Method for calculating doping amount of silicon single crystal rod and method for preparing silicon single crystal rod

In the preparation process of single crystal silicon rod, the doping amount calculation method is used to calculate the dopant evaporation loss and calculate the dopant supplementary dopant alloy and dopant, and the problem of resistivity in the traditional method is solved, and the problem of resistivity inequality is achieved. The uniformity and stability of resistivity are achieved.

CN118910727AActive Publication Date: 2024-11-08ZHEJIANG JINKO SOLAR CO LTD

Patent Information

Application Number
CN202411413136.5
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-10-11
Publication Date
2024-11-08
Estimated Expiration
2044-10-11

AI Technical Summary

Technical Problem

In the field of photovoltaic technology, it is difficult for traditional methods to effectively control the resistivity uniformity of single-crystal silicon rods doped with strong volatile properties such as phosphorus, antimony, arsenic, etc., resulting in uneven resistivity of crystal rods during crystal drawing.

Method used

Through a single crystal silicon rod doping calculation method, it includes determining the furnace report feeding, performing induction and discharge, equal diameter growth and re-injection feeding processes, and calculating the need for re-doping based on the evaporation constant and the evaporation loss of the dopant. the quality of the parent alloy and dopant to ensure the uniformity of resistivity.

Benefits of technology

The resistivity uniformity and axial resistance stability of the single crystal silicon rod are achieved, ensuring the uniform distribution of dopants and improving the overall performance of the crystal.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118910727A_ABST
    Figure CN118910727A_ABST
Patent Text Reader

Abstract

The embodiment of the invention relates to the technical field of photovoltaics, and provides a doping amount calculation method of a silicon single crystal rod and a preparation method of the silicon single crystal rod, which are applied to the silicon single crystal rod doped with a dopant with strong volatility so as to improve the resistivity uniformity of the silicon single crystal rod. The method for calculating the doping amount of the silicon single crystal rod comprises the following steps: determining a coil base material adding frequency; when the feeding frequency of the coil base is greater than 1, adding the master alloy and the dopant into the crucible; sequentially carrying out at least one drawing and releasing process, an equal-diameter growth process and a re-feeding process; after a circulating material is added into the crucible, whether # imgabs0 # is established or not is judged; if yes, calculating the actual quantity Asf of the residual dopant in the crucible after the re-feeding process is finished; according to Mb = (As0-Asf) # imgabs1 # L / NA, the mass Mb of the doping agent needing to be supplemented and doped after the re-feeding and charging procedure is finished is calculated; and according to Mc = Am # imgabs2 # P / Cc, the mass Mc of the mother alloy needing to be supplemented and doped after the re-feeding and charging process is finished is calculated.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The embodiments of the present disclosure relate to the field of photovoltaic technology, and in particular to a method for calculating the doping amount of a single crystal silicon rod and a method for preparing the single crystal silicon rod. Background Art

[0002] Compared with P-type silicon wafers, N-type silicon wafers have better efficiency; in the field of photovoltaic technology, phosphorus dopants are widely used to form N-type silicon wafers. With the continuous development of technology, single-crystal silicon cells doped with elements such as arsenic, antimony, bismuth, selenium, and tellurium have attracted much attention. These doping elements themselves have the characteristics of extremely small segregation coefficients and extremely large evaporation coefficients; in the crystal pulling process, as the crucible material decreases, the traditional method of calculating the concentration of doping elements has made it difficult to control the uniformity of the resistivity of the crystal rod. Therefore, it is urgent to study the method of calculating the doping amount of dopants with strong volatility. Summary of the invention

[0003] The embodiments of the present disclosure provide a method for calculating the doping amount of a single crystal silicon rod and a method for preparing the single crystal silicon rod, which are applied to single crystal silicon rods doped with dopants with strong volatile properties, thereby improving the uniformity of the resistivity of such single crystal silicon rods.

[0004] An embodiment of the present disclosure provides a method for calculating the doping amount of a single crystal silicon rod, comprising: Determine the number of times the furnace is reported and added; the number of times the furnace is reported and added indicates the number of times the crucible is doped with the master alloy and the dopant; the master alloy is an N-type alloy doped with a first element, the dopant is a single substance including a second element, the first element and the second element are different elements in the fifth main group, or the first element is any element in the fifth main group, and the second element is any element in the third main group; When the number of times the furnace is fed with materials is greater than 1, adding the master alloy and the dopant into the crucible; At least one leading and releasing process, equal diameter growth process and re-feeding process are sequentially performed; wherein the re-feeding process comprises adding recycled material to the crucible; After adding the recycled material to the crucible, determine Is it established, wherein M1 refers to the mass of the preset residual material in the crucible after the recycled material is added; Mg refers to the mass of the actual residual material in the crucible after the recycled material is added; My is the mass corresponding to the unit volume of the silicon rod, C1 is the first preset constant, and the range of C1 is [1.5, 3]; If it is established, then according to the evaporation constant Rd in the re-feeding process and the cumulative amount Aq of the dopant evaporated in the re-feeding process, the actual amount Asf of the dopant remaining in the crucible after the re-feeding process is completed is calculated; According to Mb = (As0-Asf) L / NA, calculate the mass Mb of the dopant that needs to be supplemented after the re-feeding process is completed, wherein As0 refers to the preset amount of the dopant in the crucible after the re-feeding process is completed, L refers to the molecular weight of the dopant, and NA refers to the Avogadro constant; According to Mc=Am P / Cc, calculate the mass Mc of the master alloy that needs to be supplemented after the re-feeding process is completed, wherein Am refers to the total number of impurities in the master alloy that actually need to be supplemented after the re-feeding process is completed, P refers to the density value of silicon in the master alloy, and Cc refers to the concentration value of the first element in the master alloy.

[0005] According to some embodiments of the present disclosure, the evaporation constant Rd in the re-feeding process satisfies: Rd=f(M1).

[0006] According to some embodiments of the present disclosure, the amount Aq of the dopant evaporated cumulatively in the re-feeding process satisfies: Aq=Rd Cs1 Tc; Wherein, Cs1 is the preset concentration of the dopant in the melt in the crucible after the recycled material is added, and Tc is the time for adding the recycled material.

[0007] According to some embodiments of the present disclosure, the total number of impurities Am in the master alloy that actually needs to be supplemented after the re-feeding process is completed satisfies: Am=Ap0-Ap-An; Among them, the Ap0 refers to the preset total number of the first element in the crucible after the re-feeding process is completed, the Ap refers to the actual remaining total number of the first element in the crucible before the re-feeding process, and the An refers to the total number of the first element added in the re-feeding process.

[0008] According to some embodiments of the present disclosure, in the judgment After the determination is made, the calculation method further comprises: like If it is not established, adding the master alloy and the dopant into the crucible again; After adding the master alloy and the dopant again, calculate the effective segregation coefficient Ks of the dopant, the actual amount As of the dopant remaining in the crucible, the effective segregation coefficient Kp of the first element, the actual amount Ap2 of the first element remaining in the crucible and the actual concentration Cs2 of the dopant in the melt in the crucible.

[0009] According to some embodiments of the present disclosure, the effective segregation coefficient Ks of the dopant satisfies: Ks=Kb / [Kb+(1-Kb) e^(-F×δ / C2 / Qs)]; Wherein, Kb is the segregation coefficient of the dopant, F is the head pulling speed, δ is the diffusion boundary coefficient, C2 is a second preset constant, the range of C2 is [3000, 7000], and Qs is the diffusion coefficient of the dopant; The actual amount As of the dopant remaining in the crucible satisfies: As=As0-Va Ks As1 / V0-Rc As1 C3 / V0; Wherein, As0 refers to the theoretical amount of the dopant remaining in the crucible after the master alloy and the dopant are added again, Va refers to the volume corresponding to a unit length of a crystal rod, As1 refers to the amount of the dopant corresponding to a unit length of a crystal rod, V0 refers to the volume of the melt remaining in the crucible after the master alloy and the dopant are added again, C3 is a third preset constant, the range of C3 is [200, 400], and Rc refers to the evaporation constant of the dopant; The actual concentration Cs2 of the dopant in the melt in the crucible satisfies: Cs2=As / V0.

[0010] According to some embodiments of the present disclosure, the effective segregation coefficient Kp of the first element satisfies: Kp=Ka / [Ka+(1-Ka) e^(-F δ / C2 / Qp)]; Wherein, Ka is the segregation coefficient of the first element, F is the head pulling speed, δ is the diffusion boundary coefficient, C2 is a second preset constant, the range of C2 is [3000, 7000], and Qp is the diffusion coefficient of the first element; The actual amount Ap2 of the first element remaining in the crucible satisfies: Ap2=Ap3-Va Kp Ap4 / V0; The Ap3 refers to the theoretical amount of the first element remaining in the crucible after the mother alloy and the dopant are added again, and the Ap4 refers to the amount of the first element corresponding to a unit length of a crystal rod.

[0011] According to some embodiments of the present disclosure, the at least one drawing and releasing process further includes: judge Whether it is established, wherein the M refers to the mass of the preset remaining amount in the crucible after the addition of the master alloy and the dopant and before the introduction and release process; the Me refers to the mass of the actual remaining amount in the crucible after the addition of the master alloy and the dopant and before the introduction and release process; If it is established, the introduction and release process is performed; and the evaporation constant Ra in the introduction and release process and the total number of impurities Aj of the dopant that is cumulatively evaporated in the introduction and release process are calculated; After the introduction and release process is completed, the actual amount Asy of the dopant remaining in the crucible is calculated according to Asy=Asy0-Aj, wherein Asy0 refers to the theoretical amount of the dopant remaining in the crucible after the introduction and release process; The actual concentration Cs of the dopant in the melt in the crucible is calculated according to Cs=Asy / V, wherein V refers to the volume of the remaining melt in the crucible after the drawing and releasing process is completed.

[0012] According to some embodiments of the present disclosure, the evaporation constant Ra in the discharge process satisfies: Ra = f(M); The total number of impurities Aj of the dopant evaporated cumulatively in the introduction and release process satisfies: Aj=Ra Cs0 She; Wherein, the Cs0 is the concentration of the dopant in the melt in the crucible, and the Ta is the release time of the release process.

[0013] Another aspect of the present disclosure provides a method for preparing a single crystal silicon rod, comprising: The silicon material melting process, the drawing process, the equal diameter growth process and the re-feeding process are carried out in sequence; After the re-feeding process is completed, a master alloy and a dopant are added; wherein the mass of the master alloy and the mass of the dopant are obtained by the above-mentioned calculation method, the master alloy is an N-type alloy doped with a first element, the dopant is a single substance including a second element, the first element and the second element are different elements in the fifth main group elements, or the first element is any element in the fifth main group elements, and the second element is any element in the third main group elements.

[0014] The embodiments of the present disclosure provide a method for calculating the doping amount of a single crystal silicon rod and a method for preparing a single crystal silicon rod. In the method for calculating the doping amount of a single crystal silicon rod, the evaporation loss is calculated in the re-feeding process, and then the mass of the master alloy and the mass of the dopant that need to be supplemented are calculated, thereby ensuring the uniformity of the resistivity of the single crystal silicon rod doped with a dopant with a strong volatile property, and then achieving axial resistance stability. BRIEF DESCRIPTION OF THE DRAWINGS

[0015] One or more embodiments are exemplarily illustrated by pictures in the corresponding drawings, and these exemplified descriptions do not constitute a limitation on the embodiments. Unless otherwise specified, the pictures in the drawings do not constitute a scale limitation. In order to more clearly illustrate the embodiments of the present disclosure or the technical solutions in the traditional technology, the drawings required for use in the embodiments are briefly introduced below. Obviously, the drawings described below are only some embodiments of the present disclosure. For ordinary technicians in this field, other drawings can be obtained based on these drawings without paying creative work.

[0016] Figure 1 A schematic flow chart of a method for calculating the doping amount of a single crystal silicon rod provided in an embodiment of the present disclosure; Figure 2 A schematic diagram of axial resistivity distribution corresponding to different doping conditions provided in an embodiment of the present disclosure; Figure 3 A schematic flow chart of another method for calculating the doping amount of a single crystal silicon rod provided in an embodiment of the present disclosure; Figure 4 A schematic flow chart of another method for calculating the doping amount of a single crystal silicon rod provided in an embodiment of the present disclosure. DETAILED DESCRIPTION

[0017] In order to make the purpose, technical solutions and advantages of the present disclosure clearer, the technical solutions of the present disclosure will be clearly and completely described below in combination with the specific embodiments of the present disclosure and the corresponding drawings. Obviously, the described embodiments are only part of the embodiments of the present disclosure, not all of the embodiments. Based on the embodiments in the present disclosure, all other embodiments obtained by ordinary technicians in this field without making creative work are within the scope of protection of the present disclosure.

[0018] In the description of the embodiments of the present disclosure, “at least one” means one or more, and “a plurality of” means two or more, unless otherwise clearly and specifically defined.

[0019] In the description of the embodiments of the present disclosure, technical terms such as "first" and "second" are only used to distinguish different objects and cannot be understood as indicating or implying relative importance or implicitly indicating the number, specific order or primary and secondary relationship of the indicated technical features.

[0020] Reference to "embodiments" herein means that a particular feature, structure, or characteristic described in conjunction with the embodiments may be included in at least one embodiment of the present disclosure. The appearance of the phrase in various places in the specification does not necessarily refer to the same embodiment, nor is it an independent or alternative embodiment that is mutually exclusive with other embodiments. It is explicitly and implicitly understood by those skilled in the art that the embodiments described herein may be combined with other embodiments.

[0021] It should be noted that in the description of the embodiments of the present disclosure, the actual quantity, quantity, preset quantity and theoretical quantity all refer to the number of atoms. For example, the number Aq of dopants evaporated cumulatively in the re-feeding process refers to the number of atoms of dopants evaporated cumulatively in the re-feeding process.

[0022] In industry, both the directional solidification method of polycrystalline silicon and the Czochralski method of single crystal silicon belong to liquid phase growth methods. The solubility of doping elements in melts and solids is different. Generally speaking, the solubility of doping elements in liquids is greater than that in solids. This difference leads to an important physical phenomenon: segregation. That is, as the crystal grows, the concentration of doping elements in the melt continues to accumulate, and the concentration of doping elements in the later grown crystals gradually increases compared to the earlier grown crystals; this is reflected in the gradual decrease in resistivity.

[0023] In order to overcome the problem of non-uniform resistivity caused by single doping, co-doping technology came into being. The so-called co-doping is to simultaneously dope two or more doping elements into silicon crystals in a certain proportion. By adjusting the segregation coefficient and doping dosage of each doping element, the resistivity can be uniformed during the crystal growth process.

[0024] Taking boron and phosphorus as an example, due to the large segregation coefficient of boron, its distribution in the head of the crystal is relatively uniform; while the segregation coefficient of phosphorus is small, and the concentration of phosphorus gradually increases as the crystal grows. When the two are co-doped in a certain proportion, complete compensation of boron and phosphorus can be achieved at a specific position of the crystal. At this time, the resistivity will be infinitely high in theory, which is called the PN transition point. Subsequently, as the concentration of phosphorus continues to increase, the crystal will exhibit N-type conductivity, and the resistivity will gradually decrease. However, due to the compensation effect of phosphorus and boron, the resistivity of the head, middle, and tail of the entire crystal can be kept very close, thereby greatly reducing the span and distribution of the resistivity.

[0025] In the N-type single crystal co-doping flattening resistivity technology, the commonly used doping elements mainly include phosphorus (P), antimony (Sb) and arsenic (As). These elements all belong to the V group elements, and their outermost electron structure has one more electron than the stable IV group silicon atom. When these V group elements are doped into silicon crystals, they will replace some silicon atoms and introduce additional free electrons into the lattice. The following describes phosphorus, antimony and arsenic respectively.

[0026] Phosphorus (P) is one of the most common elements used for N-type doping. Phosphorus atoms have five valence electrons, four of which form covalent bonds with adjacent silicon atoms, while the fifth valence electron becomes a free electron that can move in the crystal lattice, thereby increasing the conductivity of the semiconductor. The segregation coefficient of phosphorus is 0.35, which is relatively small, which means that during crystal growth, phosphorus is more likely to be enriched in the tail of the crystal, resulting in relatively low resistivity in the tail. However, by co-doping with other elements, the distribution of phosphorus can be regulated, thereby leveling the resistivity of the entire crystal.

[0027] Antimony (Sb) and arsenic (As) are also commonly used elements for N-type doping. They also have excess valence electrons that can contribute to the free electron concentration in the semiconductor material. However, it should be noted that these elements may have high volatility in some cases, which will affect their distribution in the crystal and the final resistivity performance. Therefore, when using these elements for co-doping, the doping process conditions need to be more finely controlled.

[0028] The core of co-doping technology is to simultaneously dope two or more doping elements into silicon crystals in a certain proportion. Since different elements have different segregation coefficients and volatility characteristics, their distribution in the crystal will be different. By rationally designing the co-doping scheme, this difference can be used to compensate for each other's influence on the resistivity, thereby achieving uniformity and flattening of the resistivity of the entire crystal. For example, simultaneously doping phosphorus and other group V elements (such as antimony or arsenic) into N-type single crystal silicon, or combining with group III elements (such as boron B or gallium Ga) for co-doping, can effectively improve the resistivity distribution characteristics of the crystal.

[0029] In the related art, the method for calculating the amount of dopant used in single-doped CZN-type single crystal silicon is based on the doping calculation formula given in the national standard GB / T 13389-92: (1) In formula (1), N represents the doping concentration, ρ Represents the resistivity of a single crystal silicon rod, A and B are special constants, and the specific values ​​are given by relevant standards. This standard can be well applied to the conversion of the resistivity and doping concentration of a single crystal silicon rod under single-doped N-type or P-type direct-pull single crystal silicon at room temperature. For example, it can be calculated according to S1, test the resistance level or size of the silicon material → S2, calculate the number and concentration of silicon atoms → S3, obtain the resistance level and size of the master alloy → S4, calculate the concentration and number of master alloy impurities → S5, and calculate the head-controlled resistivity feed amount. This calculation method effectively takes into account the segregation effect of dopants in the silicon melt, but for mixed calculations involving dopants with strong volatility, the applicability is stretched, and it is difficult to meet the requirements for precise control of the resistivity uniformity of single crystal silicon rods.

[0030] Based on the above, the present disclosure provides a method for calculating the doping amount of a single crystal silicon rod. Figure 1 As shown, including: S11. Determine the number of times the furnace is reported and added; the number of times the furnace is reported and added indicates the number of times the crucible is doped with the master alloy and the dopant; the master alloy is an N-type alloy doped with a first element, the dopant is a single substance including a second element, the first element and the second element are different elements in the fifth main group, or the first element is any element in the fifth main group, and the second element is any element in the third main group.

[0031] The master alloy may be a co-doped N-type master alloy, in which case the first element and the second element are different elements in the fifth main group, for example, the first element is phosphorus, and the second element is antimony or arsenic. Alternatively, the master alloy may be a mixed N-type master alloy, in which case the first element is any element in the fifth main group, for example, phosphorus, and the second element is any element in the third main group, for example, gallium (Ga) or indium (In).

[0032] S12. When the number of times the furnace is charged is greater than 1, add the master alloy and dopant into the crucible.

[0033] S13, sequentially performing at least one leading and releasing process, equal diameter growth process and re-feeding process; wherein the re-feeding process includes adding recycled material to the crucible.

[0034] The process of preparing single crystal silicon rods by the Czochralski method includes: silicon material melting, seeding, shoulder release, shoulder rotation, equal diameter growth, and re-feeding. The seeding and release process may include seeding, shoulder release and shoulder rotation.

[0035] In the above silicon material melting process, the main heater and the bottom heater are slowly and linearly heated to a preset melt power within 1 hour to 1.5 hours (for example, 1 hour, 1.1 hours, 1.2 hours, 1.3 hours, 1.4 hours or 1.5 hours), wherein the melt power range of the main heater is 70kw-100kw, and for example, the melt power of the main heater is 70kw, 75kw, 80kw, 85kw, 90kw, 95kw or 100kw; the melt power range of the bottom heater is 60-90kw, and for example, the melt power of the bottom heater is 60kw, 65kw, 70kw, 75kw, 80kw, 85kw or 90kw. At the same time, the crucible rotation is maintained at 3 rpm to 4 rpm (for example: 3 rpm, 3.2 rpm, 3.4 rpm, 3.6 rpm, 3.8 rpm or 4 rpm) so that the silicon material can be heated more evenly.

[0036] In the above seeding process, in an argon atmosphere of 5 torr to 15 torr (for example, 5 torr, 6 torr, 8 torr, 10 torr, 12 torr, 14 torr or 15 torr), the crucible rotation is maintained at 4 to 6 rpm (for example, 4 rpm, 4.5 rpm, 5 rpm, 5.5 rpm or 6 rpm) to ensure the uniformity of the melt temperature distribution. At the same time, the crystal rotation is maintained at a constant 9 rpm. Slowly descend and preheat to keep the liquid surface temperature relatively stable. The purpose of the seeding process is to eliminate the dislocation caused by the thermal difference when the seed crystal contacts the melt. The seeding length is generally 0.8-1.2 times the equal diameter, for example, 0.8, 0.9, 1.0, 1.1 or 1.2 times.

[0037] After the seeding process, the shoulder release process and shoulder rotation process are entered. In the shoulder release process, it is necessary to increase the crucible rotation.

[0038] After the shoulder turning process is completed, the equal diameter growth process begins. The cooling power can be selectively reduced to 0kw-1kw according to the actual diameter after the shoulder turning, for example: 0.2kw, 0.4kw, 0.6kw, 0.8kw or 1kw; during the equal diameter growth process, the initial pulling speed of the head is 70mm / min-80mm / min; when the equal diameter length is 1000mm, the pulling speed needs to be increased.

[0039] The above-mentioned recycled materials refer to the leftover scraps after the round single crystal silicon rods are prepared, which include master alloys and dopants. The recycled materials are used for re-feeding to improve the utilization rate of raw materials and reduce costs.

[0040] S14. After adding recycled material to the crucible, determine Is it true, where M1 refers to the mass of the preset residual amount in the crucible after the recycled material is added; Mg refers to the mass of the actual residual amount in the crucible after the recycled material is added; My is the mass corresponding to the unit volume of the silicon rod, C1 is the first preset constant, and the range of C1 is [1.5, 3].

[0041] The above M1 can be obtained in advance according to theoretical calculation, Mg can be obtained according to sensor testing, and My can be measured in advance. The specific value of C1 can be 1.5, 1.8, 2.0, 2.2, 2.4, 2.6, 2.8 or 3.0.

[0042] If the units of M1, Mg and My are not consistent, they need to be converted into consistent units before calculation. For example, if the unit of M1 is gram and the unit of Mg is kilogram, the value of Mg can be multiplied by 1000 and then calculated with the value of M1.

[0043] If established, execute S15 to calculate the actual amount Asf of the dopant remaining in the crucible after the re-feeding process is completed according to the evaporation constant Rd in the re-feeding process and the amount Aq of the dopant evaporated cumulatively in the re-feeding process.

[0044] The amount Aq of dopants evaporated cumulatively in the above-mentioned re-feeding process is related to the evaporation constant Rd in the re-feeding process, and Rd is related to the mass of the remaining material in the crucible. The specific calculation formula is not limited.

[0045] S16, according to Mb = (As0-Asf) L / NA, calculate the mass Mb of the dopant that needs to be supplemented after the re-feeding process is completed, where As0 refers to the preset amount of dopant in the crucible after the re-feeding process is completed, L refers to the molecular weight of the dopant, and NA refers to the Avogadro constant.

[0046] The above As0 can be obtained according to the master alloy addition calculation template in the related art; after determining the element of the dopant, L can be determined; for example, if the dopant is antimony, L is 121.76; NA=6.02 10^23. The master alloy addition calculation template in the related art is a co-doping calculation formula obtained based on the above-mentioned single doping calculation formula (1) and related theories.

[0047] S17, according to Mc=Am P / Cc, calculate the mass Mc of the master alloy that needs to be supplemented after the re-feeding process is completed, where Am refers to the total number of impurities in the master alloy that actually need to be supplemented after the re-feeding process is completed, P refers to the density value of silicon in the master alloy, and the density value of silicon in the master alloy corresponds to the gear value of the master alloy; Cc refers to the concentration value of the first element in the master alloy.

[0048] The specific calculation method of Am is not limited. The total number of impurities in the master alloy refers to the total number of the first element doped in the master alloy. For example, if the first element is P, the total number of impurities in the master alloy refers to the total number of P atoms doped in the master alloy. After the master alloy is selected, P and Cc are also determined accordingly.

[0049] In the process of preparing single crystal silicon rods by the direct pulling method, the time of the re-feeding process is about 5 hours to 6 hours, which is a long time, and the evaporation loss of the dopant is large. If the evaporation loss of the dopant is not considered, the resistivity uniformity of the prepared single crystal silicon rod cannot meet the requirements. In the method for calculating the doping amount of the single crystal silicon rod provided in the embodiment of the present disclosure, the evaporation loss is considered in the re-feeding process, and then the mass of the master alloy and the mass of the dopant that need to be supplemented are calculated, so as to ensure the uniformity of the resistivity of the single crystal silicon rod doped with a dopant with a strong volatile property, and then achieve axial resistance stability.

[0050] The following is a comparison table of the resistivity of the single crystal silicon prepared after supplementary doping according to the doping amount calculation method of the single crystal silicon rod provided in the embodiment of the present disclosure and the resistivity of the single crystal silicon prepared after doping according to the traditional co-doping calculation method in the related art. The basis of the traditional co-doping calculation method is GB / T13389-92 "Procedure for Calculating the Resistivity and Dopant Concentration of Boron-Doped and Phosphorus-Doped Silicon Single Crystals". Specifically, the controlled target resistivity can be converted into the dopant concentration value first, and then calculated according to the relevant formulas and tables given in GB / T13389-92.

[0051] Table 1

[0052] In Table 1, the initial polysilicon material input is 925kg, the intrinsic resistivity is 700, the N-type master alloy gear: 0.0032~0.0045, the co-doping dopant gear: single substance or pure element, the calculated equal diameter length of the straight-pulled crystal rod is not more than 6000mm, and the calculated target head-controlled resistivity is 0.97. Among them, the density of silicon in the corresponding master alloy is different for different N-type master alloy gears. In Table 1, N-type alloy refers to phosphorus silicon alloy. Because phosphorus is flammable and simple substance is not easy to maintain, phosphorus element is made into the style of master alloy for doping. The element ratio of N-type alloy is calculated by gear, and the gear is generally between 0.0032-0.0042, which is defined at the factory. For example: a 500g phosphorus silicon master alloy, the gear is 0.0038, then the weight of the phosphorus element doped in the phosphorus silicon master alloy is 500g. 0.0038 = 1.9 g, the number of atoms of doped phosphorus is 1.9 Avogadro constant / relative molecular weight of phosphorus. In Table 1, the co-doped element refers to antimony alone, and the number of atoms of the co-doped element antimony is the mass of the antimony alone. Avogadro constant / relative molecular weight of antimony. By calculating the number of atoms of the doping element phosphorus and the number of atoms of the co-doped element antimony respectively, the ratio of the number of atoms of the doping element phosphorus to the number of atoms of the co-doped element antimony can be obtained.

[0053] It can be seen from Table 1 that in the case of single doping of N-type alloy, the resistivity of the single crystal silicon prepared after doping according to the traditional co-doping calculation method is 0.96, which is slightly different from the target resistivity of 0.97; however, in the case of co-doping of co-doped elements and N-type alloys, when the number of atoms of the doping element phosphorus and the number of atoms of the co-doped element antimony are in different proportions, the resistivities of the single crystal silicon prepared after doping according to the traditional co-doping calculation method are 0.855, 0.813, 0.795 and 0.785, respectively, and the deviations from the target resistivity are 11%, 16%, 18% and 19%, respectively, that is, they are all greatly different from the target resistivity of 0.97, indicating that the resistivity control of the single crystal silicon prepared after doping according to the traditional co-doping calculation method is inaccurate. In the single crystal silicon prepared after supplementary doping using the doping amount calculation method provided in the present application, when the number of atoms of the doping element phosphorus and the number of atoms of the co-doped element antimony are in different proportions, the resistivity can be stably controlled to be the target resistivity of 0.97, which fully demonstrates that the single crystal silicon prepared after supplementary doping using the doping amount calculation method provided in the present application can stably and accurately control the resistivity. Figure 2 This is a schematic diagram of the axial distribution of resistivity corresponding to different doping conditions in Table 1. Figure 2 It can be seen that the resistivity control is different when the crystal rod is pulled under different doping amounts. Under the specified rod length, the axial uniformity of resistivity control is the highest for 25g mixed rod.

[0054] It should be noted that in step S11, if the number of times the furnace is reported and added is zero, there is no need to supplement the mother alloy and dopant. If the number of times the furnace is reported and added is 1, the mass of the mother alloy and the mass of the dopant added in the re-adding process can be calculated according to the mother alloy addition calculation template in the relevant technology, without calculating the evaporation loss. For example, first calculate the total number of the first elements added Am1=A1-A0-A2, where A1 is the number of the first element in the mother alloy addition template in the relevant technology, A0 is the number of the first element remaining in the crucible, and A2 is the number of the first element in the current addition cycle; then calculate the mass of the mother alloy added Mc1=Am1 P / Cc, P refers to the density of silicon in the master alloy, Cc refers to the concentration of the first element in the master alloy; calculate the mass of the supplementary dopant Mb1=Ma 1000, where Ma is the mass of the dopant in the master alloy feed template, the unit of Ma is kilograms, and the unit of Mb1 is grams.

[0055] In one or more embodiments, in the above step S15, the evaporation constant Rd in the re-feeding process satisfies: Rd=f(M1), Rd and M1 are in a nonlinear relationship, and the specific calculation formula is not limited.

[0056] In one or more embodiments, in the above step S15, the cumulative amount of dopant evaporated in the re-feeding process Aq satisfies: Aq=Rd Cs1 Tc; where Cs1 is the preset concentration of the dopant in the melt in the crucible after adding the recycled material, and Tc is the time of adding the recycled material. Cs1 can be calculated through the master alloy charging calculation template in the relevant technology, and Tc can be obtained through testing. Using this calculation formula, the amount of dopant that has been evaporated cumulatively in the re-charging process can be accurately calculated.

[0057] In one or more embodiments, in the above step S17, the total number of impurities Am in the master alloy that actually needs to be supplemented after the re-feeding process is completed satisfies: Am=Ap0-Ap-An; Among them, Ap0 refers to the preset total number of the first element in the crucible after the re-feeding process is completed, Ap refers to the actual remaining total number of the first element in the crucible before the re-feeding process, and An refers to the total number of the first element added in the re-feeding process. Ap0 can be obtained according to the master alloy feeding calculation template in the relevant technology, and Ap and An can be calculated by relevant technology, which will not be described in detail here. Using this calculation formula, the total number of impurities in the master alloy that actually needs to be supplemented after the re-feeding process is completed can be accurately calculated.

[0058] In one or more embodiments, reference Figure 3 As shown, in S14, it is judged After the establishment, the calculation method also includes: like If not, execute S20 to add the master alloy and dopant into the crucible again.

[0059] S21. After adding the master alloy and dopant again, calculate the effective segregation coefficient Ks of the dopant, the actual amount As of the dopant remaining in the crucible, the effective segregation coefficient Kp of the first element, the actual amount Ap2 of the first element remaining in the crucible and the actual concentration Cs2 of the dopant in the melt in the crucible.

[0060] In one or more embodiments, in step S21, the effective segregation coefficient Ks of the dopant satisfies: Ks=Kb / [Kb+(1-Kb) e^(-F δ / C2 / Qs)]; Wherein, Kb is the segregation coefficient of the dopant, F is the head pulling speed, δ is the diffusion boundary coefficient, C2 is the second preset constant, the range of C2 is [3000, 7000], Qs is the diffusion coefficient of the dopant. The value of C2 can be 3000, 3500, 4000, 4500, 5000, 5500, 6000, 6500 or 7000.

[0061] It should be noted that the above diffusion boundary coefficient δ represents the size of the diffusion boundary area. In actual systems, due to the existence of concentration gradients or temperature gradients, a certain substance (such as solute, heat, etc.) diffuses significantly near a certain interface. The area near the interface is the diffusion boundary area, which usually has a lower diffusion rate and a higher concentration change rate, and is the main resistance to material transfer. In CZ-type single crystal silicon, the size of the internal diffusion boundary area is affected by many factors such as melt flow state, temperature distribution, and impurity concentration distribution. When determining the diffusion boundary coefficient δ, detailed numerical simulation or experimental measurement is required. In practical application calculations, the diffusion boundary coefficient δ can be a value close to a dimensionless value, generally a four-digit number.

[0062] In step S21, the actual amount As of the dopant remaining in the crucible satisfies: As=As0-Va Ks As1 / V0-Rc As1 C3 / V0; Among them, As0 refers to the theoretical amount of dopant remaining in the crucible after the master alloy and dopant are added again, Va refers to the volume corresponding to the unit length of the crystal rod, As1 refers to the amount of dopant corresponding to the unit length of the crystal rod, V0 refers to the volume of the melt remaining in the crucible after the master alloy and dopant are added again, C3 is the third preset constant, the range of C3 is [200, 400], and Rc refers to the evaporation constant of the dopant.

[0063] The specific value of C3 is 200, 205, 280, 300, 330, 333.333, 350, 380 or 400. Similar to the above Rd, Rc=f(M1), Rc and M1 are in a nonlinear relationship, and the specific calculation formula is not limited.

[0064] In step S21, the actual concentration Cs2 of the dopant in the melt in the crucible satisfies: Cs2=As / V0.

[0065] In one or more embodiments, in step S21, the effective segregation coefficient Kp of the first element satisfies: Kp=Ka / [Ka+(1-Ka) e^(-F δ / C2 / Qp)]; Wherein, Ka is the segregation coefficient of the first element, F is the head pulling speed, δ is the diffusion boundary coefficient, C2 is the second preset constant, the range of C2 is [3000, 7000], and Qp is the diffusion coefficient of the first element. Wherein, the value of C2 can be 3000, 3500, 4000, 4500, 5000, 5500, 6000, 6500 or 7000.

[0066] In step S21, the actual amount Ap2 of the first element remaining in the crucible satisfies: Ap2=Ap3-Va Kp Ap4 / V0; Among them, Ap3 refers to the theoretical amount of the first element remaining in the crucible after the mother alloy and the dopant are added again, and Ap4 refers to the amount of the first element corresponding to the unit length of the crystal rod.

[0067] In one or more embodiments, reference Figure 4 As shown, at least one drawing and releasing process in step S13 includes: S30. Judgment Is it established, where M refers to the mass of the preset remaining amount in the crucible after adding the master alloy and dopant and before the lead-out process; Me refers to the mass of the actual remaining amount in the crucible after adding the master alloy and dopant and before the lead-out process; If established, the following is executed: S31, performing the lead-in process; and calculating the evaporation constant Ra in the lead-in process and the total number of impurities Aj of the dopant evaporated cumulatively in the lead-in process.

[0068] S32. After the introduction and release process is completed, the actual amount Asy of the dopant remaining in the crucible is calculated according to Asy=Asy0-Aj, wherein Asy0 refers to the theoretical amount of the dopant remaining in the crucible after the introduction and release process.

[0069] S33. Calculate the actual concentration Cs of the dopant in the melt in the crucible according to Cs=Asy / V, wherein V refers to the volume of the remaining melt in the crucible after the drawing and releasing process is completed.

[0070] refer to Figure 4As shown, after step S33, step S130 is continued, and the equal diameter growth process and the re-feeding process are performed in sequence; wherein the re-feeding process includes adding recycled material to the crucible. At this time, the aforementioned step S13 includes S30-S33 and S130.

[0071] In one or more embodiments, in step S31, the evaporation constant Ra in the release process satisfies: Ra=f(M); Ra and M are in a nonlinear relationship, and the specific calculation formula is not limited.

[0072] In step S31, the total number of impurities Aj of the dopant evaporated in the introduction process satisfies: Aj=Ra Cs0 Ta; where Cs0 is the concentration of the dopant in the melt in the crucible, and Ta is the lead-in time of the lead-in process. Through this formula, the total number of impurities of the dopant that evaporated cumulatively in one lead-in process can be accurately calculated.

[0073] It should be noted that the reference Figure 4 As shown, if step S30 is not established, then enter S40, the judgment step of the secondary drawing and releasing process, the judgment step of the secondary drawing and releasing process is similar to the above steps S30-S33, and will not be repeated here. After the drawing and releasing process is completed, the equal diameter growth process and the re-feeding process are carried out in sequence.

[0074] The present disclosure also provides a method for preparing a single crystal silicon rod, comprising: S101, sequentially carry out the silicon material melting process, the drawing and releasing process, the equal diameter growth process and the re-feeding process.

[0075] S102. After the re-feeding process is completed, add a master alloy and a dopant; wherein the mass of the master alloy and the mass of the dopant are obtained by using any of the above-mentioned calculation methods, the master alloy is an N-type alloy doped with a first element, the dopant is a single substance including a second element, the first element and the second element are different elements in the fifth main group, or the first element is any element in the fifth main group, and the second element is any element in the third main group.

[0076] For the relevant descriptions in the above steps, please refer to the aforementioned embodiments and will not be repeated here.

[0077] Through this preparation method, after the re-feeding process is completed, a master alloy and a dopant of more suitable quality can be added, thereby ensuring the uniformity of the resistivity of the single crystal silicon rod and further achieving axial resistance stability.

[0078] Those skilled in the art can understand that the above-mentioned embodiments are specific examples for realizing the present disclosure, and in practical applications, various changes can be made to them in form and details without departing from the spirit and scope of the present disclosure. Any person skilled in the art can make various changes and modifications without departing from the spirit and scope of the present disclosure, so the protection scope of the present disclosure shall be based on the scope defined in the claims.

Claims

1. A method for calculating the doping amount of a single crystal silicon rod, characterized in that: include: Determine the number of times the furnace is reported and added; the number of times the furnace is reported and added indicates the number of times the crucible is doped with the master alloy and the dopant; the master alloy is an N-type alloy doped with a first element, the dopant is a single substance including a second element, the first element and the second element are different elements in the fifth main group, or the first element is any element in the fifth main group, and the second element is any element in the third main group; When the number of times the furnace is fed with materials is greater than 1, adding the master alloy and the dopant into the crucible; At least one leading and releasing process, equal diameter growth process and re-feeding process are sequentially performed; wherein the re-feeding process comprises adding recycled material to the crucible; After adding the recycled material to the crucible, determine Is it established, wherein M1 refers to the mass of the preset residual material in the crucible after the recycled material is added; Mg refers to the mass of the actual residual material in the crucible after the recycled material is added; My is the mass corresponding to the unit volume of the silicon rod, C1 is the first preset constant, and the range of C1 is [1.5, 3]; If it is established, then according to the evaporation constant Rd in the re-feeding process and the cumulative amount Aq of the dopant evaporated in the re-feeding process, the actual amount Asf of the dopant remaining in the crucible after the re-feeding process is completed is calculated; According to Mb = (As0-Asf) L / NA, calculate the mass Mb of the dopant that needs to be supplemented after the re-feeding process is completed, wherein As0 refers to the preset amount of the dopant in the crucible after the re-feeding process is completed, L refers to the molecular weight of the dopant, and NA refers to the Avogadro constant; According to Mc=Am P / Cc, calculate the mass Mc of the master alloy that needs to be supplemented after the re-feeding process is completed, wherein Am refers to the total number of impurities in the master alloy that actually need to be supplemented after the re-feeding process is completed, P refers to the density value of silicon in the master alloy, and Cc refers to the concentration value of the first element in the master alloy.

2. The calculation method according to claim 1, characterized in that: The evaporation constant Rd in the re-feeding process satisfies: Rd=f(M1).

3. The calculation method according to claim 1, characterized in that: The amount Aq of the dopant evaporated cumulatively in the re-feeding step satisfies: Aq=Rd Cs1 Tc; Wherein, Cs1 is the preset concentration of the dopant in the melt in the crucible after the recycled material is added, and Tc is the time for adding the recycled material.

4. The calculation method according to claim 1, characterized in that: The total number of impurities Am in the master alloy that actually needs to be added after the re-feeding process is completed satisfies: Am=Ap0-Ap-An; Among them, the Ap0 refers to the preset total number of the first element in the crucible after the re-feeding process is completed, the Ap refers to the actual remaining total number of the first element in the crucible before the re-feeding process, and the An refers to the total number of the first element added in the re-feeding process.

5. The calculation method according to claim 1, characterized in that: In the judgment After the determination is made, the calculation method further comprises: like If it is not established, adding the master alloy and the dopant into the crucible again; After adding the master alloy and the dopant again, calculate the effective segregation coefficient Ks of the dopant, the actual amount As of the dopant remaining in the crucible, the effective segregation coefficient Kp of the first element, the actual amount Ap2 of the first element remaining in the crucible and the actual concentration Cs2 of the dopant in the melt in the crucible.

6. The calculation method according to claim 5, characterized in that: The effective segregation coefficient Ks of the dopant satisfies: Ks=Kb / [Kb+(1-Kb) e^(-F δ / C2 / Qs)]; Wherein, Kb is the segregation coefficient of the dopant, F is the head pulling speed, δ is the diffusion boundary coefficient, C2 is a second preset constant, the range of C2 is [3000, 7000], and Qs is the diffusion coefficient of the dopant; The actual amount As of the dopant remaining in the crucible satisfies: As=As0-Va Ks As1 / V0-Rc As1 C3 / V0; Wherein, As0 refers to the theoretical amount of the dopant remaining in the crucible after the master alloy and the dopant are added again, Va refers to the volume corresponding to a unit length of a crystal rod, As1 refers to the amount of the dopant corresponding to a unit length of a crystal rod, V0 refers to the volume of the melt remaining in the crucible after the master alloy and the dopant are added again, C3 is a third preset constant, the range of C3 is [200, 400], and Rc refers to the evaporation constant of the dopant; The actual concentration Cs2 of the dopant in the melt in the crucible satisfies: Cs2=As / V0.

7. The calculation method according to claim 5, characterized in that: The effective segregation coefficient Kp of the first element satisfies: Kp=Ka / [Ka+(1-Ka) e^(-F×δ / C2 / Qp)]; Wherein, Ka is the segregation coefficient of the first element, F is the head pulling speed, δ is the diffusion boundary coefficient, C2 is a second preset constant, the range of C2 is [3000, 7000], and Qp is the diffusion coefficient of the first element; The actual amount Ap2 of the first element remaining in the crucible satisfies: Ap2=Ap3-Va Kp Ap4 / V0; The Ap3 refers to the theoretical amount of the first element remaining in the crucible after the mother alloy and the dopant are added again, and the Ap4 refers to the amount of the first element corresponding to a unit length of a crystal rod.

8. The calculation method according to claim 1, characterized in that: The at least one drawing and releasing process also includes: judge Whether it is established, wherein the M refers to the mass of the preset remaining amount in the crucible after the addition of the master alloy and the dopant and before the introduction and release process; the Me refers to the mass of the actual remaining amount in the crucible after the addition of the master alloy and the dopant and before the introduction and release process; If it is established, the introduction and release process is performed; and the evaporation constant Ra in the introduction and release process and the total number of impurities Aj of the dopant that is cumulatively evaporated in the introduction and release process are calculated; After the introduction and release process is completed, the actual amount Asy of the dopant remaining in the crucible is calculated according to Asy=Asy0-Aj, wherein Asy0 refers to the theoretical amount of the dopant remaining in the crucible after the introduction and release process; The actual concentration Cs of the dopant in the melt in the crucible is calculated according to Cs=Asy / V, wherein V refers to the volume of the remaining melt in the crucible after the drawing and releasing process is completed.

9. The calculation method according to claim 8, characterized in that: The evaporation constant Ra in the discharge process satisfies: Ra = f(M); The total number of impurities Aj of the dopant evaporated cumulatively in the introduction and release process satisfies: Aj=Ra Cs0 Yes; Wherein, the Cs0 is the concentration of the dopant in the melt in the crucible, and the Ta is the release time of the release process.

10. A method for preparing a single crystal silicon rod, characterized in that: include: The silicon material melting process, the drawing process, the equal diameter growth process and the re-feeding process are carried out in sequence; After the re-feeding process is completed, a master alloy and a dopant are added; wherein the mass of the master alloy and the mass of the dopant are obtained by the calculation method described in any one of claims 1 to 9, the master alloy is an N-type alloy doped with a first element, the dopant is a single substance including a second element, the first element and the second element are different elements in the fifth main group elements, or the first element is any element in the fifth main group elements, and the second element is any element in the third main group elements.

Citation Information

Patent Citations

  • Crystal silicon casting ingot master alloy weight calculating method and ingot casting method

    CN110468448A

  • Master alloy manufacturing method, crucible assembly and single crystal furnace

    CN116536761A

  • Method for calculating doping amount of multiple lightly phosphorus-doped drawn silicon single crystal rods

    CN116555895A

  • Method for realizing multi-rod resistance stable control in process of continuously pulling monocrystalline silicon

    CN116623276A

  • Method and device for determining addition amount of dopant of crystal bar

    CN116949555A

Cited By

  • Drawing method of silicon single crystal rod

    CN119265690A

  • Monocrystalline silicon rod resistance control method, monocrystalline silicon rod, silicon wafer and solar cell

    CN119465378A

  • Uniformity detection method and device of silicon-based material and computer readable storage medium

    CN120609757A

  • Method for controlling resistivity of N-type crystal bar by using phosphorus and antimony

    CN120797174A

  • N-type monocrystalline silicon antimony doping amount determination method, electronic equipment, system and program product

    CN121344747A