Cation-doped nickel phosphide difunctional self-supporting electrode material, and preparation method and application thereof

Through the preparation of cationically doped nickel phosphide electrode materials, the synergistic effect of porous structure and non-precious metal elements is used to solve the problem of insufficient conductivity and catalytic activity of nickel phosphide electrode materials, and the low-cost and efficient electrochemical performance improvement is achieved , suitable for electrochemical oxygen production, hydrogen production and total water dissolution reactions.

CN118910664APending Publication Date: 2024-11-08XI AN JIAOTONG UNIV

Patent Information

Application Number
CN202411031144.3
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-07-30
Publication Date
2024-11-08

AI Technical Summary

Technical Problem

The existing nickel phosphide electrode materials have problems of insufficient conductivity and catalytic activity in electrochemical water decomposition, especially in electrochemical oxygen production and hydrogen production reactions, which lead to higher energy consumption and higher cost.

Method used

The cation-doped nickel hydroxide was prepared by immersing the foam nickel nitrate, hydrated ferric nitrate, vanadium chloride and urea in a deionized aqueous solution to form cationically doped nickel hydroxide, and then undergoing a phosphating reaction. Nickel phosphide dual-function self-supporting electrode material, which uses the synergistic effect of porous structure and non-precious metal elements to improve electrochemical performance.

Benefits of technology

It has achieved the improvement of electrochemical activity and conductivity at low cost, reduced energy consumption, and significantly improved the performance of electrochemical oxygen production, hydrogen production and full water dissolution. It has reduced overpotential and increased current density during electrochemical reactions. Broad application prospects.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118910664A_ABST
    Figure CN118910664A_ABST
Patent Text Reader

Abstract

The invention relates to a cation-doped nickel phosphide difunctional self-supporting electrode material and a preparation method application of the material, and the preparation method comprises the following steps: immersing foamed nickel into a deionized water solution containing nickel nitrate hydrate, ferric nitrate hydrate, vanadium chloride, urea and ammonium fluoride, carrying out a hydrothermal reaction, cooling, cleaning and drying to obtain cation-doped nickel hydroxide; the obtained cation-doped nickel hydroxide is placed at the downstream of a tubular furnace, sodium hypophosphite hydrate (NaH2PO2.H2O) is arranged at the upstream of the tubular furnace, a phosphating reaction is conducted, cooling is conducted to the room temperature, the product is taken out, and the cation-doped nickel phosphide difunctional self-supporting electrode material is obtained; the electrode material prepared by the invention can be used for electrochemical oxygen production (OER), electrochemical hydrogen production (HER) or electrochemical full water splitting (OWS) reaction in an alkaline environment, and has excellent performance; according to the invention, a synergistic effect is generated through cation-doped nickel phosphide, the electronic structure of the catalyst is optimized, the conductivity of the catalyst is enhanced, and the electron transfer rate is accelerated, so that the electrochemical performance is greatly improved, the effect of reducing energy consumption is achieved, and the preparation method has huge development prospect and application potential.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention belongs to the technical field of preparation of non-noble metal phosphide nanomaterials and dual-function water electrolysis, and relates to a cation-doped nickel phosphide dual-function self-supporting electrode material, a preparation method of the material and application. Background Art

[0002] Against the backdrop of global energy structure transformation and rising demand for clean energy, electrochemical water splitting technology, that is, producing hydrogen and oxygen through the electrolysis of water, has become an efficient way of energy conversion. As a clean energy carrier, the green and efficient production of hydrogen is the key to achieving carbon peak and carbon neutrality goals. Among them, non-precious metal electrode materials play a core role in electrochemical hydrogen and oxygen production technologies, which not only promotes the innovation of energy technology, but also reduces costs by reducing dependence on precious metals, and enhances energy security and environmental sustainability. The research on non-precious metal electrode materials mainly focuses on transition metal oxides, sulfides, nitrides and phosphides. These materials have become a hot topic of research due to their low cost, abundant resources and environmental friendliness. Among them, transition metal phosphides, especially nickel phosphide (Ni2P), have excellent electrochemical performance due to their good electrical conductivity, unique electronic structure and chemical stability. In recent years, they have attracted extensive attention in the field of electrochemical water splitting, especially in electrochemical oxygen production (OER) and electrochemical hydrogen production (HER) reactions.

[0003] By constructing heterogeneous structures, surface modification, element doping and other optimization strategies for nickel phosphide (Ni2P), its nanostructure can be precisely controlled, thereby further improving its electrochemical catalytic performance in alkaline and neutral media. For example, the patent application with application number CN201710414816.2 provides a NiFeP bifunctional transition metal phosphide catalyst and its preparation and use. The invented NiFeP bifunctional transition metal phosphide was tested for complete water splitting in an alkaline environment (1M potassium hydroxide, pH = 14). When the current density was 1010mA·cm -2When the NiFeP nanosheet electrode is at 1.55 volts relative to the standard electrode, the potential is 1.55 volts. The patent application with application number CN201711348778.1 provides a ternary nickel iron phosphide nanosheet, a preparation method thereof and the use of electrolyzed water, wherein the invented ternary nickel iron phosphide nanosheet is applied to electrochemical hydrogen evolution, and an electrochemical test is carried out in a 1M KOH solution. When the current density reaches 10mA / cm2, its overpotential is 151mV. However, compared with single element doping, co-doping of multiple metal elements has greater advantages. It can not only produce synergistic effects at the atomic scale, optimize the electronic structure of the catalyst, adjust the conductivity of the catalyst, and accelerate the electron transfer rate, but also increase the number and diversity of catalytic active sites, provide more reaction paths, reduce the reaction energy barrier, and ultimately achieve the effect of reducing energy consumption. Summary of the invention

[0004] In order to overcome the defects of the above-mentioned prior art, the purpose of the present invention is to provide a cation-doped nickel phosphide bifunctional self-supporting electrode material, a method for preparing the material and an application thereof, wherein the foamed nickel is immersed in a deionized water solution containing hydrated nickel nitrate, hydrated ferric nitrate, vanadium chloride, urea and ammonium fluoride, a hydrothermal reaction is carried out, and the material is cleaned and dried after cooling to obtain cation-doped nickel hydroxide; the obtained cation-doped nickel hydroxide is placed downstream of a tubular furnace, and hydrated sodium hypophosphite (NaH2PO2·H2O) is placed upstream to carry out a phosphating reaction, and the material is cooled to room temperature and taken out to obtain a cation-doped nickel phosphide bifunctional self-supporting electrode material; the cation-doped nickel phosphide bifunctional self-supporting electrode material prepared by the method has excellent electrochemical oxygen production (OER), electrochemical hydrogen production (HER) and electrochemical overall water splitting (OWS) performance, and has stable electrochemical properties and has broad application prospects.

[0005] To achieve the above object, the technical solution adopted by the present invention is as follows:

[0006] A cation-doped nickel phosphide bifunctional self-supporting electrode material comprises a nickel foam substrate and an attachment material on the surface of the nickel foam substrate; the attachment material comprises, by weight, the following:

[0007] Hydrated nickel nitrate, 1-2 parts;

[0008] Hydrated ferric nitrate, 0-1 part;

[0009] Vanadium chloride, 0-1 part;

[0010] Hydrated sodium hypophosphite (NaH2PO2·H2O), 6 to 8 parts.

[0011] The thickness of the nickel foam is 2.0 mm to 3.0 mm.

[0012] A method for preparing a cation-doped nickel phosphide bifunctional self-supporting electrode material comprises the following steps:

[0013] Step 1), cutting nickel foam with a thickness of 2.0 mm to 3.0 mm, and pretreating the cut nickel foam;

[0014] Step 2), immersing the nickel foam pretreated in step 1) in a deionized water solution containing 2.4-4.8 mmol of hydrated nickel nitrate, 0-2.4 mmol of hydrated iron nitrate, 0-2.4 mmol of vanadium chloride, 4-6 mmol of urea and 4-6 mmol of ammonium fluoride, hydrothermally reacting at 110-130° C. for 10-12 hours, cooling to room temperature, washing and drying to obtain cation-doped nickel hydroxide;

[0015] Step 3), placing the cation-doped nickel hydroxide obtained in step 2) downstream of a tubular furnace, with 14.4-19.2 mmol hydrated sodium hypophosphite (NaH2PO2·H2O) upstream, and performing a phosphating reaction at 300-350° C. for 1.5-2 hours. After the reaction is completed, cooling to room temperature and taking out, a cation-doped nickel phosphide bifunctional self-supporting electrode material is obtained.

[0016] The specific method of pretreating the cut nickel foam in step 1) is as follows: ultrasonically cleaning the cut nickel foam with acetone and dilute hydrochloric acid (HCl), respectively, with an ultrasonic power of 95 to 100 W and an ultrasonic time of 10 to 20 min, then ultrasonically cleaning the cut nickel foam with deionized water and anhydrous ethanol alternately for multiple times, with an ultrasonic power of 95 to 100 W and an ultrasonic time of 10 to 20 min, and finally vacuum drying at 60 to 80° C. for 8 to 10 h to obtain a pretreated nickel foam substrate.

[0017] The deionized water solution in step 2) contains 30-35 ml of deionized water.

[0018] The cleaning and drying conditions in step 2) are: ultrasonic cleaning with anhydrous ethanol and water alternately for multiple times, with an ultrasonic power of 95 to 100 W and an ultrasonic time of 10 to 20 minutes, followed by vacuum drying at 60 to 80° C. for 8 to 10 hours.

[0019] In the step 2), urea and ammonium fluoride are morphology control agents, which assist in the synthesis of electrode materials and do not participate in the reaction.

[0020] The cation-doped nickel phosphide bifunctional self-supporting electrode material prepared according to the above method is applied to electrochemical oxygen production (OER), electrochemical hydrogen production (HER) or electrochemical water splitting (OWS); and the electrolyte during the electrochemical reaction test is 1M potassium hydroxide (KOH) solution, and the test temperature is room temperature 20-30°C.

[0021] Compared with the prior art, the present invention has the following beneficial effects:

[0022] The present invention uses nickel foam as a substrate, and can prepare a cation-doped nickel phosphide bifunctional self-supporting electrode material through two steps of hydrothermal and phosphating. The microstructure of the nanoflowers loaded on the porous nickel foam greatly increases the electrochemical active area, exposes more active sites to participate in the reaction, and improves the efficiency of the catalytic reaction; and the addition of three non-precious metal elements, nickel, iron and vanadium, can not only improve the conductivity, but also coordinately adjust the electronic structure, accelerate the electron transfer process, and thus improve the kinetic performance of the electrocatalytic reaction. In terms of cost, the use of non-precious metals also has huge economic benefits, achieving the advantages of simple preparation process, convenient operation and low cost.

[0023] Due to the incorporation of iron-vanadium cations, the cation-doped nickel phosphide of the present invention improves the conductivity of the material, accelerates the electron transfer process, and at the same time increases the electrochemical active area, which also improves the catalytic efficiency, so that it obtains high electrochemical activity and low overpotential effects, and can be applied to electrochemical oxygen production (OER), electrochemical hydrogen production (HER) or electrochemical water splitting (OWS). When the material is applied to electrochemical oxygen production (OER), only an overpotential of 193mV is required to reach 10mA / cm 2 When applied to electrochemical hydrogen production (HER), only 68mV overpotential is required to reach 10mA / cm 2 When applied to electrochemical water splitting (OWS), only 1.5V external voltage is required to reach 10mA / cm 2 of current density.

[0024] In summary, the present invention has good electrochemical activity, high electrical conductivity, and excellent catalytic performance for overall water splitting. At the same time, the present invention has simple operation process, low cost, and high scalability. BRIEF DESCRIPTION OF THE DRAWINGS

[0025] Figure 1 1 is the X-ray diffraction (XRD) spectrum of the iron-vanadium cation-doped nickel phosphide bifunctional self-supporting electrode material (Fe1V1-Ni2P) obtained in the comparative example Ni2P and Example 1 of the present invention.

[0026] Figure 2 It is the ultraviolet visible absorption spectrum (UV / Vis) of the iron-vanadium cation-doped nickel phosphide bifunctional self-supporting electrode material (Fe1V1-Ni2P) obtained in the comparative example Ni2P and Example 1 of the present invention.

[0027] Figure 3 It is the full X-ray photoelectron spectrum (XPS) of the iron-vanadium cation-doped nickel phosphide bifunctional self-supporting electrode material (Fe1V1-Ni2P) obtained in the comparative example Ni2P and Example 1 of the present invention.

[0028] Figure 4a This is a low-magnification scanning electron microscope (SEM) image of the iron-vanadium cation-doped nickel phosphide bifunctional self-supporting electrode material (Fe1V1-Ni2P) obtained in Example 1 of the present invention.

[0029] Figure 4b This is a high-magnification scanning electron microscope (SEM) image of the iron-vanadium cation-doped nickel phosphide bifunctional self-supporting electrode material (Fe1V1-Ni2P) obtained in Example 1 of the present invention.

[0030] Figure 5a This is a transmission electron microscope (TEM) image of the iron-vanadium cation-doped nickel phosphide bifunctional self-supporting electrode material (Fe1V1-Ni2P) obtained in Example 1 of the present invention.

[0031] Figure 5b This is a high-resolution transmission electron microscopy (HRTEM) image of the iron-vanadium cation-doped nickel phosphide bifunctional self-supporting electrode material (Fe1V1-Ni2P) obtained in Example 1 of the present invention.

[0032] Figure 5c This is a transmission electron microscope mapping (TEM-EDX elemental mapping) of different elements of the iron-vanadium cation-doped nickel phosphide bifunctional self-supporting electrode material (Fe1V1-Ni2P) obtained in Example 1 of the present invention.

[0033] Figure 6a This is a performance diagram of electrochemical oxygen production (OER) of various cation-doped nickel phosphide bifunctional self-supporting electrode materials obtained in the present invention in an alkaline environment (the electrolyte is 1M KOH solution).

[0034] Figure 6b The graph is a performance diagram of electrochemical hydrogen production (HER) of various cation-doped nickel phosphide bifunctional self-supporting electrode materials obtained in the present invention in an alkaline environment (the electrolyte is 1M KOH solution).

[0035] Figure 6c This is a performance diagram of electrochemical water splitting (OWS) of the iron-vanadium cation-doped nickel phosphide bifunctional self-supporting electrode material (Fe1V1-Ni2P) obtained in Example 1 of the present invention in an alkaline environment (the electrolyte is 1M KOH solution). DETAILED DESCRIPTION

[0036] The present invention is now described with the following preferred embodiments, but they are not intended to limit the scope of protection of the present invention. Unless otherwise specified, the means used in the embodiments are all commonly used technical means in the art.

[0037] Example 1

[0038] A method for preparing a cation-doped nickel phosphide bifunctional self-supporting electrode material comprises the following steps:

[0039] 1) cutting nickel foam with a thickness of 3.0 mm, and then ultrasonically cleaning with acetone and 3M HCl respectively, with an ultrasonic power of 100 W for 10 min, and then ultrasonically cleaning with deionized water and anhydrous ethanol alternately for multiple times, with an ultrasonic power of 100 W and an ultrasonic time of 10 min, and finally vacuum drying at 60° C. for 8 h to obtain a pretreated nickel foam substrate;

[0040] 2) The nickel foam obtained in step 1) is immersed in a mixed solution containing 35 ml of deionized water, 2.4 mmol of hydrated nickel nitrate (Ni(NO3)2·6H2O), 1.2 mmol of hydrated iron nitrate (Fe(NO3)3·9H2O), 1.2 mmol of vanadium chloride (VCl3), 5 mmol of urea (CO(NH2)2) and 5 mmol of ammonium fluoride (NH4F), and then transferred to a high-temperature reactor for hydrothermal reaction at a constant temperature of 120°C for 12 hours. After the reaction is completed, it is cooled to room temperature, taken out and ultrasonically cleaned alternately in deionized water and anhydrous ethanol for multiple times, with an ultrasonic power of 100 W and an ultrasonic time of 10 min, and then vacuum dried at 60°C for 8 hours to obtain a nickel foam loaded with nickel-iron-vanadium hydroxide nanoflowers (Fe1V1-Ni(OH)2);

[0041] 3) The obtained nickel foam loaded with nickel iron vanadium hydroxide nanoflowers (Fe1V1-Ni(OH)2) was placed downstream of a tubular furnace, with 18.8 mmol hydrated sodium hypophosphite (NaH2PO2·H2O) upstream, and the phosphating reaction temperature was set to 350°C, the time was set to 2 h, and the heating rate was set to 5°C / min. After the reaction was completed, it was naturally cooled to room temperature to obtain an iron vanadium cation-doped nickel phosphide bifunctional self-supporting electrode material (Fe1V1-Ni2P).

[0042] Example 2

[0043] A method for preparing a cation-doped nickel phosphide bifunctional self-supporting electrode material comprises the following steps:

[0044] 1) cutting a nickel foam with a thickness of 2.0 mm, and then ultrasonically cleaning it with acetone and 3M HCl for 15 min, with an ultrasonic power of 95 W, and then ultrasonically cleaning it with deionized water and anhydrous ethanol alternately for multiple times, with an ultrasonic power of 95 W and an ultrasonic time of 15 min, and finally vacuum drying at 70° C. for 9 h to obtain a pretreated nickel foam substrate;

[0045] 2) The nickel foam obtained in step 1) is immersed in a mixed solution containing 35 ml of deionized water, 2.4 mmol of hydrated nickel nitrate (Ni(NO3)2·6H2O), 1.6 mmol of hydrated iron nitrate (Fe(NO3)3·9H2O), 0.8 mmol of vanadium chloride (VCl3), 5 mmol of urea (CO(NH2)2) and 5 mmol of ammonium fluoride (NH4F), and then transferred to a high-temperature reactor for hydrothermal reaction at a constant temperature of 110°C for 10 hours. After the reaction is completed, it is cooled to room temperature, taken out and ultrasonically cleaned alternately in deionized water and anhydrous ethanol for multiple times, with an ultrasonic power of 95 W and an ultrasonic time of 15 min, and vacuum dried at 70°C for 9 hours to obtain a nickel foam loaded with nickel-iron-vanadium hydroxide nanoflowers (Fe2V1-Ni(OH)2);

[0046] 3) The obtained nickel foam loaded with nickel iron vanadium hydroxide nanoflowers (Fe2V1-Ni(OH)2) was placed downstream of a tubular furnace, with 18.8 mmol hydrated sodium hypophosphite (NaH2PO2·H2O) upstream, and the phosphating reaction temperature was set to 300°C, the time was 1.5 h, the heating rate was 3°C / min, and after the reaction was completed, it was naturally cooled to room temperature to obtain an iron vanadium cation-doped nickel phosphide bifunctional self-supporting electrode material (Fe2V1-Ni2P).

[0047] Example 3

[0048] A method for preparing a cation-doped nickel phosphide bifunctional self-supporting electrode material comprises the following steps:

[0049] 1) cutting a nickel foam with a thickness of 3.0 mm, and then ultrasonically cleaning it with acetone and 3M HCl for 20 min, with an ultrasonic power of 100 W, and then ultrasonically cleaning it with deionized water and anhydrous ethanol alternately for multiple times, with an ultrasonic power of 100 W and an ultrasonic time of 20 min, and finally vacuum drying it at 60° C. for 8 h to obtain a pretreated nickel foam substrate;

[0050] 2) The nickel foam obtained in step 1) is immersed in a mixed solution containing 35 ml of deionized water, 2.4 mmol of hydrated nickel nitrate (Ni(NO3)2·6H2O), 0.8 mmol of hydrated iron nitrate (Fe(NO3)3·9H2O), 1.6 mmol of vanadium chloride (VCl3), 5 mmol of urea (CO(NH2)2) and 5 mmol of ammonium fluoride (NH4F), and then transferred to a high-temperature reactor for hydrothermal reaction at a constant temperature of 130°C for 11 hours. After the reaction is completed, it is cooled to room temperature, taken out and ultrasonically cleaned alternately in water and ethanol for multiple times, with an ultrasonic power of 100 W and an ultrasonic time of 20 min, and vacuum dried at 70°C for 9 hours to obtain a nickel foam loaded with nickel-iron-vanadium hydroxide nanoflowers (Fe1V2-Ni(OH)2);

[0051] 3) The obtained nickel foam loaded with nickel iron vanadium hydroxide nanoflowers (Fe1V2-Ni(OH)2) was placed downstream of a tubular furnace, with 18.8 mmol hydrated sodium hypophosphite (NaH2PO2·H2O) upstream, and the phosphating reaction temperature was set to 320°C, the time was 1 h, and the heating rate was 4°C / min. After the reaction was completed, it was naturally cooled to room temperature to obtain an iron vanadium cation-doped nickel phosphide bifunctional self-supporting electrode material (Fe1V2-Ni2P).

[0052] Example 4

[0053] A method for preparing a cation-doped nickel phosphide bifunctional self-supporting electrode material comprises the following steps:

[0054] 1) cutting a nickel foam with a thickness of 2.5 mm, and then ultrasonically cleaning it with acetone and 3M HCl for 15 min, with an ultrasonic power of 95 W, and then ultrasonically cleaning it with deionized water and anhydrous ethanol alternately for multiple times, with an ultrasonic power of 95 W and an ultrasonic time of 15 min, and finally vacuum drying at 70° C. for 9 h to obtain a pretreated nickel foam substrate;

[0055] 2) The nickel foam obtained in step 1) is immersed in a mixed solution containing 35 ml of deionized water, 2.4 mmol of hydrated nickel nitrate (Ni(NO3)2·6H2O), 2.4 mmol of hydrated iron nitrate (Fe(NO3)3·9H2O), 5 mmol of urea (CO(NH2)2) and 5 mmol of ammonium fluoride (NH4F), and then transferred to a high-temperature reactor for hydrothermal reaction at a constant temperature of 115°C for 1.2 hours. After the reaction is completed, it is cooled to room temperature, taken out and ultrasonically cleaned alternately in deionized water and anhydrous ethanol for multiple times, with an ultrasonic power of 95 W and an ultrasonic time of 15 min, and vacuum dried at 65°C for 8.5 hours to obtain a nickel foam loaded with nickel-iron hydroxide nanoflowers (Fe-Ni(OH)2);

[0056] 3) The obtained nickel foam loaded with nickel-iron hydroxide nanoflowers (Fe-Ni(OH)2) was placed downstream of a tubular furnace, with 18.8 mmol hydrated sodium hypophosphite (NaH2PO2·H2O) upstream, and the phosphating reaction temperature was set to 330°C, the time was 1.8 h, the heating rate was 4°C / min, and the reaction was naturally cooled to room temperature after completion to obtain an iron cation-doped nickel phosphide bifunctional self-supporting electrode material (Fe-Ni2P).

[0057] Example 5

[0058] A method for preparing a cation-doped nickel phosphide bifunctional self-supporting electrode material comprises the following steps:

[0059] 1) cutting a nickel foam with a thickness of 2 mm, and then ultrasonically cleaning it with acetone and 3M HCl for 10 min, with an ultrasonic power of 100 W, and then ultrasonically cleaning it with deionized water and anhydrous ethanol alternately for multiple times, with an ultrasonic power of 100 W and an ultrasonic time of 10 min, and finally vacuum drying it at 60° C. for 10 h to obtain a pretreated nickel foam substrate;

[0060] 2) The nickel foam obtained in step 1) is immersed in a mixed solution containing 35 ml of deionized water, 2.4 mmol of hydrated nickel nitrate (Ni(NO3)2·6H2O), 2.4 mmol of vanadium chloride (VCl3), 5 mmol of urea (CO(NH2)2) and 5 mmol of ammonium fluoride (NH4F), and then transferred to a high-temperature reactor for hydrothermal reaction at a constant temperature of 120°C for 10 hours. After the reaction is completed, it is cooled to room temperature, taken out and ultrasonically cleaned alternately in deionized water and anhydrous ethanol for multiple times, with an ultrasonic power of 100 W and an ultrasonic time of 10 min, and then vacuum dried at 60°C for 10 hours to obtain a nickel foam loaded with nickel-vanadium hydroxide nanoflowers (V-Ni(OH)2);

[0061] 3) The obtained nickel foam loaded with nickel vanadium hydroxide nanoflowers (V-Ni(OH)2) was placed downstream of a tubular furnace, with 18.8 mmol hydrated sodium hypophosphite (NaH2PO2·H2O) upstream, and the phosphating reaction temperature was set to 300°C, the time was set to 2 h, and the heating rate was set to 3°C / min. After the reaction was completed, it was naturally cooled to room temperature to obtain a vanadium cation-doped nickel phosphide bifunctional self-supporting electrode material (V-Ni2P).

[0062] Comparative Example 1

[0063] A method for preparing a nickel phosphide bifunctional self-supporting electrode material (Ni2P), comprising the following steps:

[0064] 1) cutting a nickel foam with a thickness of 3.0 mm, and then ultrasonically cleaning it with acetone and 3M HCl for 15 min, with an ultrasonic power of 95 W, and then ultrasonically cleaning it with deionized water and anhydrous ethanol alternately for multiple times, with an ultrasonic power of 95 W and an ultrasonic time of 15 min, and finally vacuum drying it at 70° C. for 10 h to obtain a pretreated nickel foam substrate;

[0065] 2) The nickel foam obtained in step 1) is immersed in a 50ml high-temperature reactor containing 35ml deionized water, 4.8mmol hydrated nickel nitrate (Ni(NO3)2·6H2O), 5mmol urea (CO(NH2)2) and 5mmol ammonium fluoride (NH4F) for hydrothermal reaction at a constant temperature of 120°C for 12h. After the reaction is completed, it is cooled to room temperature, taken out and ultrasonically cleaned alternately in deionized water and anhydrous ethanol for multiple times, with an ultrasonic power of 95W and an ultrasonic time of 15min, and then vacuum dried at 8°C for 8h to obtain a nickel foam loaded with nickel hydroxide nanoflowers (Ni(OH)2);

[0066] 3) The obtained nickel foam loaded with nickel hydroxide nanoflowers (Ni(OH)2) was placed downstream of a tubular furnace, with 18.8 mmol hydrated sodium hypophosphite (NaH2PO2·H2O) upstream, and the phosphating reaction temperature was set to 350°C, the time was 1.5 h, the heating rate was 5°C / min, and the reaction was naturally cooled to room temperature after completion to obtain a nickel phosphide bifunctional self-supporting electrode material (Ni2P).

[0067] The cation-doped nickel phosphide bifunctional self-supporting electrode material prepared by the present invention can be applied to electrochemical oxygen production (OER), electrochemical hydrogen production (HER) or electrochemical water splitting (OWS). The electrolyte for testing the electrochemical reaction is 1M potassium hydroxide (KOH) solution, and the test temperature is room temperature 20-30°C.

[0068] An X-ray diffractometer, an ultraviolet spectrometer, an X-ray photoelectron spectrometer, a scanning electron microscope, a transmission electron microscope, and an electrochemical workstation were used to characterize the physical structure morphology, component distribution, and electrochemical oxygen production (OER), electrochemical hydrogen production (HER), and electrochemical water splitting (OWS) performance of the iron-vanadium cation co-doped nickel phosphide bifunctional self-supporting electrode material (Fe1V1-Ni2P) prepared in Example 1.

[0069] Electrochemical experiments:

[0070] The cation-doped nickel phosphide bifunctional self-supporting electrode material prepared in the above embodiment was subjected to electrochemical tests. All electrochemical tests were performed on an Ivium electrochemical workstation, and the test parameters were as follows: the cation-doped nickel phosphide bifunctional self-supporting electrode material was used as the working electrode, the mercury / mercury oxide electrode was used as the reference electrode, the Pt electrode was used as the counter electrode for the electrochemical oxygen production (OER) test, and the carbon rod was used as the counter electrode for the electrochemical hydrogen production (HER) test. The electrolyte was 1 M potassium hydroxide (KOH) (pH 13.8) solution, and the working electrode retained a working area of ​​1x1 cm 2 . During the full hydrolysis reaction test, the reference electrode and the counter electrode were connected, and the cation-doped nickel phosphide bifunctional self-supporting electrode was used as the anode and cathode respectively, and the changes between the potential and the current were recorded by the linear scanning curve. All the tested potentials were converted to the reversible hydrogen electrode RHE and calibrated according to the following formula: E(RHE)=E(GOE)+0.0592pH+0.098V. The linear scanning voltammetry (LSV) was measured at a scan rate of 5mV / s, and all LSV values ​​were iR compensated. The results are as follows:

[0071] Figure 1The X-ray diffraction (XRD) patterns of the comparative example Ni2P and the iron-vanadium cation-doped nickel phosphide bifunctional self-supporting electrode material (Fe1V1-Ni2P) obtained in Example 1 of the present invention show that the X-ray diffraction patterns of the two are similar, proving the successful synthesis of nickel phosphide. Among them, the (111), (210) and (211) diffraction peaks of Fe1V1-Ni2P are slightly shifted to the right compared with those of Ni2P, indicating that the lattice spacing has changed due to the incorporation of Fe and V.

[0072] Figure 2 The UV / Vis absorption spectra (UV / Vis) of the Ni2P and the iron-vanadium cation-doped nickel phosphide bifunctional self-supporting electrode material (Fe1V1-Ni2P) obtained in the comparative example are shown in Example 1 of the present invention. It can be seen that Fe1V1-Ni2P and Ni2P have different band gaps. Specifically, the band gap of the modified Fe1V1-Ni2P is 1.35eV, while the band gap of the original Ni2P is 1.61eV, indicating that the co-doping modification of Fe and V reduces the band gap width, enhances the conductivity, and is conducive to the transfer of electrons.

[0073] Figure 3 The full spectrum of X-ray photoelectron spectroscopy (XPS) of the nickel phosphide bifunctional self-supporting electrode material (Fe1V1-Ni2P) doped with iron-vanadium cations obtained in the comparative example Ni2P and the present invention in Example 1. It can be seen that the characteristic peaks of 856.9eV and 874.2eV correspond to the Ni-O bond, and the characteristic peaks of 129.4eV and 130.3eV correspond to the MP bond, indicating the presence of nickel and phosphorus in Ni2P, and not only nickel and phosphorus, but also iron and vanadium in Fe1V1-Ni2P, indicating the successful incorporation of Fe and V in Fe1V1-Ni2P.

[0074] Figure 4a This is a low-magnification scanning electron microscope (SEM) image of the iron-vanadium cation-doped nickel phosphide bifunctional self-supporting electrode material (Fe1V1-Ni2P) obtained in Example 1 of the present invention. It can be seen from the figure that Fe1V1-Ni2P grows uniformly on the nickel foam substrate (NF).

[0075] Figure 4b This is a high-magnification scanning electron microscope (SEM) image of the iron-vanadium cation-doped nickel phosphide bifunctional self-supporting electrode material (Fe1V1-Ni2P) obtained in Example 1 of the present invention. It can be seen from the figure that Fe1V1-Ni2P presents a nanoflower structure formed by vertical growth and stacking of nanosheets.

[0076] Figure 5aThis is a transmission electron microscope (TEM) image of the iron-vanadium cation-doped nickel phosphide bifunctional self-supporting electrode material (Fe1V1-Ni2P) obtained in Example 1 of the present invention. It can be seen from the image that the size of the Fe1V1-Ni2P nanosheets is about 1 micron.

[0077] Figure 5b This is a high-resolution transmission electron microscopy (HRTEM) image of the iron-vanadium cation-doped nickel phosphide bifunctional self-supporting electrode material (Fe1V1-Ni2P) obtained in Example 1 of the present invention. It can be seen from the figure that the interplanar spacing of the white frame part in Fe1V1-Ni2P is 0.209, corresponding to the (111) crystal plane, and is slightly smaller than the standard interplanar spacing (0.224) of the (111) crystal plane, indicating that the incorporation of Fe and V elements causes the (111) interplanar spacing to change.

[0078] Figure 5c This is a transmission electron microscope mapping (TEM-EDX elemental mapping) of different elements of the iron-vanadium cation-doped nickel phosphide bifunctional self-supporting electrode material (Fe1V1-Ni2P) obtained in Example 1 of the present invention. It can be seen from the figure that the four elements Fe, Ni, V and P in Fe1V1-Ni2P are evenly distributed on the nanosheets, which also proves the successful incorporation of Fe and V elements.

[0079] Figure 6a The electrochemical oxygen evolution (OER) performance diagram of the various cation-doped nickel phosphide bifunctional self-supporting electrode materials obtained in the present invention in an alkaline environment (the electrolyte is 1M KOH solution). It can be seen that at a current density of 10 mA cm -2 When Fe1V1-Ni2P has a very small OER overpotential of 193 mV, which is much smaller than Ni2P at a current density of 10 mA cm -2 The overpotential at 267 mV was 2. This shows that Fe1V1-Ni2P exhibits excellent OER catalytic performance, and the introduction of Fe and V greatly improves the catalytic performance of Ni2P.

[0080] Figure 6b The electrochemical hydrogen production (HER) performance diagram of the various cation-doped nickel phosphide bifunctional self-supporting electrode materials obtained in the present invention in an alkaline environment (the electrolyte is 1M KOH solution). It can be seen that at a current density of 10 mA cm -2 When the current density is 10 mA cm, Fe1V1-Ni2P has a very small HER overpotential of 68 mV, which is much smaller than Ni2P. -2 The overpotential at 177 mV was 177 mV. This shows that Fe1V1-Ni2P exhibits excellent HER catalytic performance, and the introduction of Fe and V greatly improves the catalytic performance of Ni2P.

[0081] Figure 6c The electrochemical overall water splitting (OWS) performance diagram of the iron-vanadium cation-doped nickel phosphide bifunctional self-supporting electrode material (Fe1V1-Ni2P) obtained in Example 1 of the present invention in an alkaline environment (the electrolyte is 1M KOH solution). It can be seen that the dual-electrode overall water splitting system constructed by Fe1V1-Ni2P only requires an applied voltage of 1.5V to reach 10mAcm -2 The current density is 2.47 W, which has excellent catalytic performance for water splitting.

Claims

1. A cation-doped nickel phosphide bifunctional self-supporting electrode material, characterized in that: It includes a nickel foam substrate and an attachment material on the surface of the nickel foam substrate; the attachment material includes, by weight: Hydrated nickel nitrate, 1-2 parts; Hydrated ferric nitrate, 0-1 part; Vanadium chloride, 0-1 part; Hydrated sodium hypophosphite (NaH2PO2·H2O), 6 to 8 parts.

2. The cation-doped nickel phosphide bifunctional self-supporting electrode material according to claim 1, characterized in that: The thickness of the nickel foam substrate is 2.0 mm to 3.0 mm.

3. A method for preparing a cation-doped nickel phosphide bifunctional self-supporting electrode material according to claim 1 or 2, characterized in that: The specific steps include: Step 1), cutting nickel foam with a thickness of 2.0 mm to 3.0 mm, and pretreating the cut nickel foam; Step 2), immersing the nickel foam pretreated in step 1) in a mixed solution of deionized water containing 2.4-4.8 mmol of hydrated nickel nitrate, 0-2.4 mmol of hydrated iron nitrate, 0-2.4 mmol of vanadium chloride, 4-6 mmol of urea and 4-6 mmol of ammonium fluoride, hydrothermally reacting at 110-130° C. for 10-12 hours, cooling to room temperature, washing and drying to obtain cation-doped nickel hydroxide; Step 3), placing the cation-doped nickel hydroxide obtained in step 2) downstream of a tubular furnace, with 14.4-19.2 mmol of hydrated sodium hypophosphite (NaH2PO2·H2O) upstream, and performing a phosphating reaction at 300-350°C for 1.5-2h, with a heating rate of 3-5°C / min. After the reaction is completed, the nickel phosphide is cooled to room temperature and taken out to obtain a cation-doped nickel phosphide bifunctional self-supporting electrode material.

4. The method for preparing a cation-doped nickel phosphide bifunctional self-supporting electrode material according to claim 3, characterized in that: The specific method of pretreating the cut nickel foam in step 1) is as follows: ultrasonically cleaning the cut nickel foam with acetone and dilute hydrochloric acid (HCl), respectively, with an ultrasonic power of 95 to 100 W and an ultrasonic time of 10 to 20 min, then ultrasonically cleaning the cut nickel foam with deionized water and anhydrous ethanol alternately for multiple times, with an ultrasonic power of 95 to 100 W and an ultrasonic time of 10 to 20 min, and finally vacuum drying at 60 to 80° C. for 8 to 10 h to obtain a pretreated nickel foam substrate.

5. The method for preparing a cation-doped nickel phosphide bifunctional self-supporting electrode material according to claim 3, characterized in that: The deionized water solution in step 2) contains 30-35 ml of deionized water.

6. The method for preparing a cation-doped nickel phosphide bifunctional self-supporting electrode material according to claim 3, characterized in that: The cleaning and drying conditions in step 2) are: ultrasonic cleaning with anhydrous ethanol and deionized water alternately for multiple times, with an ultrasonic power of 95 to 100 W and an ultrasonic time of 10 to 20 minutes, followed by vacuum drying at 60 to 80° C. for 8 to 10 hours.

7. A cation-doped nickel phosphide bifunctional self-supporting electrode material according to any one of claims 1 to 7 is applied to electrochemical oxygen production (OER), electrochemical hydrogen production (HER) or electrochemical water splitting (OWS); and the electrolyte during the electrochemical reaction test is 1M potassium hydroxide (KOH) solution, and the test temperature is room temperature 20-30°C.

8. A method for preparing a cation-doped nickel phosphide bifunctional self-supporting electrode material, characterized in that: The following steps are involved: 1) cutting nickel foam with a thickness of 3.0 mm, and then ultrasonically cleaning with acetone and 3M HCl respectively, with an ultrasonic power of 100 W for 10 min, and then ultrasonically cleaning with deionized water and anhydrous ethanol alternately for multiple times, with an ultrasonic power of 100 W and an ultrasonic time of 10 min, and finally vacuum drying at 60° C. for 8 h to obtain a pretreated nickel foam substrate; 2) The nickel foam obtained in step 1) is immersed in a mixed solution containing 35 ml of deionized water, 2.4 mmol of hydrated nickel nitrate (Ni(NO3)2·6H2O), 1.2 mmol of hydrated iron nitrate (Fe(NO3)3·9H2O), 1.2 mmol of vanadium chloride (VCl3), 5 mmol of urea (CO(NH2)2) and 5 mmol of ammonium fluoride (NH4F), and then transferred to a high-temperature reactor for hydrothermal reaction at a constant temperature of 120°C for 12 hours. After the reaction is completed, it is cooled to room temperature, taken out and ultrasonically cleaned alternately in deionized water and anhydrous ethanol for multiple times, with an ultrasonic power of 100 W and an ultrasonic time of 10 min, and then vacuum dried at 60°C for 8 hours to obtain a nickel foam loaded with nickel-iron-vanadium hydroxide nanoflowers (Fe1V1-Ni(OH)2); 3) The obtained nickel foam loaded with nickel iron vanadium hydroxide nanoflowers (Fe1V1-Ni(OH)2) was placed downstream of a tubular furnace, with 18.8 mmol hydrated sodium hypophosphite (NaH2PO2·H2O) upstream, and the phosphating reaction temperature was set to 350°C, the time was set to 2 h, and the heating rate was set to 5°C / min. After the reaction was completed, it was naturally cooled to room temperature to obtain an iron vanadium cation-doped nickel phosphide bifunctional self-supporting electrode material (Fe1V1-Ni2P).

9. A method for preparing a cation-doped nickel phosphide bifunctional self-supporting electrode material, characterized in that: The following steps are involved: 1) cutting a nickel foam with a thickness of 2.0 mm, and then ultrasonically cleaning it with acetone and 3M HCl for 15 min, with an ultrasonic power of 95 W, and then ultrasonically cleaning it with deionized water and anhydrous ethanol alternately for multiple times, with an ultrasonic power of 95 W and an ultrasonic time of 15 min, and finally vacuum drying at 70° C. for 9 h to obtain a pretreated nickel foam substrate; 2) The nickel foam obtained in step 1) is immersed in a mixed solution containing 35 ml of deionized water, 2.4 mmol of hydrated nickel nitrate (Ni(NO3)2·6H2O), 1.6 mmol of hydrated iron nitrate (Fe(NO3)3·9H2O), 0.8 mmol of vanadium chloride (VCl3), 5 mmol of urea (CO(NH2)2) and 5 mmol of ammonium fluoride (NH4F), and then transferred to a high-temperature reactor for hydrothermal reaction at a constant temperature of 110°C for 10 hours. After the reaction is completed, it is cooled to room temperature, taken out and ultrasonically cleaned alternately in deionized water and anhydrous ethanol for multiple times, with an ultrasonic power of 95 W and an ultrasonic time of 15 min, and vacuum dried at 70°C for 9 hours to obtain a nickel foam loaded with nickel-iron-vanadium hydroxide nanoflowers (Fe2V1-Ni(OH)2); 3) The obtained nickel foam loaded with nickel iron vanadium hydroxide nanoflowers (Fe1V1-Ni(OH)2) was placed downstream of a tubular furnace, with 18.8 mmol hydrated sodium hypophosphite (NaH2PO2·H2O) upstream, and the phosphating reaction temperature was set to 300°C, the time was 1.5 h, the heating rate was 3°C / min, and after the reaction was completed, it was naturally cooled to room temperature to obtain an iron vanadium cation-doped nickel phosphide bifunctional self-supporting electrode material (Fe1V1-Ni2P).

10. A method for preparing a cation-doped nickel phosphide bifunctional self-supporting electrode material, characterized in that: The following steps are involved: 1) cutting a nickel foam with a thickness of 3.0 mm, and then ultrasonically cleaning it with acetone and 3M HCl for 20 min, with an ultrasonic power of 100 W, and then ultrasonically cleaning it with deionized water and anhydrous ethanol alternately for multiple times, with an ultrasonic power of 100 W and an ultrasonic time of 20 min, and finally vacuum drying it at 60° C. for 8 h to obtain a pretreated nickel foam substrate; 2) The nickel foam obtained in step 1) is immersed in a mixed solution containing 35 ml of deionized water, 2.4 mmol of hydrated nickel nitrate (Ni(NO3)2·6H2O), 0.8 mmol of hydrated iron nitrate (Fe(NO3)3·9H2O), 1.6 mmol of vanadium chloride (VCl3), 5 mmol of urea (CO(NH2)2) and 5 mmol of ammonium fluoride (NH4F), and then transferred to a high-temperature reactor for hydrothermal reaction at a constant temperature of 130°C for 11 hours. After the reaction is completed, it is cooled to room temperature, taken out and ultrasonically cleaned alternately in water and ethanol for multiple times, with an ultrasonic power of 100 W and an ultrasonic time of 20 min, and vacuum dried at 70°C for 9 hours to obtain a nickel foam loaded with nickel-iron-vanadium hydroxide nanoflowers (Fe1V2-Ni(OH)2); 3) The obtained nickel foam loaded with nickel iron vanadium hydroxide nanoflowers (Fe1V2-Ni(OH)2) was placed downstream of a tubular furnace, with 18.8 mmol hydrated sodium hypophosphite (NaH2PO2·H2O) upstream, and the phosphating reaction temperature was set to 320°C, the time was 1 h, and the heating rate was 4°C / min. After the reaction was completed, it was naturally cooled to room temperature to obtain an iron vanadium cation-doped nickel phosphide bifunctional self-supporting electrode material (Fe1V2-Ni2P).

Citation Information

Patent Citations

  • NiFeP bifunctional transition metal phosphide catalyst as well as preparation and use thereof

    CN107376958A

  • Ternary nickeliron phosphidenanosheet, preparation method thereof and application of electrolytic water

    CN108083242A

Cited By

  • V-doped nickel phosphorus material and preparation method and application thereof

    CN119506934A

  • Method for preparing adiponitrile by coupling electrochemical hydrogen evolution with electrochemical oxidation of waste PA-66 plastic

    CN119956373A

  • A method for producing adiponitrile from waste PA-66 plastic via electrochemical hydrogen evolution coupled with electrochemical oxidation.

    CN119956373B

  • Preparation and application method of nickel-based electrode for hydrogen evolution by electrolyzing water

    CN119980319A

  • Preparation and application method of nickel-based electrode for electrolysis of water to produce hydrogen

    CN119980319B