Self-adhesive macromolecular pre-paved waterproof coiled material and preparation method thereof
By modifying the sandwich structure of the emulsion layer and the coextruded additional layer, the low molecular weight substances in the hot melt pressure-sensitive adhesive layer are prevented from migrating into the substrate, and the problems of decreasing adhesion force and increasing dimensional change rate in the prior art are solved, and the problems of increasing adhesion force in the prior art are improved. The durability and applicability of the waterproof coil material are suitable for existing testing methods.
Patent Information
- Application Number
- CN202410960182.0
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-07-17
- Publication Date
- 2024-11-08
AI Technical Summary
Plasticizers and low molecular weight substances of the hot melt pressure-sensitive adhesive layer in the existing pre-layed waterproof coils are migrated to the substrate, resulting in a decrease in adhesive force, a decrease in substrate performance and an increase in dimensional change rate, and an increased barrier layer It is easy to cause the adhesive layer to separate from the substrate, affecting the waterproof performance, and is not applicable to the current testing methods.
The sandwich structure of the modified emulsion layer-coextruded additional layer-main material layer-coextruded additional layer-modified emulsion layer-modified emulsion layer is adopted to prevent the migration of low molecular weight substances in the hot melt pressure-sensitive adhesive layer by coextruded additional layer and modified emulsion layer. It is suitable for the existing pre-layed waterproof coil testing method.
Effectively prevent low molecular weight substances in the hot melt pressure-sensitive adhesive layer from migrating into the substrate, reducing the dimensional change rate, improving the peel strength of thermal aging, and enhancing the physical properties of the substrate. It is suitable for the existing pre-layed waterproof coil testing methods, and improving the overall Durability and waterproofing.
Smart Images

Figure CN118909559A_ABST
Abstract
Description
Technical Field
[0001] The invention relates to a self-adhesive polymer pre-laid waterproof coiled material and a preparation method thereof, and is applied in the field of waterproof coiled material production. Background Art
[0002] The statements in this section merely provide background information related to the present disclosure and may not constitute prior art.
[0003] In the existing pre-laid waterproofing membrane system (such as CN202311648071.8), the adhesive layer bonded to the substrate is a hot melt pressure-sensitive adhesive. Since the hot melt pressure-sensitive adhesive contains a large amount of plasticizer components, the plasticizer in the adhesive layer and the low-molecular substances produced by aging will move to the surface of the adhesive layer and gradually migrate into the substrate during long-term use. This phenomenon will lead to the following two situations: 1. The average molecular weight of the hot melt pressure-sensitive adhesive system gradually increases, resulting in a decrease in adhesion; 2. The average molecular weight of the substrate decreases due to the migration of the plasticizer, and substances of different polarities are also introduced, causing the physical properties and durability of the substrate to decrease, and the dimensional change rate to increase, thereby affecting the overall waterproofing effect of the waterproofing membrane.
[0004] In order to avoid this situation, manufacturers often adopt the method of adding a barrier layer with low deformation rate. However, this method reduces the elongation of the waterproof membrane under the maximum tensile force, and because the physical properties of the barrier layer and the substrate are too different (such as the elongation under maximum tensile force, tensile strength and other properties), the waterproof membrane is prone to stratification or breakage during the foundation settlement process, which affects its waterproof performance. As mentioned in Chinese Patent 202310799247.3: A hot melt adhesive film is arranged between the polymer substrate layer and the adhesive layer, and the hot melt adhesive film includes a first adhesive layer, a transition layer, a barrier layer and a second adhesive layer which are stacked in sequence. The first adhesive layer is used to bond with the polymer substrate layer, and the second adhesive layer is used to bond with the adhesive layer. The isolation layer is a nylon layer to block the migration of plasticizers in the adhesive layer and reduce the dimensional change rate of the waterproof membrane. However, the tensile properties between the nylon layer and the polyethylene main layer (i.e., the second adhesive layer) are too different, which will still cause the waterproof membrane to be easily delaminated or broken during the foundation settlement process, thereby affecting its waterproof performance. The problem is that when testing the tensile properties of the waterproof membrane, the nylon layer will break in advance, causing the adhesive layer to separate from the substrate, resulting in a test failure. At the same time, the various performance test methods related to sheets in the national standard GB / T 23457-2017 for pre-laid waterproof membranes are a continuation of the homogeneous sheet (JS2) test method in the national standard GB 18173.1-2012 for polymer waterproof membranes, while the sheet described in the patent belongs to the composite sheet (FS2) in the national standard GB 18172.1-2012. This type of sheet is not suitable for the current homogeneous sheet (JS2) test method, that is, it is not suitable for the current pre-laid waterproof membrane test method.
[0005] Therefore, it has become an urgent task to provide a self-adhesive polymer pre-laid waterproof membrane and a preparation method thereof, which can effectively prevent the plasticizer and low molecular weight substances in the hot-melt pressure-sensitive adhesive layer from migrating into the substrate, has a low dimensional change rate, high thermal aging peel strength, and is suitable for the existing pre-laid waterproof membrane (homogeneous sheet) testing method. Summary of the invention
[0006] In order to overcome the practice of adding a barrier layer to block the migration of plasticizer in the adhesive layer in the existing pre-laid waterproof membrane, which has the disadvantages that the barrier layer can easily cause the adhesive layer to separate from the substrate, resulting in test failure, and the testing method of the existing pre-laid waterproof membrane is not applicable. The present invention provides a self-adhesive polymer pre-laid waterproof membrane and a preparation method thereof, which improves the structure and system formula of the substrate, and has a sandwich structure of a modified emulsion layer-coextruded additional layer-main material layer-coextruded additional layer-modified emulsion layer, and a preferred system formula of the synergistic coextruded additional layer, modified emulsion layer, and main material layer. It can effectively prevent low molecular weight substances in the hot melt pressure-sensitive adhesive layer from migrating into the substrate, and has the advantages of low dimensional change rate, high thermal aging peel strength, and is applicable to the existing testing method of pre-laid waterproof membrane.
[0007] The technical solution of the present invention is as follows:
[0008] A self-adhesive polymer pre-laid waterproofing coiled material, comprising an isolation sand layer, an isolation film layer, a hot melt pressure-sensitive adhesive layer, a substrate, a hot melt pressure-sensitive adhesive layer and an isolation film layer stacked in sequence from top to bottom, wherein the substrate comprises a modified latex layer, a co-extruded additional layer, a main material layer, a co-extruded additional layer and a modified latex layer stacked in sequence from top to bottom, the pressure-sensitive adhesive layer is a hot melt pressure-sensitive adhesive; the isolation sand layer adopts isolation sand;
[0009] The co-extruded additional layer is mainly prepared from the following components in the following weight ratios:
[0010]
[0011] The main material layer is mainly prepared from the following components in the following weight ratios:
[0012]
[0013] The modified emulsion layer adopts a silane coupling agent modified emulsion, and the silane coupling agent modified emulsion is mainly prepared from the following components in the following weight ratio:
[0014] 9-11 parts of nano-TiO2 dispersion solution,
[0015] Silane coupling agent solution 9-11 parts,
[0016] 48-52 parts of emulsion;
[0017] The mass concentration of the silane coupling agent in the silane coupling agent solution is 20-30%, the mass concentration of the nano-TiO2 in the nano-TiO2 dispersion solution is 0.05-0.1%, and the emulsion is one of acrylic emulsion, methyl methacrylate emulsion or methacrylic acid emulsion or any combination of any two or more thereof.
[0018] The self-adhesive polymer pre-laid waterproofing membrane of the present application improves the structure and system formula of the substrate, and through the sandwich structure of modified emulsion layer-coextruded additional layer-main material layer-coextruded additional layer-modified emulsion layer, the preferred system formula of the coextruded additional layer, the modified emulsion layer, and the main material layer, it has the advantages of being able to effectively prevent low molecular weight substances in the hot melt pressure-sensitive adhesive layer from migrating into the substrate, and having a low dimensional change rate, high thermal aging peeling strength, and being applicable to the existing pre-laid waterproofing membrane test method. That is, the self-adhesive polymer pre-laid waterproofing membrane is based on the original homogeneous single-layer main material layer, and a double-layer coextruded additional layer is superimposed and compounded on both sides, and then the modified emulsion layer is coated on the outer side walls of the two layers, and after curing into a film, the modified emulsion layer is attached to the outer side wall of the coextruded additional layer. The substrate sandwich structure of modified emulsion layer-coextruded additional layer-main material layer-coextruded additional layer-modified emulsion layer effectively prevents the low molecular weight substances in the hot melt pressure sensitive adhesive layer from migrating into the main material layer, and the simple compound between the modified emulsion layer, the coextruded additional layer and the main material layer can prevent the substrate from being delaminated during the tensile test. While improving the physical properties of the substrate, it increases the bonding effect between the hot melt pressure sensitive adhesive layer and the substrate, and to a certain extent prevents the migration of plasticizers and low molecular weight substances in the hot melt pressure sensitive adhesive layer to the substrate, thereby improving the overall durability of the roll material, making it have a low dimensional change rate and high thermal aging peeling strength, making the self-adhesive polymer pre-laid waterproof roll material suitable for the existing pre-laid waterproof roll material (homogeneous sheet) test method. Among them, the density range of high-density polyethylene is 0.94-0.96g / cm 3 The density of linear low-density polyethylene ranges from 0.915 to 0.935 g / cm 3 .
[0019] The preferred functions of the components of the co-extruded additional layer are as follows:
[0020] ① The high-density polyethylene may preferably be injection-molding grade high-density and high-strength polyethylene, the main function of which is to improve the density of its surface by increasing the overall density of the co-extruded additional layer;
[0021] ② The styrene-isoprene-styrene block copolymer elastomer is preferably the same type of rubber component as the hot melt pressure sensitive adhesive system of the hot melt pressure sensitive adhesive layer. After the low molecular weight substances in the hot melt pressure sensitive adhesive migrate to the co-extruded additional layer, the fusion of the two can form a mixed component similar to the hot melt pressure sensitive adhesive, which plays a certain role in promoting adhesion; at the same time, because of the principle of like dissolves like, the hot melt pressure sensitive adhesive can be made more difficult to peel off from the substrate in this component;
[0022] ③ The polypropylene preferably has a higher melt index than the high-density polyethylene, and acts as a bridge for the fusion of the high-density polyethylene and the styrene-isoprene-styrene block copolymer elastomer during the extrusion plasticization stage;
[0023] ④ Maleic anhydride grafted polyethylene can be used as a fusion aid between high-density polyethylene, styrene-isoprene-styrene block copolymer elastomer and polypropylene, which can also improve the density of the system and further increase the surface density;
[0024] ⑤ Titanium dioxide can preferably be treated with organic coating on the surface (i.e., coated with stearic acid, because stearic acid is a long-chain saturated fatty acid, which has a long carbon chain lipophilic end and a carboxyl hydrophilic end. After being coated with stearic acid, it can increase the affinity with organic polymers). Nano-sized titanium dioxide can act as the crystal nucleus of the crystallization while being melt-mixed with various organic polymers, thereby increasing the overall density by increasing the crystallization rate;
[0025] ⑥ Antioxidants can prevent the co-extruded additional layer from aging during the blending, granulation and extrusion stages.
[0026] The modified emulsion layer is formed by re-treating the surface of the coil after it is formed using a silane coupling agent modified emulsion, forming a thin protective layer on the surface of the substrate, which prevents the adhesive layer from ironing the substrate during high-temperature coating of the hot-melt pressure-sensitive adhesive during the production process, as well as the rapid migration of plasticizers and low-molecular substances to the substrate at high temperatures.
[0027] The main material layer is the main body of the substrate, based on high-density polyethylene supplemented with linear low-density polyethylene and thermoplastic elastomer to improve flexibility, and then adds polypropylene that can improve impact resistance to improve its impact resistance and puncture resistance. Its preferred formula can increase the density of the polymer system and reduce the content of fillers in the system. These two changes can prevent the migration of plasticizers and low molecular weight substances of hot melt pressure-sensitive adhesives to the main material layer, making the main material layer stronger and lower in cost.
[0028] The hot melt pressure sensitive adhesive is mainly prepared from the following components in the following weight ratios:
[0029]
[0030] The diblock content of the styrene-isoprene-styrene block copolymer elastomer is 50%.
[0031] The hot melt pressure sensitive adhesive used in the hot melt pressure sensitive adhesive layer adopts raw materials without low molecular weight plasticizers, while the common hot melt pressure sensitive adhesive formula on the market includes styrene-isoprene-styrene block copolymer, cyclohexane oil and petroleum resin, etc. The present invention adjusts the selection and proportion of its raw materials, and improves the overall molecular weight of the system without reducing the initial adhesion strength of the system. At the same time, a variety of raw materials with high hydrogenation degree are introduced to improve the aging resistance of the system. These two means can improve the stability and aging resistance of the system, so that the hot melt pressure sensitive adhesive is not easy to produce low molecular weight substances. Furthermore, discarding the low molecular weight raw materials in the existing formula, such as cyclohexane oil and low softening point petroleum resin, etc., can further reduce the content of low molecular weight substances in the system, so as to further reduce the probability and rate of low molecular weight substances in the hot melt pressure sensitive adhesive migrating into the substrate from the aspect of reducing the content of low molecular weight substances.
[0032] The role of each component in the system:
[0033] ① Elastomer: Styrene-isoprene-styrene block copolymer elastomer is used as the main material, and styrene-ethylene-butylene-styrene block copolymer elastomer, styrene-butadiene rubber elastomer and maleic anhydride modified amorphous α-olefin copolymer are used in combination. The diblock content of the styrene-isoprene-styrene block copolymer elastomer is 50% to provide suitable cohesion and initial adhesion to the hot melt pressure-sensitive adhesive system. Styrene-ethylene-butylene-styrene block copolymer elastomer can improve the overall molecular weight and aging resistance of the system. Styrene-butadiene rubber can improve the heat resistance, initial adhesion and molecular weight of the system. Maleic anhydride modified amorphous α-olefin copolymer can improve the initial adhesion of the system and make the polarity of the system more suitable for bonding with the substrate.
[0034] ② Tackifier: Fully hydrogenated dicyclopentadiene petroleum resin is used as the main component, and C5 / C9 copolymerized petroleum resin and maleic anhydride modified C5 petroleum resin are used in combination. Fully hydrogenated dicyclopentadiene petroleum resin is used as the main component of the tackifier to improve the aging resistance of the system and prevent the system from aging and producing low molecular weight substances; C5 / C9 copolymerized petroleum resin can improve the initial viscosity of the system; maleic anhydride modified C5 petroleum resin makes the polarity of the system more suitable for bonding of the substrate.
[0035] ③ The softener is selected from medium molecular weight polyisobutylene to increase the molecular weight of the entire system and reduce the probability of precipitation of low molecular weight substances.
[0036] ④ Increase the dosage of antioxidants and other additives in the existing hot melt pressure sensitive adhesive system to reduce the aging rate of the hot melt pressure sensitive adhesive system and avoid the production of excessive low molecular weight substances due to the aging of the hot melt pressure sensitive adhesive.
[0037] The isolation sand is mainly prepared from the following components in the following weight ratios:
[0038]
[0039] The composite osmotic crystal is mainly prepared from the following components in the following weight ratios:
[0040]
[0041] The isolation sand used in the isolation layer has calcium carbonate mineral particles as the core layer. The surface density of the isolation sand is increased by adding emulsion and composite penetration crystallization into the system to prevent low molecular weight substances in the hot melt pressure sensitive adhesive from penetrating and migrating into the isolation sand. The emulsion uses a general acrylic emulsion. The introduction of the emulsion can increase the surface density and strength of the cement after curing. The composite penetration crystallization will produce its own penetration crystallization effect during the preparation and use process. During the aging process of the isolation sand, the surface density and strength can be gradually increased through the reaction between its material and cement to prevent the plasticizer and low molecular weight substances of the hot melt pressure sensitive adhesive from migrating into the isolation sand. Among them, the color powder can be an inorganic color powder.
[0042] The isolation sand is composed of isolation sand with a particle size of 40-50 meshes, isolation sand with a particle size of 60-70 meshes and isolation sand with a particle size of 80 meshes, and the weight percentages thereof are 70±2%, 25±5% and 2-8% respectively.
[0043] The preferred graded isolation sand has a better barrier effect on the migration of plasticizers and low molecular weight substances in hot melt pressure sensitive adhesives.
[0044] The silane coupling agent is one of alkyl silane coupling agents, aromatic silane coupling agents, vinyl triethoxysilane, vinyl trimethoxysilane or vinyl tri-β-methylethoxysilane, or any combination of any two or more thereof; the isolation film layer adopts a release film with a PE substrate and a release agent coated on one side.
[0045] The modified emulsion layer prepared by the preferred silane coupling agent has better barrier effect. The preferred isolation film layer is easy to use and has good barrier effect.
[0046] The thickness of the modified emulsion layer is 0.06-0.10 mm, the thickness of the co-extruded additional layer is 0.08-0.12 mm, the thickness of the hot melt pressure sensitive adhesive layer is 0.27-0.3 mm, and the thickness of the isolation film layer is 0.03-0.04 mm.
[0047] The preferred thicknesses of the modified emulsion layer, the co-extruded additional layer, and the isolation film layer can ensure the barrier effect on the migration of hot-melt pressure-sensitive adhesive plasticizers and low molecular weight substances, and can also make the overall thickness of the self-adhesive polymer pre-laid waterproof membrane moderate.
[0048] The method for preparing the self-adhesive polymer pre-laid waterproofing membrane mainly comprises the following steps performed in sequence:
[0049] (I) Preparation of substrate
[0050] (1) Preparation of main material layer particles
[0051] The production temperature of the twin-screw extruder is set at 180-200°C, high-density polyethylene, linear low-density polyethylene, polypropylene, thermoplastic elastomer, maleic anhydride grafted polyethylene, titanium dioxide and antioxidant are fed into the first feeding port of the twin-screw extruder, and heavy calcium carbonate is fed into the second feeding port of the twin-screw extruder, and the main material layer particles are obtained by discharging the materials;
[0052] (2) Preparation of co-extruded additional layer particles
[0053] The production temperature of the single-screw extruder is set at 180-200°C, and high-density polyethylene, styrene-isoprene-styrene block copolymer elastomer, polypropylene, maleic anhydride grafted polyethylene, titanium dioxide and antioxidant are fed into the feeding port of the single-screw extruder, and the co-extruded additional layer particles are obtained by discharging the materials;
[0054] (3) Preparation of silane coupling agent modified emulsion
[0055] ① Slowly drip a silane coupling agent solution with a silane coupling agent mass concentration of 20-30% into a nano-TiO2 dispersion solution with a nano-TiO2 mass concentration of 0.05-0.1% under a pH value of 3-5, disperse evenly, adjust the pH value to 9-10, and then dry and grind until there are no obvious particles to obtain TiO2 modified by silane coupling agent;
[0056] ② Add the TiO2 modified with the silane coupling agent obtained in step ① into the emulsion, and stir at 800-1000 rpm for 20-30 minutes to obtain a silane coupling agent modified emulsion;
[0057] (4) Preparation of substrate
[0058] ① Put the co-extruded additional layer particles and the main material layer particles into the screw extruder together, and extrude the co-extruded additional layer, the main material layer and the co-extruded additional layer from the upper die port, the middle die port and the lower die port at 180-200°C respectively, and then extrude and laminate with three rollers to obtain a laminated coil with the co-extruded additional layer sandwiching the main material layer;
[0059] ② After the laminated coil is cooled and shaped, spray the silane coupling agent modified emulsion on the upper and lower surfaces of the laminated coil respectively, and then dry it at 60-90°C to obtain a modified emulsion layer, that is, to obtain the substrate;
[0060] (II) Preparation of self-adhesive polymer pre-laid waterproof membrane
[0061] A hot melt pressure-sensitive adhesive melting at 150-180°C is coated on the upper and lower surfaces of the substrate to obtain a hot melt pressure-sensitive adhesive layer, and then isolation films are respectively covered on the outer surfaces of the two hot melt pressure-sensitive adhesive layers to obtain an isolation film layer, and then isolation sand is fully spread on the outer surface of the isolation film layer above the substrate to obtain an isolation sand layer.
[0062] The preparation method of the self-adhesive polymer pre-laid waterproofing membrane of the present application has simple steps and is easy to operate. The co-extruded additional layer and the main material layer are co-extruded at the same temperature and laminated by three-roll calendering (taking 3-5 seconds), ensuring that the composite strength between the two meets the test requirements.
[0063] The preparation method of the hot melt pressure sensitive adhesive mainly comprises the following steps performed in sequence:
[0064] (1) starting a stirrer, adjusting the temperature to 160-170° C., adjusting the stirring speed to 150-250 rpm, adding styrene-ethylene-butylene-styrene block copolymer elastomer, styrene-isoprene-styrene block copolymer elastomer, styrene-butadiene rubber elastomer, maleic anhydride modified amorphous α-olefin copolymer, medium molecular weight polyisobutylene and antioxidant into the stirrer, and stirring for 20-30 minutes;
[0065] (2) adjusting the temperature of the mixer to 170-180° C. and the stirring speed to 250-350 rpm, and continuing to add maleic anhydride-modified C5 petroleum resin, C5 / C9 copolymerized petroleum resin and fully hydrogenated dicyclopentadiene petroleum resin into the mixer, and stirring for 30-40 minutes;
[0066] (3) The stirring speed of the mixer is adjusted to 150-250 rpm, the temperature is maintained at 170-180° C., and the light stabilizer and the ultraviolet absorber are continuously added to the mixer, and stirred for at least 30 minutes to obtain a hot melt pressure-sensitive adhesive.
[0067] The preparation method of the hot melt pressure sensitive adhesive has simple steps and is easy to operate.
[0068] The preparation method of the isolation sand mainly comprises the following steps performed in sequence:
[0069] (1) Preparation of composite infiltration crystals
[0070] The sodium silicate or potassium silicate, calcium hydroxide or sodium hydroxide, benzalkonium bromide, thiosulfate, citrate and calcium lactate are uniformly mixed to obtain composite osmotic crystals;
[0071] (2) mixing acrylic emulsion, water, composite infiltration crystal, silane coupling agent, color powder and ordinary Portland cement to obtain slurry;
[0072] (3) starting the mixer and adjusting the stirring speed to 60-100 rpm, wetting the surface of the calcium carbonate mineral particles and then putting them into the mixer, then slowly adding the slurry obtained in step (2) into the mixer and stirring until uniform, to obtain particles coated with the slurry;
[0073] (4) The particles coated with the slurry obtained in step (3) are taken out, sieved and graded, and dried at 75-85° C. until completely dry, thereby obtaining the isolation sand to be prepared.
[0074] The preparation method of the isolation sand has simple steps and is easy to operate.
[0075] The sieving and grading in step (4) includes the following steps performed in sequence: the particles coated with the slurry are sieved through a 40-50 mesh sieve, a 60-70 mesh sieve and an 80 mesh sieve respectively, and then the three are mixed in a ratio of 70%, 25% and 5% by weight.
[0076] The screening and grading steps are simple and easy to operate.
[0077] Compared with the prior art, the present invention has the following advantages:
[0078] 1) The structure and system formula of the improved substrate of the self-adhesive polymer pre-laid waterproofing membrane of the present application, through the sandwich structure of modified emulsion layer-coextruded additional layer-main material layer-coextruded additional layer-modified emulsion layer, and the preferred system formula of the synergistic coextruded additional layer, modified emulsion layer, and main material layer, has the advantages of being able to effectively prevent low molecular weight substances in the hot melt pressure-sensitive adhesive layer from migrating into the substrate, and having low dimensional change rate, high thermal aging peel strength, and being applicable to the existing pre-laid waterproofing membrane test method;
[0079] 2) The hot melt pressure sensitive adhesive layer preferably has a low content of low molecular weight substances;
[0080] 3) The preferred isolation sand can effectively prevent the plasticizer and low molecular weight substances of the hot melt pressure sensitive adhesive from migrating to the isolation sand;
[0081] 4) The preferred graded isolation sand has a better barrier effect on the migration of plasticizers and low molecular weight substances in hot melt pressure sensitive adhesives;
[0082] 5) The preparation method of the self-adhesive polymer pre-laid waterproofing membrane has simple steps and is easy to operate. BRIEF DESCRIPTION OF THE DRAWINGS
[0083] Figure 1 It is a cross-sectional view of the self-adhesive polymer pre-laid waterproofing membrane and the preparation method thereof of the present invention;
[0084] Figure 2It is a cross-sectional view of a substrate of the self-adhesive polymer pre-laid waterproofing coiled material and a preparation method thereof according to the present invention.
[0085] Description of labels:
[0086] An isolation sand layer 1, an isolation film layer 2, a hot-melt pressure-sensitive adhesive layer 3, a substrate 4, a modified latex layer 4-1, a co-extruded additional layer 4-2, and a main material layer 4-3. DETAILED DESCRIPTION
[0087] The technical solution of the present invention will be clearly and completely described below in conjunction with various embodiments.
[0088] Example 1
[0089] like Figure 1-2 As shown, the self-adhesive polymer pre-laid waterproofing membrane described in the present invention comprises an isolation sand layer 1, an isolation film layer 2, a hot melt pressure-sensitive adhesive layer 3, a substrate 4, a hot melt pressure-sensitive adhesive layer 3 and an isolation film layer 2 stacked in sequence from top to bottom, wherein the substrate 4 comprises a modified emulsion layer 4-1, a co-extruded additional layer 4-2, a main material layer 4-3, a co-extruded additional layer 4-2 and a modified emulsion layer 4-1 stacked in sequence from top to bottom, and the pressure-sensitive adhesive layer is a hot melt pressure-sensitive adhesive; the isolation sand layer 1 is made of isolation sand;
[0090] The co-extruded additional layer 4-2 is mainly prepared from the following components in the following weight ratios:
[0091]
[0092] The main material layer 4-3 is mainly prepared from the following components in the following weight ratios:
[0093]
[0094]
[0095] The modified emulsion layer 4-1 adopts a silane coupling agent modified emulsion, and the silane coupling agent modified emulsion is mainly prepared from the following components in the following weight ratios:
[0096] 10 parts of nano-TiO2 dispersion solution,
[0097] Silane coupling agent solution 10 parts,
[0098] Emulsion 50 parts;
[0099] The mass concentration of the silane coupling agent in the silane coupling agent solution is 25%, the mass concentration of the nano-TiO2 in the nano-TiO2 dispersion solution is 0.08%, and the emulsion is an acrylic emulsion.
[0100] The hot melt pressure sensitive adhesive is mainly prepared from the following components in the following weight ratios:
[0101]
[0102] The diblock content of the styrene-isoprene-styrene block copolymer elastomer is 50%.
[0103] The isolation sand is mainly prepared from the following components in the following weight ratios:
[0104]
[0105]
[0106] The composite osmotic crystal is mainly prepared from the following components in the following weight ratios:
[0107]
[0108] The isolation sand is composed of isolation sand with a particle size of 40-50 meshes, isolation sand with a particle size of 60-70 meshes and isolation sand with a particle size of 80 meshes, and the weight percentages thereof are 70%, 27% and 3% respectively.
[0109] The silane coupling agent is an alkyl silane coupling agent; the isolation film layer 2 is a release film with PE as the base material 4 and a release agent coated on one side.
[0110] The thickness of the modified emulsion layer 4 - 1 is 0.08 mm, the thickness of the co-extruded additional layer 4 - 2 is 0.1 mm, the thickness of the hot-melt pressure-sensitive adhesive layer 3 is 0.28 mm, and the thickness of the isolation film layer 2 is 0.035 mm.
[0111] The method for preparing the self-adhesive polymer pre-laid waterproofing membrane mainly comprises the following steps performed in sequence:
[0112] (I) Preparation of substrate 4
[0113] (1) Preparation of main material layer 4-3 particles
[0114] The production temperature of the twin-screw extruder is set to 1900°C, high-density polyethylene, linear low-density polyethylene, polypropylene, thermoplastic elastomer, maleic anhydride grafted polyethylene, titanium dioxide and antioxidant are fed into the first feeding port of the twin-screw extruder, and heavy calcium carbonate is fed into the second feeding port of the twin-screw extruder, and the main material layer 4-3 particles are obtained by discharging the materials;
[0115] (2) Preparation of co-extruded additional layer 4-2 particles
[0116] The production temperature of the single screw extruder is set at 180-200°C, and high-density polyethylene, styrene-isoprene-styrene block copolymer elastomer, polypropylene, maleic anhydride grafted polyethylene, titanium dioxide and antioxidant are fed into the feeding port of the single screw extruder, and the co-extruded additional layer 4-2 particles are obtained by discharging the materials;
[0117] (3) Preparation of silane coupling agent modified emulsion
[0118] ① Slowly drip a silane coupling agent solution with a silane coupling agent mass concentration of 25% into a nano-TiO2 dispersion solution with a nano-TiO2 mass concentration of 0.08% at a pH value of 4, disperse evenly, adjust the pH value to 9.5, and then dry and grind until there are no obvious particles to obtain TiO2 modified by a silane coupling agent;
[0119] ② Add the TiO2 modified with the silane coupling agent obtained in step ① into the emulsion, and stir at 900 rpm for 25 minutes to obtain a silane coupling agent modified emulsion;
[0120] (4) Preparation of substrate 4
[0121] ① Put the co-extruded additional layer particles and the main material layer particles into a screw extruder together, extrude the co-extruded additional layer, the main material layer and the co-extruded additional layer from the upper die port, the middle die port and the lower die port at 190°C respectively, and then extrude and laminate them with three rollers to obtain a laminated coil with the co-extruded additional layer 4-2 sandwiching the main material layer 4-3;
[0122] ② After the laminated coil is cooled and shaped, the silane coupling agent modified emulsion is sprayed on the upper and lower surfaces of the laminated coil respectively, and then dried at 80° C. to obtain a modified emulsion layer 4-1, that is, a substrate 4 is obtained;
[0123] (II) Preparation of self-adhesive polymer pre-laid waterproof membrane
[0124] A hot-melt pressure-sensitive adhesive melting at 160° C. is coated on the upper and lower surfaces of a substrate 4 to obtain a hot-melt pressure-sensitive adhesive layer 3, and then isolation films are respectively covered on the outer surfaces of the two hot-melt pressure-sensitive adhesive layers 3 to obtain an isolation film layer 2, and then isolation sand is fully spread on the outer surface of the isolation film layer 2 located above the substrate 4 to obtain an isolation sand layer 1.
[0125] The preparation method of the hot melt pressure sensitive adhesive mainly comprises the following steps performed in sequence:
[0126] (1) starting a stirrer, adjusting the temperature to 165° C. and the stirring speed to 200 rpm, adding a styrene-ethylene-butylene-styrene block copolymer elastomer, a styrene-isoprene-styrene block copolymer elastomer, a styrene-butadiene rubber elastomer, a maleic anhydride-modified amorphous α-olefin copolymer, a medium molecular weight polyisobutylene, and an antioxidant into the stirrer, and stirring for 25 minutes;
[0127] (2) adjusting the temperature of the mixer to 175° C. and the stirring speed to 300 rpm, and continuing to add maleic anhydride-modified C5 petroleum resin, C5 / C9 copolymerized petroleum resin and fully hydrogenated dicyclopentadiene petroleum resin into the mixer, and stirring for 35 minutes;
[0128] (3) The stirring speed of the mixer is adjusted to 200 rpm, the temperature is maintained at 175° C., and the light stabilizer and the ultraviolet absorber are continuously added to the mixer, and stirred for 30 minutes to obtain a hot melt pressure-sensitive adhesive.
[0129] The preparation method of the isolation sand mainly comprises the following steps performed in sequence:
[0130] (1) Preparation of composite infiltration crystals
[0131] The sodium silicate, sodium hydroxide, benzalkonium bromide, thiosulfate, citrate and calcium lactate are uniformly mixed to obtain composite osmotic crystals;
[0132] (2) mixing acrylic emulsion, water, composite infiltration crystal, silane coupling agent, color powder and ordinary Portland cement to obtain slurry;
[0133] (3) starting the mixer and adjusting the stirring speed to 80 rpm, wetting the surface of the calcium carbonate mineral particles and then putting them into the mixer, then slowly adding the slurry obtained in step 2 into the mixer and stirring until uniform to obtain particles coated with the slurry;
[0134] (4) The particles coated with the slurry obtained in step 3 are taken out, sieved and graded, and dried at 80° C. until completely dry, thereby obtaining the isolation sand to be prepared.
[0135] The sieving and grading in step 4 includes the following steps performed in sequence: the particles wrapped with the slurry are sieved through a 40-50 mesh sieve, a 60-70 mesh sieve and an 80 mesh sieve respectively, and then the three are mixed in a ratio of 70%, 27% and 3% by weight.
[0136] Example 2
[0137] like Figure 1-2 As shown, the self-adhesive polymer pre-laid waterproofing membrane described in the present invention comprises an isolation sand layer 1, an isolation film layer 2, a hot melt pressure-sensitive adhesive layer 3, a substrate 4, a hot melt pressure-sensitive adhesive layer 3 and an isolation film layer 2 stacked in sequence from top to bottom, wherein the substrate 4 comprises a modified emulsion layer 4-1, a co-extruded additional layer 4-2, a main material layer 4-3, a co-extruded additional layer 4-2 and a modified emulsion layer 4-1 stacked in sequence from top to bottom, and the pressure-sensitive adhesive layer is a hot melt pressure-sensitive adhesive; the isolation sand layer 1 is made of isolation sand;
[0138] The co-extruded additional layer 4-2 is mainly prepared from the following components in the following weight ratios:
[0139]
[0140] The main material layer 4-3 is mainly prepared from the following components in the following weight ratios:
[0141]
[0142] The modified emulsion layer 4-1 adopts a silane coupling agent modified emulsion, and the silane coupling agent modified emulsion is mainly prepared from the following components in the following weight ratios:
[0143] 9 parts of nano-TiO2 dispersion solution,
[0144] Silane coupling agent solution 11 parts,
[0145] Emulsion 48 parts;
[0146] The mass concentration of the silane coupling agent in the silane coupling agent solution is 20%, the mass concentration of the nano-TiO2 in the nano-TiO2 dispersion solution is 0.1%, and the emulsion is any combination of acrylic emulsion and methyl methacrylate emulsion.
[0147] The hot melt pressure sensitive adhesive is mainly prepared from the following components in the following weight ratios:
[0148]
[0149]
[0150] The diblock content of the styrene-isoprene-styrene block copolymer elastomer is 50%.
[0151] The isolation sand is mainly prepared from the following components in the following weight ratios:
[0152]
[0153] The composite osmotic crystal is mainly prepared from the following components in the following weight ratios:
[0154]
[0155] The isolation sand is composed of isolation sand with a particle size of 40-50 meshes, isolation sand with a particle size of 60-70 meshes and isolation sand with a particle size of 80 meshes, and the weight percentages thereof are 68%, 30% and 2% respectively.
[0156] The silane coupling agent is any combination of an alkyl silane coupling agent and an aromatic silane coupling agent; the isolation film layer 2 is a release film with a PE substrate 4 and a release agent coated on one side.
[0157] The thickness of the modified emulsion layer 4 - 1 is 0.06 mm, the thickness of the co-extruded additional layer 4 - 2 is 0.12 mm, the thickness of the hot melt pressure sensitive adhesive layer 3 is 0.27 mm, and the thickness of the isolation film layer 2 is 0.04 mm.
[0158] The method for preparing the self-adhesive polymer pre-laid waterproofing membrane mainly comprises the following steps performed in sequence:
[0159] (I) Preparation of substrate 4
[0160] (1) Preparation of main material layer 4-3 particles
[0161] The production temperature of the twin-screw extruder is set at 180°C, high-density polyethylene, linear low-density polyethylene, polypropylene, thermoplastic elastomer, maleic anhydride grafted polyethylene, titanium dioxide and antioxidant are fed into the first feeding port of the twin-screw extruder, and heavy calcium carbonate is fed into the second feeding port of the twin-screw extruder, and the main material layer 4-3 particles are obtained by discharging the materials;
[0162] (2) Preparation of co-extruded additional layer 4-2 particles
[0163] The production temperature of the single-screw extruder is set at 180° C. High-density polyethylene, styrene-isoprene-styrene block copolymer elastomer, polypropylene, maleic anhydride grafted polyethylene, titanium dioxide and antioxidant are fed into the feeding port of the single-screw extruder, and the co-extruded additional layer 4-2 particles are obtained by discharging the materials;
[0164] (3) Preparation of silane coupling agent modified emulsion
[0165] ① Slowly drip a silane coupling agent solution with a silane coupling agent mass concentration of 20% into a nano-TiO2 dispersion solution with a nano-TiO2 mass concentration of 0.1% under a pH value of 3-5, disperse evenly, then adjust the pH value to 9, and then dry and grind until there are no obvious particles to obtain TiO2 modified by a silane coupling agent;
[0166] ② Add the TiO2 modified with the silane coupling agent obtained in step ① into the emulsion, and stir at 1000 rpm for 20 minutes to obtain a silane coupling agent modified emulsion;
[0167] (4) Preparation of substrate 4
[0168] ① Put the co-extruded additional layer particles and the main material layer particles into the screw extruder together, and extrude the co-extruded additional layer, the main material layer and the co-extruded additional layer from the upper die port, the middle die port and the lower die port at 180°C respectively, and then extrude and laminate them with three rollers to obtain a laminated coil with the co-extruded additional layer 4-2 sandwiching the main material layer 4-3;
[0169] ② After the laminated coil is cooled and shaped, the silane coupling agent modified emulsion is sprayed on the upper and lower surfaces of the laminated coil respectively, and then dried at 60-90° C. to obtain a modified emulsion layer 4-1, that is, a substrate 4 is obtained;
[0170] (II) Preparation of self-adhesive polymer pre-laid waterproof membrane
[0171] A hot-melt pressure-sensitive adhesive melting at 150° C. is coated on the upper and lower surfaces of a substrate 4 to obtain a hot-melt pressure-sensitive adhesive layer 3, and then isolation films are respectively covered on the outer surfaces of the two hot-melt pressure-sensitive adhesive layers 3 to obtain an isolation film layer 2, and then isolation sand is fully spread on the outer surface of the isolation film layer 2 located above the substrate 4 to obtain an isolation sand layer 1.
[0172] The preparation method of the hot melt pressure sensitive adhesive mainly comprises the following steps performed in sequence:
[0173] (1) starting a stirrer, adjusting the temperature to 160° C. and the stirring speed to 250 rpm, adding a styrene-ethylene-butylene-styrene block copolymer elastomer, a styrene-isoprene-styrene block copolymer elastomer, a styrene-butadiene rubber elastomer, a maleic anhydride-modified amorphous α-olefin copolymer, a medium molecular weight polyisobutylene, and an antioxidant into the stirrer, and stirring for 20 minutes;
[0174] (2) adjusting the temperature of the mixer to 170° C. and the stirring speed to 350 rpm, and continuing to add maleic anhydride-modified C5 petroleum resin, C5 / C9 copolymerized petroleum resin and fully hydrogenated dicyclopentadiene petroleum resin into the mixer, and stirring for 30 minutes;
[0175] (3) The stirring speed of the mixer is adjusted to 150 rpm, the temperature is maintained at 180° C., and the light stabilizer and the ultraviolet absorber are continuously added to the mixer, and stirred for 35 minutes to obtain a hot melt pressure-sensitive adhesive.
[0176] The preparation method of the isolation sand mainly comprises the following steps performed in sequence:
[0177] (1) Preparation of composite infiltration crystals
[0178] The potassium silicate, calcium hydroxide, benzalkonium bromide, thiosulfate, citrate and calcium lactate are uniformly mixed to obtain composite osmotic crystals;
[0179] (2) mixing acrylic emulsion, water, composite infiltration crystal, silane coupling agent, color powder and ordinary Portland cement to obtain slurry;
[0180] (3) starting the mixer and adjusting the stirring speed to 60 rpm, wetting the surface of the calcium carbonate mineral particles and putting them into the mixer, then slowly adding the slurry obtained in step 2 into the mixer and stirring until uniform to obtain particles coated with the slurry;
[0181] (4) The particles coated with the slurry obtained in step 3 are taken out, sieved and graded, and dried at 85° C. until completely dry, thereby obtaining the isolation sand to be prepared.
[0182] The sieving and grading in step 4 includes the following steps performed in sequence: the particles wrapped with the slurry are sieved through a 40-50 mesh sieve, a 60-70 mesh sieve and an 80 mesh sieve respectively, and then the three are mixed in a ratio of 68%, 30% and 2% by weight.
[0183] Example 3
[0184] like Figure 1-2 As shown, the self-adhesive polymer pre-laid waterproofing membrane described in the present invention comprises an isolation sand layer 1, an isolation film layer 2, a hot melt pressure-sensitive adhesive layer 3, a substrate 4, a hot melt pressure-sensitive adhesive layer 3 and an isolation film layer 2 stacked in sequence from top to bottom, wherein the substrate 4 comprises a modified emulsion layer 4-1, a co-extruded additional layer 4-2, a main material layer 4-3, a co-extruded additional layer 4-2 and a modified emulsion layer 4-1 stacked in sequence from top to bottom, and the pressure-sensitive adhesive layer is a hot melt pressure-sensitive adhesive; the isolation sand layer 1 is made of isolation sand;
[0185] The co-extruded additional layer 4-2 is mainly prepared from the following components in the following weight ratios:
[0186]
[0187] The main material layer 4-3 is mainly prepared from the following components in the following weight ratios:
[0188]
[0189]
[0190] The modified emulsion layer 4-1 adopts a silane coupling agent modified emulsion, and the silane coupling agent modified emulsion is mainly prepared from the following components in the following weight ratios:
[0191] 11 parts of nano-TiO2 dispersion solution,
[0192] Silane coupling agent solution 9 parts,
[0193] Emulsion 52 parts;
[0194] The mass concentration of the silane coupling agent in the silane coupling agent solution is 30%, the mass concentration of the nano-TiO2 in the nano-TiO2 dispersion solution is 0.05%, and the emulsion is any combination of acrylic emulsion, methyl methacrylate emulsion and methacrylic acid emulsion.
[0195] The hot melt pressure sensitive adhesive is mainly prepared from the following components in the following weight ratios:
[0196]
[0197] The diblock content of the styrene-isoprene-styrene block copolymer elastomer is 50%.
[0198] The isolation sand is mainly prepared from the following components in the following weight ratios:
[0199]
[0200]
[0201] The composite osmotic crystal is mainly prepared from the following components in the following weight ratios:
[0202]
[0203] The isolation sand is composed of isolation sand with a particle size of 40-50 meshes, isolation sand with a particle size of 60-70 meshes and isolation sand with a particle size of 80 meshes, and the weight percentages thereof are 70±2%, 25±5% and 2-8% respectively.
[0204] The silane coupling agent is any combination of an alkyl silane coupling agent, an aromatic silane coupling agent, vinyl triethoxysilane, vinyl trimethoxysilane and vinyl tri-β-methylethoxysilane; the isolation film layer 2 is a release film with a PE substrate 4 and a release agent applied on one side.
[0205] The thickness of the modified emulsion layer 4-1 is 0.10 mm, the thickness of the co-extruded additional layer 4-2 is 0.08 mm, the thickness of the hot-melt pressure-sensitive adhesive layer 3 is 00.3 mm, and the thickness of the isolation film layer 2 is 0.03 mm.
[0206] The method for preparing the self-adhesive polymer pre-laid waterproofing membrane mainly comprises the following steps performed in sequence:
[0207] (I) Preparation of substrate 4
[0208] (1) Preparation of main material layer 4-3 particles
[0209] The production temperature of the twin-screw extruder is set at 200°C, high-density polyethylene, linear low-density polyethylene, polypropylene, thermoplastic elastomer, maleic anhydride grafted polyethylene, titanium dioxide and antioxidant are fed into the first feeding port of the twin-screw extruder, and heavy calcium carbonate is fed into the second feeding port of the twin-screw extruder, and the main material layer 4-3 particles are obtained by discharging the materials;
[0210] (2) Preparation of co-extruded additional layer 4-2 particles
[0211] The production temperature of the single-screw extruder is set at 200°C, and high-density polyethylene, styrene-isoprene-styrene block copolymer elastomer, polypropylene, maleic anhydride grafted polyethylene, titanium dioxide and antioxidant are fed into the feeding port of the single-screw extruder, and the co-extruded additional layer 4-2 particles are obtained by discharging the materials;
[0212] (3) Preparation of silane coupling agent modified emulsion
[0213] ① Slowly drip a silane coupling agent solution with a silane coupling agent mass concentration of 30% into a nano-TiO2 dispersion solution with a nano-TiO2 mass concentration of 0.05% at a pH value of 3-5, disperse evenly, adjust the pH value to 10, and then dry and grind until there are no obvious particles to obtain TiO2 modified by a silane coupling agent;
[0214] ② Add the TiO2 modified with the silane coupling agent obtained in step ① into the emulsion, and stir at 1000 rpm for 20 minutes to obtain a silane coupling agent modified emulsion;
[0215] (4) Preparation of substrate 4
[0216] ① The co-extruded additional layer particles and the main material layer particles are put into a screw extruder together, and the co-extruded additional layer, the main material layer and the co-extruded additional layer are extruded from the upper die port, the middle die port and the lower die port at 200°C respectively, and then three rollers are used for extrusion and lamination to obtain a laminated coil with the co-extruded additional layer 4-2 sandwiching the main material layer 4-3;
[0217] ② After the laminated coil is cooled and shaped, the silane coupling agent modified emulsion is sprayed on the upper and lower surfaces of the laminated coil respectively, and then dried at 90° C. to obtain a modified emulsion layer 4-1, that is, a substrate 4 is obtained;
[0218] (II) Preparation of self-adhesive polymer pre-laid waterproof membrane
[0219] A hot-melt pressure-sensitive adhesive melting at 180° C. is coated on the upper and lower surfaces of a substrate 4 to obtain a hot-melt pressure-sensitive adhesive layer 3, and then isolation films are respectively covered on the outer surfaces of the two hot-melt pressure-sensitive adhesive layers 3 to obtain an isolation film layer 2, and then isolation sand is fully spread on the outer surface of the isolation film layer 2 located above the substrate 4 to obtain an isolation sand layer 1.
[0220] The preparation method of the hot melt pressure sensitive adhesive mainly comprises the following steps performed in sequence:
[0221] (1) starting a stirrer, adjusting the temperature to 170° C. and the stirring speed to 150 rpm, adding a styrene-ethylene-butylene-styrene block copolymer elastomer, a styrene-isoprene-styrene block copolymer elastomer, a styrene-butadiene rubber elastomer, a maleic anhydride-modified amorphous α-olefin copolymer, a medium molecular weight polyisobutylene, and an antioxidant into the stirrer, and stirring for 30 minutes;
[0222] (2) adjusting the temperature of the mixer to 180° C. and the stirring speed to 250 rpm, and continuing to add maleic anhydride-modified C5 petroleum resin, C5 / C9 copolymerized petroleum resin and fully hydrogenated dicyclopentadiene petroleum resin into the mixer, and stirring for 40 minutes;
[0223] (3) The stirring speed of the mixer is adjusted to 250 rpm, the temperature is maintained at 170° C., and the light stabilizer and the ultraviolet absorber are continuously added to the mixer, and stirred for 40 minutes to obtain a hot melt pressure-sensitive adhesive.
[0224] The preparation method of the isolation sand mainly comprises the following steps performed in sequence:
[0225] (1) Preparation of composite infiltration crystals
[0226] The sodium silicate, calcium hydroxide, benzalkonium bromide, thiosulfate, citrate and calcium lactate are uniformly mixed to obtain composite osmotic crystals;
[0227] (2) mixing acrylic emulsion, water, composite infiltration crystal, silane coupling agent, color powder and ordinary Portland cement to obtain slurry;
[0228] (3) starting the mixer and adjusting the stirring speed to 100 rpm, wetting the surface of the calcium carbonate mineral particles and putting them into the mixer, then slowly adding the slurry obtained in step 2 into the mixer and stirring until uniform to obtain particles coated with the slurry;
[0229] (4) The particles coated with the slurry obtained in step 3 are taken out, sieved and graded, and dried at 75° C. until completely dry, thereby obtaining the isolation sand to be prepared.
[0230] The sieving and grading in step 4 includes the following steps in sequence: the particles wrapped with the slurry are sieved through a 40-50 mesh sieve, a 60-70 mesh sieve and an 80 mesh sieve respectively, and then the three are mixed in a weight percentage ratio of 70±2%, 25±5% and 2-8%.
[0231] Raw material information involved in this case:
[0232] Medium molecular weight polyisobutylene: Korea Dalin PB950
[0233] Antioxidant: BASF B225
[0234] Experimental data:
[0235] Comparative Example 1
[0236] The difference between this case and Example 1 is that the structure on the substrate is different, and the substrate is only a single-layer main material layer.
[0237] Comparative Example 2
[0238] The differences between this case and Example 1 are: ① The structure on the substrate is different, and the substrate is only a single-layer main material layer; ② Both the upper pressure-sensitive adhesive layer and the lower pressure-sensitive adhesive layer use existing commercially available hot-melt pressure-sensitive adhesive.
[0239] Comparative Example 3
[0240] The difference between this case and implementation case 1 is that the structure on the substrate is different and there is no modified emulsion layer in the substrate.
[0241] Comparative Example 4
[0242] The difference between this case and implementation case 1 is that the structure on the substrate is different and there is no coextruded additional layer in the substrate.
[0243] Detection method:
[0244] The test was carried out in accordance with the requirements of the national standard GB / T 23457-2017. The main test items were dimensional change rate, peeling strength between untreated and post-cast concrete, and peeling strength between heat-treated and post-cast concrete.
[0245] Test results:
[0246] Table 1 Test results of performance parameters of each sample
[0247]
[0248] From the comparison of various performance data in the above table, we can see that:
[0249] ① The introduction of the modified emulsion layer and the co-extruded additional layer has a certain effect on preventing the migration of low molecular weight substances in the hot melt pressure sensitive adhesive system of the two hot melt pressure sensitive adhesive layers;
[0250] ② The modified latex layer is better than the co-extruded additional layer in preventing the migration of low molecular weight substances;
[0251] ③ From the comparison data of Comparative Example 1 and Comparative Example 2, it can be seen that the preferred hot-melt pressure-sensitive adhesive layer system of the present application can alleviate the negative impact caused by the migration of low molecular weight substances to a certain extent.
Claims
1. A self-adhesive polymer pre-laid waterproof membrane, characterized by: The invention comprises an isolation sand layer (1), an isolation film layer (2), a hot melt pressure sensitive adhesive layer (3), a substrate (4), a hot melt pressure sensitive adhesive layer (3) and an isolation film layer (2) stacked in sequence from top to bottom, wherein the substrate (4) comprises a modified emulsion layer (4-1), a co-extruded additional layer (4-2), a main material layer (4-3), a co-extruded additional layer (4-2) and a modified emulsion layer (4-1) stacked in sequence from top to bottom, and the pressure sensitive adhesive layer is a hot melt pressure sensitive adhesive; the isolation sand layer (1) is made of isolation sand; The co-extruded additional layer (4-2) is mainly prepared from the following components in the following weight ratios: The main material layer (4-3) is mainly prepared from the following components in the following weight ratios: The modified emulsion layer (4-1) adopts a silane coupling agent modified emulsion, which is mainly prepared from the following components in the following weight ratios: 9-11 parts of nano-TiO2 dispersion solution, 9-11 parts of silane coupling agent solution, 48-52 parts of emulsion; The mass concentration of the silane coupling agent in the silane coupling agent solution is 20-30%, the mass concentration of the nano-TiO2 in the nano-TiO2 dispersion solution is 0.05-0.1%, and the emulsion is one of acrylic emulsion, methyl methacrylate emulsion or methacrylic acid emulsion or any combination of any two or more thereof.
2. The self-adhesive polymer pre-laid waterproof membrane according to claim 1, characterized in that: The hot melt pressure sensitive adhesive is mainly prepared from the following components in the following weight ratios: The diblock content of the styrene-isoprene-styrene block copolymer elastomer is 50%.
3. The self-adhesive polymer pre-laid waterproof membrane according to claim 1, characterized in that: The isolation sand is mainly prepared from the following components in the following weight ratios: The composite osmotic crystallization is mainly prepared from the following components in the following weight ratios:
4. The self-adhesive polymer pre-laid waterproof membrane according to claim 3, characterized in that: The isolation sand is composed of isolation sand with a particle size of 40-50 meshes, isolation sand with a particle size of 60-70 meshes and isolation sand with a particle size of 80 meshes, and the weight percentages thereof are 70±2%, 25±5% and 2-8% respectively.
5. The self-adhesive polymer pre-laid waterproof membrane according to claim 1, characterized in that: The silane coupling agent is one of an alkyl silane coupling agent, an aromatic silane coupling agent, vinyl triethoxysilane, vinyl trimethoxysilane or vinyl tri-β-methylethoxysilane, or any combination of any two or more thereof; the isolation film layer (2) adopts a release film with a PE substrate (4) and a release agent applied on one side.
6. The self-adhesive polymer pre-laid waterproof membrane according to claim 1, characterized in that: The thickness of the modified emulsion layer (4-1) is 0.06-0.10 mm, the thickness of the co-extruded additional layer (4-2) is 0.08-0.12 mm, the thickness of the hot melt pressure sensitive adhesive layer (3) is 0.27-0.3 mm, and the thickness of the isolation film layer (2) is 0.03-0.04 mm.
7. The method for preparing the self-adhesive polymer pre-laid waterproof membrane according to any one of claims 1 to 6, characterized in that: It mainly includes the following steps in order: (1) Preparation of substrate (1) Preparation of main material layer particles The production temperature of the twin-screw extruder is set at 180-200°C, and high-density polyethylene, linear low-density polyethylene, polypropylene, thermoplastic elastomer, maleic anhydride grafted polyethylene, titanium dioxide and antioxidant are added to the first feeding port of the twin-screw extruder, and heavy calcium carbonate is added to the second feeding port of the twin-screw extruder. The main material layer particles are obtained by discharging the materials; (2) Preparation of co-extruded additional layer particles The production temperature of the single-screw extruder is set at 180-200°C, and high-density polyethylene, styrene-isoprene-styrene block copolymer elastomer, polypropylene, maleic anhydride grafted polyethylene, titanium dioxide and antioxidant are fed into the feeding port of the single-screw extruder, and the co-extruded additional layer particles are obtained upon discharge; (3) Preparation of silane coupling agent modified emulsion ① Slowly drip a silane coupling agent solution with a silane coupling agent mass concentration of 20-30% into a nano-TiO2 dispersion solution with a nano-TiO2 mass concentration of 0.05-0.1% at a pH value of 3-5, disperse evenly, then adjust the pH value to 9-10, and then dry and grind until there are no obvious particles to obtain silane coupling agent-modified TiO2; ② Add the silane coupling agent-modified TiO2 obtained in step ① to the emulsion and stir at 800-1000 rpm for 20-30 minutes to obtain a silane coupling agent-modified emulsion; (4) Preparation of substrate ① The co-extruded additional layer particles and the main material layer particles are fed into a screw extruder together, and the co-extruded additional layer, the main material layer and the co-extruded additional layer are extruded simultaneously from the upper die port, the middle die port and the lower die port at 180-200° C., and then three rollers are used for extrusion and lamination to obtain a laminated coil with the co-extruded additional layer (4-2) sandwiching the main material layer (4-3); ② After the laminated coil is cooled and shaped, the silane coupling agent modified emulsion is sprayed on the upper and lower surfaces of the laminated coil respectively, and then dried at 60-90° C. to obtain a modified emulsion layer (4-1), thereby obtaining a substrate (4); (2) Preparation of self-adhesive polymer pre-laid waterproof membrane Hot melt pressure sensitive adhesive melted at 150-180° C. is coated on the upper and lower surfaces of a substrate (4) to obtain a hot melt pressure sensitive adhesive layer (3), and then an isolation film is coated on the outer surfaces of the two hot melt pressure sensitive adhesive layers (3) to obtain an isolation film layer (2). After that, isolation sand is spread on the outer surface of the isolation film layer (2) located above the substrate (4) to obtain an isolation sand layer (1).
8. The method for preparing the self-adhesive polymer pre-laid waterproof membrane according to claim 7, characterized in that: The preparation method of the hot melt pressure sensitive adhesive mainly includes the following steps performed in sequence: (1) starting a mixer, adjusting the temperature to 160-170° C., adjusting the stirring speed to 150-250 rpm, adding a styrene-ethylene-butylene-styrene block copolymer elastomer, a styrene-isoprene-styrene block copolymer elastomer, a styrene-butadiene rubber elastomer, a maleic anhydride-modified amorphous α-olefin copolymer, a medium molecular weight polyisobutylene, and an antioxidant into the mixer, and stirring for 20-30 minutes; (2) Adjust the mixer temperature to 170-180°C and the stirring speed to 250-350 rpm, continue to add maleic anhydride modified C5 petroleum resin, C5 / C9 copolymerized petroleum resin and fully hydrogenated dicyclopentadiene petroleum resin into the mixer, and stir for 30-40 minutes; (3) Adjust the stirring speed of the mixer to 150-250 rpm, maintain the temperature at 170-180° C., continue to add the light stabilizer and the ultraviolet absorber into the mixer, and stir for at least 30 minutes to obtain the hot melt pressure-sensitive adhesive.
9. The method for preparing the self-adhesive polymer pre-laid waterproof membrane according to claim 7, characterized in that: The preparation method of the isolation sand mainly includes the following steps performed in sequence: (1) Preparation of composite infiltration crystallization Sodium silicate or potassium silicate, calcium hydroxide or sodium hydroxide, benzalkonium bromide, thiosulfate, citrate and calcium lactate are mixed evenly to obtain composite osmotic crystals; (2) uniformly mixing acrylic emulsion, water, composite infiltration crystallization, silane coupling agent, color powder and ordinary Portland cement to obtain a slurry; (3) starting the mixer and adjusting the stirring speed to 60-100 rpm, wetting the surface of the calcium carbonate mineral particles and then putting them into the mixer, then slowly adding the slurry obtained in step (2) into the mixer and stirring until uniform to obtain particles coated with the slurry; (4) The slurry-coated particles obtained in step (3) are taken out, sieved and graded, and dried at 75-85° C. until completely dry, thereby obtaining the isolation sand to be prepared.
10. The self-adhesive polymer pre-laid waterproof membrane according to claim 9, characterized in that: The sieving and grading in step (4) includes the following steps performed in sequence: the particles coated with the slurry are sieved through a 40-50 mesh sieve, a 60-70 mesh sieve, and an 80 mesh sieve respectively, and then the three are mixed in a ratio of 70±2%, 25±5%, and 2-8% by weight.