was set to 60°C, and the air in the vacuum drying oven was evacuated with a vacuum pump. The drying time was 14 hours.

[0186] (6) The dried sample was placed in a muffle furnace for annealing to obtain nanoporous La(Fe 0.2 Co 0.2 Cr 0.2 Mn 0.2 Ni 0.2 )O3 high entropy perovskite oxide electrocatalytic materials.

[0187] The specific steps are as follows:

[0188] The dried sample was ground in a mortar and then fired in a porcelain boat in a muffle furnace. The temperature of the muffle furnace was set to rise from room temperature to 850°C at a heating rate of 3°C / min, kept at 850°C for 3h, and then cooled to room temperature at a cooling rate of 4°C / min. The annealing atmosphere was air. 0.2 Co 0.2 Cr 0.2 Mn 0.2 Ni 0.2 )O3 high entropy perovskite electrocatalytic materials.

[0189] After testing, the XRD spectrum of the catalytic material prepared in this Example 6 is as follows: Figure 1 As shown in the figure, it is consistent with the lattice structure of perovskite oxide; the SEM results of the catalytic material prepared in Example 6 are as follows Figure 2 As shown in f, the figure shows that it presents a uniformly distributed nanoporous structure.

[0190] The HER performance of the catalytic material was tested according to the method of Example 1. The HER polarization curve is shown in Figure 4 As shown. The current density is -10mA cm -2 The hydrogen evolution overpotential is 466 mV.

[0191] The specific surface area of ​​the catalytic material prepared in this example is as follows Figure 6 As shown in f, it reaches 14.4m 2 ·g -1 .

[0192] Comparative Example 1

[0193] A LaFe 1 / 3 Co 1 / 3 Ni 1 / 3 O3 low entropy perovskite oxide electrocatalytic material is prepared by the following method:

[0194] (1) Al, Sr, La, Fe, Co, and Ni, the original metals with a purity greater than 99.9%, are mixed according to the following atomic ratio: 88:2:5:1.667:1.667:1.667;

[0195] (2) melting the above raw metal in a vacuum arc furnace;

[0196] The specific steps are as follows:

[0197] The prepared raw metals are placed in a graphite crucible, and the graphite crucible is then placed in a smelting pit of a vacuum arc furnace;

[0198] The air is exhausted by combining mechanical pump rough pumping and molecular pump fine pumping: First, the mechanical pump roughly pumps to make the vacuum degree reach 1×10 -1 Pa, high-purity argon gas was injected; the second rough pumping to 1×10 -1 Pa, inject high-purity argon gas; the third vacuum pumping to 1×10 -1 Pa, turn on the molecular pump to make the vacuum degree reach 4×10 -3 Pa, and high-purity argon gas is injected again;

[0199] Under the protection of high-purity argon, the induction coil current was adjusted to 350A, and the mixture was melted at this temperature for 0.5 min and then cooled to room temperature. The above melting steps were repeated 6 times to obtain an alloy ingot.

[0200] (3) placing the obtained alloy ingot in a vacuum belt spinning machine for belt spinning to obtain alloy strips;

[0201] The specific steps are as follows:

[0202] The alloy ingot is physically crushed, and the alloy ingot of suitable size is selected as the master alloy and placed in the quartz tube of the vacuum belt spinning machine (the nozzle is a small round hole with a diameter of 0.6-0.7 mm);

[0203] When the vacuum degree of the vacuum belt spinning machine chamber reaches 4×10 -3 After Pa, start the stepless speed regulating motor, and after the copper roller speed reaches 2865rpm (surface linear speed is about 30m / s), connect the induction coil power supply, and adjust the induction coil current to 320A to completely melt the master alloy in the quartz tube;

[0204] High-purity argon gas is immediately injected into the quartz tube, and the pressure difference (0.05MPa) between the quartz tube and the furnace is used to spray the molten liquid onto the surface of the high-speed rotating copper roller, causing it to cool rapidly to obtain an alloy strip with a width of about 2-4mm and a thickness of about 20-50μm.

[0205] (4) performing dealloying treatment on the alloy strip;

[0206] The specific steps are as follows:

[0207] Place the alloy strip in a 150 mL beaker, then pour in 120 mL of 2 M NaOH aqueous solution and let stand at 25 °C for 12 h. When no bubbles appear in the beaker, pour out the supernatant and wash with ultrapure water and anhydrous ethanol for 7 times each to remove impurities.

[0208] (5) vacuum drying the cleaned sample;

[0209] The specific steps are as follows:

[0210] The cleaned alloy was placed in a vacuum drying oven, the temperature was set to 60°C, and the air in the vacuum drying oven was evacuated with a vacuum pump. The drying time was 14 hours.

[0211] (6) The dried sample was placed in a muffle furnace for annealing to obtain nanoporous LaFe 1 / 3 Co 1 / 3 Ni 1 / 3 O3 low entropy perovskite oxide electrocatalytic materials.

[0212] The specific steps are as follows:

[0213] The dried sample was ground with a mortar and then placed in a porcelain boat in a muffle furnace for firing. The temperature of the muffle furnace was set to rise from room temperature to 850°C at a heating rate of 3°C / min, kept at 850°C for 3h, and then cooled to room temperature at a cooling rate of 4°C / min. The annealing atmosphere was air. 1 / 3 Co 1 / 3 Ni 1 / 3 O3 low entropy perovskite oxide electrocatalytic materials.

[0214] After testing, the XRD spectrum of the catalytic material prepared in this comparative example 1 is as follows Figure 1 As shown in the figure, the lattice structure is consistent with that of perovskite oxide; the LaFe prepared in this comparative example 1 1 / 3 Co 1 / 3 Ni 1 / 3 The SEM results of O3 low entropy perovskite oxide electrocatalyst materials are shown in Figure 3 As shown in a, the figure shows that it presents a nanoporous structure.

[0215] The HER performance of the catalytic material was tested according to the method of Example 1. The HER polarization curve is shown in Figure 4 As shown. The current density is -10mA cm -2 The overpotential for hydrogen evolution is 340 mV.

[0216] Comparative Example 2

[0217] A LaFe 1.25 Co 1.25 Mn 1.25 Ni 1.25 The O3 medium entropy perovskite oxide electrocatalytic material is prepared by the following method:

[0218] (1) raw metals Al, Sr, La, Fe, Co, Mn, and Ni with a purity greater than 99.9% are mixed according to the following atomic ratio: 88:2:5:1.25:1.25:1.25:1.25;

[0219] (2) melting the above raw metal in a vacuum arc furnace;

[0220] The specific steps are as follows:

[0221] The prepared raw metals are placed in a graphite crucible, and the graphite crucible is then placed in a smelting pit of a vacuum arc furnace;

[0222] The air is exhausted by combining mechanical pump rough pumping and molecular pump fine pumping: First, the mechanical pump roughly pumps to make the vacuum degree reach 1×10 -1 Pa, high-purity argon gas was injected; the second rough pumping to 1×10 -1 Pa, inject high-purity argon gas; the third vacuum pumping to 1×10 -1 Pa, turn on the molecular pump to make the vacuum degree reach 4×10 -3 Pa, and high-purity argon gas is injected again;

[0223] Under the protection of high-purity argon, the induction coil current was adjusted to 350A, and the mixture was melted for 0.5 min under this condition and then cooled to room temperature. The above melting steps were repeated 6 times to obtain an alloy ingot.

[0224] (3) placing the obtained alloy ingot in a vacuum belt spinning machine for belt spinning to obtain alloy strips;

[0225] The specific steps are as follows:

[0226] The alloy ingot is physically crushed, and the alloy ingot of suitable size is selected as the master alloy and placed in the quartz tube of the vacuum belt spinning machine (the nozzle is a small round hole with a diameter of 0.6-0.7 mm);

[0227] When the vacuum degree of the vacuum belt spinning machine chamber reaches 4×10 -3 After Pa, start the stepless speed regulating motor, and after the copper roller speed reaches 2865rpm (surface linear speed is about 30m / s), connect the induction coil power supply, and adjust the induction coil current to 320A to completely melt the master alloy in the quartz tube;

[0228] High-purity argon gas is immediately injected into the quartz tube, and the pressure difference (0.05MPa) between the quartz tube and the furnace is used to spray the molten liquid onto the surface of the high-speed rotating copper roller, causing it to cool rapidly to obtain an alloy strip with a width of about 2-4mm and a thickness of about 20-50μm.

[0229] (4) performing dealloying treatment on the alloy strip;

[0230] The specific steps are as follows:

[0231] Place the alloy strip in a 150 mL beaker, then pour in 120 mL of 2 M NaOH aqueous solution and let stand at 25 °C for 12 h. When no bubbles appear in the beaker, pour out the supernatant and wash with ultrapure water and anhydrous ethanol for 7 times each to remove impurities.

[0232] (5) vacuum drying the cleaned sample;

[0233] The specific steps are as follows:

[0234] The cleaned alloy was placed in a vacuum drying oven, the temperature was set to 60°C, and the air in the vacuum drying oven was evacuated with a vacuum pump. The drying time was 14 hours.

[0235] (6) The dried sample was placed in a muffle furnace for annealing to obtain nanoporous LaFe 1.25 Co 1.25 Mn 1.25 Ni 1.25 O3 medium-entropy perovskite oxide electrocatalytic materials.

[0236] The specific steps are as follows:

[0237] The dried sample was ground in a mortar and then fired in a porcelain boat in a muffle furnace. The temperature of the muffle furnace was set to rise from room temperature to 850°C at a heating rate of 3°C / min, kept at 850°C for 3h, and then cooled to room temperature at a cooling rate of 4°C / min. The annealing atmosphere was air. 1.25 Co 1.25 Mn 1.25 Ni 1.25 O3 medium-entropy perovskite oxide electrocatalytic materials.

[0238] After testing, the XRD spectrum of the catalytic material prepared in this comparative example 2 is as follows Figure 1 As shown in the figure, the lattice structure is consistent with that of perovskite oxide; the LaFe prepared in this comparative example 2 1.25 Co 1.25 Mn 1.25 Ni 1.25 SEM results of O3 entropy perovskite oxide electrocatalyst materials Figure 3 As shown in b, the figure shows that it presents a nanoporous structure.

[0239] The HER performance of the catalytic material was tested according to the method of Example 1. The HER polarization curve is shown in Figure 4 As shown. The current density is -10mAcm -2 The overpotential for hydrogen evolution is 401 mV.

[0240] Application Example 1

[0241] The overall water splitting performance test method is: using a two-electrode system, the anode is an electrode made of the high entropy perovskite oxide electrocatalytic material prepared in Example 1, and the cathode is an electrode made of RuO2. The electrolyte used is: 1M KOH aqueous solution. The scanning speed is 0.05V s -1 , the voltage range is 1~2V.

[0242] Electrode preparation method: The high entropy perovskite oxide electrocatalytic material prepared in Example 1 or RuO2: acetylene black: PVDF = 8:1:1 mass ratio is mixed evenly, and then 3-4 drops of N-methylpyrrolidone (NMP) are dripped in and fully ground. A 1*2cm nickel sheet is folded into two 1*1cm parts with tweezers, and the evenly ground sample is coated on one of the 1*1cm parts, and then placed in a vacuum drying oven at 60°C for drying. The dried nickel sheet is flattened with a tablet press to obtain an anode or cathode.

[0243] Figure 5 The nanoporous La(Fe 0.2 Co 0.2 Mn 0.2 Ni 0.2 Ru 0.2 )O3 high entropy perovskite oxide electrocatalyst in 1M KOH aqueous solution at a scan rate of 0.05V s -1 , the overall water splitting performance curve with a voltage range of 1 to 2V.

[0244] Depend on Figure 5 It can be seen that the nanoporous La(Fe 0.2 Co 0.2 Mn 0.2 Ni 0.2 Ru 0.2 )O3 high entropy perovskite oxide electrocatalytic material has excellent overall water decomposition performance. As can be seen from the figure, by applying a voltage of 1.61vs.RHE between the two electrodes, 10mAcm -2 The current density is comparable to the voltage required for commercial Pt / C‖RuO2 (1.61vs.RHE). 0.2 Co0.2 Mn 0.2 Ni 0.2 Ru 0.2 )O3‖RuO2 electrolyzer is a material with superior performance in alkaline solution.

Claims

1. A nanoporous B-site high entropy perovskite oxide electrocatalytic material, It is characterized in that The chemical formula of the high entropy perovskite oxide electrocatalytic material is LaBO 3 , wherein the B-site elements are selected from any five elements of Fe, Co, Cr, Mn, Ni or Ru, and are composed in an equimolar ratio.

2. The nanoporous B-site high entropy perovskite oxide electrocatalytic material according to claim 1, It is characterized in that The microstructure of the high entropy perovskite oxide electrocatalytic material is a nanoporous structure with a pore size between 8 and 200 nm.

3. The method for preparing the nanoporous B-site high entropy perovskite oxide electrocatalytic material according to claim 1 or 2, comprising the steps of: (1) mixing metals Al, Sr, La and B-site metals, smelting and spinning to obtain alloy strips; the B-site metals are any five metals selected from Fe, Co, Cr, Mn, Ni or Ru mixed in an equal molar ratio; (2) The alloy strips are dealloyed and then annealed to obtain nanoporous B-site high entropy perovskite oxide electrocatalytic materials.

4. The method for preparing the nanoporous B-site high entropy perovskite oxide electrocatalytic material according to claim 3, It is characterized in that In step (1), the atomic ratio of metal Al, Sr, La and B-site metal is 85-90:1-2:4-5:4-5, preferably 88:2:5:

5.

5. The method for preparing the nanoporous B-site high entropy perovskite oxide electrocatalytic material according to claim 3, It is characterized in that In step (1), smelting is carried out in a vacuum arc furnace; the smelting atmosphere is nitrogen or argon, the induced current during the smelting process is between 300 and 370A, and the smelting is carried out for 0.5-1min before cooling to room temperature; then the above smelting steps are repeated 4-7 times to obtain a uniform alloy ingot.

6. The method for preparing the nanoporous B-site high entropy perovskite oxide electrocatalytic material according to claim 3, It is characterized in that In step (1), the B-site metal is an equimolar mixture of Fe, Co, Mn, Ni, and Ru, an equimolar mixture of Fe, Co, Cr, Mn, and Ru, an equimolar mixture of Fe, Co, Cr, Ni, and Ru, an equimolar mixture of Fe, Cr, Mn, Ni, and Ru, an equimolar mixture of Co, Cr, Mn, Ni, and Ru, or an equimolar mixture of Fe, Co, Cr, Mn, and Ni; preferably, the B-site metal is an equimolar mixture of Fe, Co, Mn, Ni, and Ru.

7. The method for preparing the nanoporous B-site high entropy perovskite oxide electrocatalytic material according to claim 3, It is characterized in that In step (2), the dealloying treatment is performed as follows: immersing the alloy strip in a NaOH aqueous solution, leaving it to stand at room temperature until no bubbles are generated, and then washing and drying to obtain a dealloyed alloy strip.

8. The method for preparing the nanoporous B-site high entropy perovskite oxide electrocatalytic material according to claim 7, It is characterized in that Includes one or more of the following conditions: i. The concentration of NaOH aqueous solution is 2-5 mol / L; the standing time is 10-15h; ii. Washing is done by using ultrapure water and anhydrous ethanol 5-6 times each; iii. Drying is vacuum drying, the drying temperature is 40-80°C, and the drying time is 10-14h.

9. The method for preparing the nanoporous B-site high entropy perovskite oxide electrocatalytic material according to claim 3, It is characterized in that In step (2), the annealing treatment conditions are: in an air atmosphere, heating to 800-900°C at a heating rate of 3-5°C / min, keeping at 800-900°C for 2-4h, and then cooling to room temperature at a cooling rate of 3-5°C / min.

10. Use of the nanoporous B-site high entropy perovskite oxide electrocatalytic material as claimed in claim 1 or 2, It is characterized in that Applied to electrocatalytic hydrogen evolution reaction or electrocatalytic water decomposition.

Citation Information

Patent Citations

  • Perovskite oxide catalyst and preparation method and application thereof

    CN109759077A

  • High-entropy perovskite oxide and preparation method and application thereof

    CN116177627A

Cited By

  • High-entropy perovskite oxide catalyst and preparation method and application thereof

    CN119456053A

  • High-entropy double-perovskite type direct ammonia solid oxide fuel cell anode material as well as preparation method and application thereof

    CN120136537A

  • High-entropy perovskite material and preparation method and application thereof

    CN120649063A

  • Lanthanum-based perovskite oxide electrode material for electrochemical energy storage applications

    US12534386B1