Radiation refrigeration fiber with heterostructure and special-shaped section as well as preparation method and fabric of radiation refrigeration fiber

Through heterogeneous structure and special-shaped cross-section, the problems of single thermal regulation and insufficient material performance of thermal and humidity collaborative management in the prior art are solved, and efficient radiation refrigeration and humidity regulation are achieved, which is suitable for human heat Management has the advantages of low cost and recyclability.

CN118910762AActive Publication Date: 2024-11-08SICHUAN UNIV

Patent Information

Application Number
CN202410965011.7
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-07-18
Publication Date
2024-11-08
Estimated Expiration
2044-07-18

AI Technical Summary

Technical Problem

The existing radiation refrigerated fiber materials have a single thermal regulation pathway in terms of thermal and humidity collaborative management, poor breathability and hygroscopicity, low processing efficiency, high cost and complex construction of special-shaped cross-sections, which is difficult to meet the complex human thermal management needs.

Method used

Using high-infrared emission polymer fibers with heterostructure and special-shaped cross-sections, fibers with good mid-infrared emissivity and wicking effects are constructed through solution blending and wet spinning technology, achieving low concentration heterodoping and high-efficiency humidity adjustment. , suitable for the preparation of human cooling textiles.

Benefits of technology

It achieves efficient radiation refrigeration and humidity regulation performance, has the advantages of large-scale batch preparation, low cost and recyclability, improves the mechanical properties and flexibility of the fibers, and is suitable for thermal management in complex environments.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118910762A_ABST
    Figure CN118910762A_ABST
Patent Text Reader

Abstract

The invention relates to a radiation refrigeration fiber with a heterostructure and a special-shaped section, a preparation method of the radiation refrigeration fiber and a fabric, and the method comprises the following steps: dissolving a polymer matrix material in an organic solvent, and dispersing an inorganic micro-nano sheet or a second component polymer in the organic solvent to obtain a spinning solution; and extruding the spinning solution from a spinning nozzle at a constant speed, carrying out phase separation on the extruded fiber precursor through a coagulating bath and a warm water bath in sequence at a draw ratio of 2-4 to form nascent fibers, and washing the nascent fibers through a hot water bath at a draw ratio of 2-4 to obtain the radiation refrigeration fiber with the heterostructure and the special-shaped section. According to the invention, a heterostructure is introduced into a polyester type polyurethane or polyether type polyurethane base material by utilizing solution blending, and the special-shaped cross-section fiber with good mid-infrared emissivity and wicking effect is constructed by regulating and controlling the solution spinning process. The fiber can be used for weaving radiation refrigeration and humidity regulation fabrics suitable for human skin cooling, and has the advantages of large-scale batch preparation, low cost and recyclability and reconstruction.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the field of radiation refrigeration materials, and in particular to a radiation refrigeration fiber with a heterogeneous structure and a special-shaped cross-section, a preparation method thereof, and a fabric. Background Art

[0002] With the annual increase in greenhouse gas emissions and fossil energy consumption, global warming and energy crisis have become major challenges facing human society. The extreme weather caused by this has seriously affected the thermal / humidity comfort of people's living space. At present, temperature control mainly relies on high-energy-consuming traditional air compression refrigeration technology. Although this active cooling technology can effectively reduce the ambient temperature and improve the thermal comfort of the environment, it also brings many hazards, such as increasing energy consumption and greenhouse gas emissions. Therefore, there is an urgent need for an environmentally friendly, cheap, and energy-free refrigeration method to reduce the temperature of objects.

[0003] According to Planck's blackbody radiation law, all objects with a temperature above absolute zero will continuously emit / absorb electromagnetic waves (thermal radiation). Objects of different temperatures can exchange heat energy (radiative heat transfer) by absorbing and emitting these energy-carrying electromagnetic waves. Radiative heat transfer is the most common form of energy transfer in the universe. The temperature of outer space is about 3K, while the average temperature of the earth's surface is about 300K. The earth and outer space also exchange heat through radiative heat transfer. Radiative heat management is usually a thermodynamic spontaneous process, in which the heat of an object can be regulated without consuming external energy.

[0004] Radiative cooling, as a zero-energy, environmentally friendly refrigeration technology, has attracted widespread attention from researchers at home and abroad, but there are still some problems with the application of existing radiative heat management materials to the human body.

[0005] In recent years, infrared transparent-visibly opaque textiles have been considered as an effective passive cooling strategy for the human body. Such textiles allow the infrared radiation of the human body to be directly emitted to the external environment to achieve minimal absorption. Cui et al. developed a uniform / continuous high infrared transparent nanoporous PE fiber for indoor cooling. The nanoporous structure in the PE fiber can effectively enhance visible light scattering, achieve nearly 90% solar light reflection and high infrared transparency of over 70%. The skin temperature covered by the nano PE fabric is 2.3℃ lower than that of ordinary cotton fabric, showing a good cooling effect. From the perspective of energy saving, the temperature difference of 2.3℃ between nano PE fabric and cotton fabric can reduce the cooling energy consumption by about 20.1%. However, under high outdoor solar radiation intensity, the radiative cooling effect of porous PE fiber is relatively poor. At the same time, since infrared transparent radiative cooling textiles can only be used for cooling the surface of high infrared emitting objects, there are limitations in the use of this series of products. In addition, due to the hydrophobicity of PE, it has poor hygroscopicity when worn as clothing and is prone to static electricity.

[0006] In addition to mid-infrared transparent fibers, high and medium infrared emitting fiber materials can also achieve radiative cooling. Zeng et al. used polylactic acid and high concentration of inorganic doping to prepare a multi-layer metamaterial fabric woven from micro-nano composite fibers, and achieved high emissivity (0.94) and high solar reflectivity (0.92) in the atmospheric window range through graded morphological design. Compared with commercial fabrics (cotton, chiffon, linen), the simulated skin temperature covered by metamaterial fabric can be 5-7°C lower. In the cooling test of the car model, the internal temperature of the model covered with metamaterial fabric can be cooled by 27°C compared with the commercially available car cover. During the preparation process of the composite fabric, a porous micro-nano fiber membrane layer was introduced on its upper surface. This design improves the solar reflectivity and surface hydrophobicity of the fabric, but also increases the cost and process complexity of clothing preparation, and is not conducive to the moisture absorption and perspiration properties of the fabric.

[0007] Radiative cooling fabric coatings have also been widely studied. Invention patent CN201911075603.7 discloses a radiative cooling functional layer, a radiative cooling fabric and a preparation method thereof. The radiative cooling fabric includes a flexible substrate layer and a radiative cooling functional layer disposed on the flexible substrate layer, the radiative cooling functional layer including: a first functional layer disposed on the flexible substrate layer, the first functional layer including a first radiative cooling functional resin; and a second functional layer formed by a radiative cooling functional powder, the radiative cooling functional powder being laid on the surface of the first functional layer, and the radiative cooling functional powder being bonded to the first radiative cooling functional resin. The radiative cooling functional layer of the invention has a good radiative cooling effect. Although the coating material has radiative cooling properties, the density of the coating leads to poor air permeability, and there are certain problems with the bonding strength and durability of the coating and the substrate, which limits its large-scale application in the field of human body cooling.

[0008] Human body heat management can be achieved by regulating human body thermal radiation, but for the complex human body temperature regulation process, a single radiation regulation is insufficient in some cases. For example, when the human body is in a high temperature and high humidity environment or exercising outdoors, in addition to the metabolic heat produced by the human body itself, it will also absorb solar radiation energy, which will cause the skin to produce a lot of sweat. Radiant heat management fibers can reduce human skin temperature to a certain extent, but they cannot prevent the production of sweat and its accumulation on the inner surface of the fiber material. If the sweat fails to transfer to the outer surface of the fiber material at this time, the accumulated excessive sweat will drip or be wiped off directly, and the sweat evaporation will not be effectively utilized to dissipate heat. At the same time, sweat will also inhibit heat transfer between the fiber and the skin, thereby reducing the effect of radiant cooling. Therefore, it is urgent to synergistically couple multiple heat regulation pathways to optimize the heat and moisture transfer performance of fiber materials.

[0009] The water in sweat has a high specific heat capacity (2400 kJ kg -1), in the process of evaporation to the environment, it can absorb more heat from the human body to achieve evaporative cooling. Usually when the ambient temperature is higher than the skin temperature or the sweating phenomenon is obvious due to human exercise, evaporative cooling becomes the main way for the human body to dissipate heat. Ding et al. successfully prepared a bionic multi-level composite fiber membrane with a multi-level bifurcation network and a mesh-interconnected heat transfer network by using electrospinning and plasma double-sided hydrophilic modification technology through the efficient mass transfer and heat transfer mechanism of bionic plant transpiration. Driven by the multi-level bifurcation network, sweat can be conducted from the inner layer (large pores) of the multi-level fiber membrane to the outer layer (small pores) against gravity. The out-of-plane and in-plane thermal conductivity of the bionic multi-level fiber membrane can reach 0.182 and 1.137 W m, respectively. -1 K -1 , the temperature difference between the inner and outer layers is only 0.6℃ under natural evaporation. The bionic multi-layer composite fabric promotes heat conduction and evaporative heat dissipation from the skin to the surrounding environment, but the structural design of the multi-layer micro-nano fiber membrane reduces the air permeability and preparation efficiency of the fabric, and also affects the durability of the fabric. At the same time, due to the lack of a good radiation heat dissipation mechanism, the cooling effect of the fabric is affected when the human body sweats slightly or not sweating.

[0010] In order to achieve rapid evaporative cooling of sweat, fibers with special cross-sections have also been increasingly studied. Chinese invention patent CN201711341959.1 discloses a moisture wicking fiber and a method for preparing the same. The polyester melt is extruded, cooled, oiled, stretched, heat-set and wound through a metering pump and a composite spinneret to obtain the moisture wicking fiber. The composite spinneret is provided with cross-shaped spinnerets and Wang-shaped spinnerets. Since the introduction of the special-shaped cross-section increases the capillary effect of the fiber, the fiber in this invention exhibits good moisture wicking properties. However, the formation of the special-shaped cross-section fiber in this method is inseparable from the special-shaped spinneret assembly with a complex structure and extremely high processing precision requirements, and the special-shaped fiber in this invention only focuses on the optimization of the evaporative cooling thermal regulation strategy.

[0011] From a functional perspective, current research on thermal management fiber materials is mostly focused on a single thermal regulation pathway to achieve human thermal management, such as heat conduction, thermal radiation, and evaporative heat dissipation; from a macroscopic fabric structure perspective, most of the focus is on electrospinning multilayer film structures, coated fabric structures, or melt-spinning new fibers. However, these materials usually have the following problems: (1) The thermal regulation pathway is single and cannot meet the complex human thermal management needs; (2) The coating and multilayer fiber membrane structures have poor air permeability and hygroscopicity, making them difficult to be widely used in human skin cooling; (3) Processing methods such as electrospinning and electrostatic spraying are inefficient and costly; (4) Traditional melt spinning requires high levels of nanoparticles to be doped internally to improve the radiative cooling effect; (5) In the field of traditional fiber processing, the construction of fiber profiles is inseparable from complex spinneret components. Summary of the invention

[0012] At present, there is a lack of a heat and moisture coordinated management fiber preparation technology with low-concentration heterogeneous doping radiative cooling and humidity regulation functions, which has good radiative cooling performance and humidity regulation performance while realizing low doping and controllable construction of special-shaped cross-sections, and is suitable for preparing human body cooling textiles. To this end, the present invention provides a radiative cooling fiber with a heterogeneous structure and a special-shaped cross-section, a preparation method thereof, and a fabric.

[0013] To achieve the above object, the present invention provides a method for preparing a radiation refrigeration fiber having a heterogeneous structure and a special-shaped cross-section, which comprises the following steps:

[0014] S1. Prepare spinning solution:

[0015] The polymer matrix material is dissolved in an organic solvent, and inorganic micro-nano sheets or a second component polymer having non-uniform lateral sizes are dispersed therein to obtain a spinning solution;

[0016] Wherein, the polymer matrix material is polyester polyurethane and / or polyether polyurethane, the polyester polyurethane is obtained by reacting poly(hexamethylene carbonate) glycol, polycaprolactone alcohol or polyhexamethylene carbonate glycol with isophorone diisocyanate or hexamethylene diisocyanate to obtain prepolymer A, and prepolymer A is polymerized with chain extender 1,4-butanediol to obtain polyester polyurethane, and the polyether polyurethane is obtained by reacting polypropylene oxide, polytetrahydrofuran or polyethylene glycol with isophorone diisocyanate or hexamethylene diisocyanate to obtain prepolymer B, and prepolymer B is polymerized with chain extender 1,4-butanediol to obtain polyether polyurethane, wherein the structural formulas of some reactants are as follows;

[0017]

[0018]

[0019] The refractive index coefficient of the inorganic micro-nanosheet is greater than 1.2, the second component polymer is cellulose or a cellulose derivative, and the organic solvent is N,N-dimethylformamide, N,N-dimethylacetamide, dimethyl sulfoxide, ethyl acetate, acetone, toluene or tetrahydrofuran;

[0020] S2, wet spinning:

[0021] The diameter of the nozzle hole of the spinneret is 100-300 μm, the extrusion rate is 2-12 m / min, the spinning solution is uniformly extruded from the spinneret, the extruded fiber precursor is sequentially passed through a coagulation bath and a warm water bath for phase separation at a draft ratio of 2-4 to form a primary fiber, and then the primary fiber is washed in a hot water bath at a draft ratio of 2-6 to obtain a radiation refrigeration fiber with a heterogeneous structure and a special-shaped cross-section;

[0022] The coagulation bath contains 10-50% by mass of a solvent that is the same as the polymer matrix material to be dissolved, the temperatures of the coagulation bath and the warm water bath are 20-40°C, and the temperature of the hot water bath is 50-90°C.

[0023] As a further preferred technical solution of the present invention, in step S1, the specific synthesis steps of polyester polyurethane and polyether polyurethane are:

[0024] (I) Preparation of polyester polyurethane

[0025] Adding poly(hexamethylene carbonate) diol, polycaprolactone alcohol or polyhexamethylene carbonate diol and isophorone diisocyanate or hexamethylene diisocyanate to N,N-dimethylformamide solution, reacting at 60-100° C. for 3-6 hours to obtain prepolymer A, wherein the molar ratio of poly(hexamethylene carbonate) diol, polycaprolactone alcohol or polyhexamethylene carbonate diol to isophorone diisocyanate or hexamethylene diisocyanate is 1:(2-2.5); adding chain extender 1,4-butanediol to the prepolymer A solution, reacting at 40-80° C. for 1-6 hours to form a polyester polyurethane solution with a mass fraction of 20-40%, wherein the molar ratio of isocyanate to hydroxyl is 1:(1-1.2); washing the polyester polyurethane solution with water, drying and granulating to obtain polyester polyurethane masterbatch;

[0026] (II) Preparation of polyether polyurethane

[0027] Adding polypropylene oxide, polytetrahydrofuran or polyethylene glycol and isophorone diisocyanate or hexamethylene diisocyanate to N,N-dimethylformamide solution, reacting at 60-100° C. for 3-6 hours to obtain prepolymer B, wherein the molar ratio of polypropylene oxide, polytetrahydrofuran or polyethylene glycol to isophorone diisocyanate or hexamethylene diisocyanate is 1:(2-2.5); adding the chain extender 1,4-butanediol to the prepolymer B solution, reacting at 40-80° C. for 1-6 hours to form a polyether polyurethane solution with a mass fraction of 20-40%, wherein the molar ratio of isocyanate to hydroxyl is 1:(1-1.2); washing the polyether polyurethane solution with water, drying and granulating to obtain a polyether polyurethane masterbatch;

[0028] As a further preferred technical solution of the present invention, in step S1, the specific steps of preparing the spinning solution are:

[0029] Dissolving the polymer matrix material in any one organic solvent of N,N-dimethylformamide, N,N-dimethylacetamide, dimethyl sulfoxide, ethyl acetate, acetone, toluene or tetrahydrofuran, stirring evenly to obtain a pure polymer solution;

[0030] Adding the inorganic micro-nano sheets or the second component polymer into the same solvent used to dissolve the polymer matrix material, and ultrasonically treating the solvent to obtain a dispersion;

[0031] The above pure polymer solution is mixed with the above dispersion and treated by ultrasound / stirring to obtain a spinning solution.

[0032] As a further preferred technical solution of the present invention, the mass fraction of the polymer matrix material in the spinning solution is 18-26%, and the doping mass of the inorganic micro-nano sheets or the second component polymer is 5-30% of the mass of the polymer matrix material.

[0033] As a further preferred technical solution of the present invention, the polymer matrix material is a polyester polyurethane or polyether polyurethane containing carbon-oxygen bonds, silicon-oxygen bonds, carbon-silicon bonds or carbon-fluorine bonds, and the polymer matrix material has an absorptivity greater than 90% in the mid-infrared region of 8-13 μm.

[0034] As a further preferred technical solution of the present invention, the inorganic micro-nano sheet is one or more of flaky micro-nano boron nitride, flaky micro-nano aluminum nitride, flaky micro-nano silicon nitride, flaky micro-nano titanium dioxide, flaky micro-nano silicon dioxide, and flaky micro-nano aluminum dioxide.

[0035] As a further preferred technical solution of the present invention, the lateral dimension (sheet width dimension) of the inorganic micro-nano sheet is in the range of 100nm-2500nm. The inorganic micro-nano sheet is preferably in the shape of a disc.

[0036] As a further preferred technical solution of the present invention, the second component polymer is one or more of cellulose nanofibers, bacterial cellulose, cellulose nanocrystals, cellulose esters, and cellulose ether esters.

[0037] According to another aspect of the present invention, the present invention also provides a radiation refrigeration fiber, which is prepared by the above method.

[0038] According to another aspect of the present invention, the present invention further provides a fabric, which adopts the above-mentioned radiation refrigeration fiber.

[0039] Compared with the prior art, the present invention can achieve the following beneficial effects:

[0040] 1) The present invention uses solution blending to introduce a heterogeneous structure into a high-mid infrared emitting polymer fiber substrate, and constructs a special-section fiber with good mid-infrared emissivity and wicking effect through the regulation of the solution spinning process. The fiber can be woven into a radiation cooling and humidity regulating fabric suitable for cooling human skin, and has the advantages of large-scale batch preparation, low cost and recyclable reconstruction;

[0041] 2) In view of the low backscattering efficiency caused by the current doping of spherical particles and quasi-spherical particles, which requires high-concentration heterogeneous filling, the present invention designs / selects non-spherical heterogeneous structures to dope the high-emission polymer fiber substrate, and utilizes the strong backlight scattering effect of non-spherical heterogeneous filling to achieve the reduction of the concentration of the heterogeneous structure while improving the reflectivity of the fiber in the solar band, thereby preparing low-doped radiation cooling fibers that maintain good mechanical properties, elasticity and flexibility.

[0042] 3) In view of the current technical bottleneck that the preparation of special-shaped cross-section fibers requires special auxiliary equipment such as special-shaped spinnerets, the preparation method provided by the present invention, without the need for additional auxiliary equipment, realizes the construction of multi-groove special-shaped fibers only through the regulation of the phase separation process during solution spinning and stretching orientation treatment, thereby giving the fibers a good wicking effect while the fibers maintain good mechanical properties, elasticity and flexibility. BRIEF DESCRIPTION OF THE DRAWINGS

[0043] The present invention will be further described in detail below in conjunction with the accompanying drawings and specific embodiments.

[0044] Figure 1 Microscopic morphology of the radiation cooling fiber prepared in Example 1 of the present invention at different magnifications.

[0045] Figure 2 This is a data graph of the solar reflectivity of the radiative cooling fabric prepared in Example 1 of the present invention.

[0046] Figure 3 This is a data graph of infrared emissivity of the radiative cooling fabric prepared in Example 1 of the present invention.

[0047] Figure 4 This is a diagram showing the wicking effect of the radiation refrigeration fiber bundle prepared in Example 1 of the present invention.

[0048] Figure 5 This is a radiative cooling temperature variation curve of the radiative cooling fabric prepared in Example 1 of the present invention at night (17:00-07:00).

[0049] Figure 6 This is a microscopic morphology of the radiation refrigeration fiber prepared in Comparative Example 1 of the present invention.

[0050] Figure 7 This is a data graph of the solar reflectivity of the radiative cooling fabric prepared in Comparative Example 2 of the present invention.

[0051] Figure 8 This is a surface morphology of the radiation refrigeration fiber prepared in Example 2 of the present invention.

[0052] Fig. 9 This is a data graph of infrared emissivity of the radiative cooling fabric prepared in Example 2 of the present invention.

[0053] The purpose, features and advantages of the present invention will be further described with reference to the accompanying drawings in conjunction with the embodiments. DETAILED DESCRIPTION

[0054] The specific implementation of the present invention is described in detail below in conjunction with the accompanying drawings. It should be understood that the specific implementation described here is only used to illustrate and explain the present invention, and is not used to limit the present invention.

[0055] Unless otherwise defined, the technical terms used in the following examples have the same meanings as those generally understood by those skilled in the art to which the present invention belongs. The test reagents used in the following examples, unless otherwise specified, are all conventional biochemical reagents; the experimental methods, unless otherwise specified, are all conventional methods.

[0056] Example 1

[0057] The radiation cooling fiber with heterogeneous structure and special-shaped cross section provided in this embodiment uses high-mid infrared absorbing polyester polyurethane rich in carbon-oxygen bonds as the fiber substrate, and the doped heterogeneous material is a circular sheet-like micro-nano boron nitride, the lateral size of the sheet-like micro-nano boron nitride is 200nm, 500nm, 1000nm (mass ratio is 1:1:1), and the total mass of boron nitride accounts for 20% of the mass of the fiber substrate. After testing, the radiation cooling fiber exhibits excellent mid-infrared emissivity, good spinning stability and a certain wicking effect.

[0058] The method for preparing the radiation refrigeration fiber with a heterogeneous structure and a special-shaped cross-section provided in this embodiment includes:

[0059] Preparation of polyester polyurethane:

[0060] According to the following synthesis route, poly(hexamethylene carbonate) diol and isophorone diisocyanate are added to an N,N-dimethylformamide solution, and reacted at 80° C. for 5 hours to obtain a prepolymer A, wherein the molar ratio of poly(hexamethylene carbonate) diol to isophorone diisocyanate is 1:2.1; a chain extender 1,4-butanediol is added to the prepolymer A solution, and reacted at 60° C. for 3 hours to form a polyester polyurethane solution with a mass fraction of 30%, wherein the molar ratio of isocyanate to hydroxyl is 1:1.1; the polyester polyurethane solution is washed with water, dried and granulated to obtain a polyester polyurethane masterbatch containing rich carbon-oxygen bonds;

[0061]

[0062] Step S1, preparation of radiation refrigeration composite material spinning solution:

[0063] The polyester polyurethane containing abundant carbon-oxygen bonds is dissolved in N,N-dimethylformamide to obtain a pure polymer solution with a mass fraction of 26%;

[0064] Putting flake micro-nano boron nitride with lateral sizes of 200 nm, 500 nm and 1000 nm in a mass ratio of 1:1:1 in N,N-dimethylformamide, and ultrasonically treating the solvent to obtain a uniform dispersion;

[0065] According to the doping amount of boron nitride being 20% ​​of the polymer mass, the above pure polymer solution is mixed with the boron nitride dispersion, and the mixed solution is subjected to ultrasonic / stirring treatment to obtain a spinning solution with a polyurethane mass fraction of 18-24%.

[0066] Step S2, preparing radiation refrigeration fibers by wet spinning:

[0067] Uniform extrusion of spinning solution: the spinning solution is extruded from the spinneret at a uniform speed, the diameter of the nozzle hole of the spinneret used is 200 μm, and the extrusion rate is 2-12 m / min;

[0068] Phase separation coagulation: the extruded fiber precursor is sequentially passed through a coagulation bath and a water bath for phase separation to form a fiber precursor, the mass fraction of N,N-dimethylformamide in the coagulation bath is 30%, and the temperatures of the coagulation bath and the water bath are 35°C;

[0069] Water washing: The fiber precursor is passed through a hot water bath to remove excess solvent on the fiber, and the hot water temperature is 60°C.

[0070] During the phase separation coagulation and water washing process, the total draft ratio of the fiber precursor in the entire spinning process was controlled to be 6, wherein the draft ratio in the phase separation process was 3, and the draft ratio in the water washing process was 2.

[0071] Winding: The washed fibers are wound at a speed of 800-900 m / h and then doffed to obtain pure white radiation cooling fibers doped with boron nitride in a flake form and having a groove structure on the surface. Finally, the fibers are twisted into yarns and woven into fabrics.

[0072] The fibers, yarns and fabrics prepared above were tested using the following methods:

[0073] The microstructure of the prepared radiation cooling fibers was observed using a scanning electron microscope (Nova Nano SEM 450).

[0074] The mid-infrared (8-13 μm) emissivity of the fabrics was measured using a Fourier transform infrared spectrometer (Nicolet 6700) with a gold integrating sphere.

[0075] The reflectivity of the fabric in the solar band (250-2200nm) was tested using a UV-visible-near infrared spectrometer (Nicolet 6700) with an integrating sphere.

[0076] To test the wicking height of the yarn, suspend the yarn over the water containing blue dye (one end of the yarn is below the water surface) and record the height of the blue dye water above the yarn within 10 minutes.

[0077] To test the radiation cooling performance of the fabric, place a thermocouple close to the bottom of the fabric, record the temperature under the fabric, and record the ambient temperature at the same time. The greater the temperature difference between the bottom of the fabric and the ambient temperature, the better the cooling effect.

[0078] Figure 1 1 shows the microscopic morphology of the fiber, and it can be seen that the fiber surface has an obvious groove structure; 2 is the solar reflectivity of the fabric. Because, in the solution spinning process, the primary fiber forms a skin-core structure by regulating the phase separation process, and then the stretching orientation treatment is used to force the fiber with the skin-core structure to undergo anisotropic deformation in the radial direction, thereby generating a groove structure. It is precisely because of the groove structure on the fiber surface and the filling of flake boron nitride that the average reflectivity of the fabric in the sunlight band can reach 79%. The test data is as follows: Figure 2 shown.

[0079] Figure 3 The infrared emissivity data of the fabric is shown in FIG. Since polyurethane contains abundant carbon-oxygen bonds, etc., it has a high absorptivity in the mid-infrared region. The average absorptivity of the fabric woven with the fiber in this embodiment is as high as 95% in the 8-13 μm band, which lays a good foundation for radiation cooling.

[0080] Figure 4 The wicking height diagram of the yarn. Due to the groove structure on the fiber surface, the fiber bundle has a good capillary effect (wicking effect). The test results show that the wicking height of the yarn is 3.5 cm, which lays a good foundation for moisture transfer (humidity regulation).

[0081] Figure 5 This is the radiation cooling temperature curve of the fabric. Due to the high emissivity of the fabric (95%), it shows a good cooling effect in the nighttime radiation cooling performance test, and the temperature at the bottom of the fabric can be more than 5.5°C lower than the ambient temperature.

[0082] Comparative Example 1

[0083] The preparation method of the radiation cooling fiber with a heterogeneous structure and a non-special-shaped cross section provided in this comparative example is different from the preparation method in Example 1 in that the draft ratio is different. The preparation method includes:

[0084] Step S1, preparation of radiation refrigeration composite material spinning solution:

[0085] The polyester polyurethane containing rich carbon-oxygen bonds prepared in Example 1 was dissolved in N,N-dimethylformamide to obtain a pure polymer solution with a mass fraction of 26%;

[0086] Circular flake-shaped micro-nano boron nitride with lateral sizes of 200 nm, 500 nm and 1000 nm respectively in a mass ratio of 1:1:1 is placed in N,N-dimethylformamide, and the solvent is ultrasonically treated to obtain a uniform dispersion;

[0087] According to the doping amount of boron nitride being 20% ​​of the polymer mass, the above pure polymer solution is mixed with the boron nitride dispersion, and the mixed solution is subjected to ultrasonic / stirring treatment to obtain a spinning solution with a polyurethane mass fraction of 18-24%.

[0088] Step S2, preparing radiation refrigeration fibers by wet spinning:

[0089] Uniform extrusion of spinning solution: the spinning solution is extruded from the spinneret at a uniform speed, the diameter of the nozzle hole of the spinneret used is 200 μm, and the extrusion rate is 2-12 m / min;

[0090] Phase separation coagulation: the extruded fiber precursor is sequentially passed through a coagulation bath and a water bath for phase separation to form a fiber precursor, the mass fraction of N,N-dimethylformamide in the coagulation bath is 30%, and the temperatures of the coagulation bath and the water bath are 35°C;

[0091] Water washing: The fiber precursor is passed through a hot water bath with a water temperature of 60°C.

[0092] During the phase separation coagulation and water washing process, the total draw ratio of the fiber precursor in the entire spinning process was controlled to be 3, the draw ratio in the phase separation process was 1.5, and the draw ratio in the water washing process was 2.

[0093] Winding: The washed fibers are wound at a speed of 800-900 m / h and then doffed to obtain pure white radiation cooling fibers doped with boron nitride in a flake form and without groove structures on the surface. Finally, the fibers are twisted into yarns and woven into fabrics.

[0094] Figure 6 The microscopic morphology of the fiber is shown, and it can be seen that the fiber surface does not have an obvious groove structure. This is because the spinning solution undergoes relatively complete phase separation in the coagulation bath and does not contain an obvious skin-core structure. Therefore, during the stretching and orientation process, the fiber radial direction cannot undergo anisotropic deformation, and thus no obvious groove structure can be produced.

[0095] Table 1 shows the solar reflectivity, infrared emissivity, wicking height and radiative cooling temperature difference data of the fabric in Comparative Example 1. Since polyurethane contains abundant carbon-oxygen bonds, etc., which makes it absorptive in the mid-infrared region, but the surface of the prepared fiber is relatively flat, the average reflectivity of the fiber-woven fabric in this implementation case in the solar band is 72%, and the average absorptivity in the 8-13μm band is only 90%. Since the fiber surface does not have a groove structure, the capillary effect is poor, and the maximum wicking height of the yarn is 1.8cm. In the nighttime radiative cooling performance test, the bottom temperature of the fabric can be about 4°C lower than the ambient temperature. Therefore, the overall performance of the fibers prepared by the method of Comparative Example 1 is significantly worse than that of Example 1.

[0096] Comparative Example 2

[0097] The method for preparing a radiation cooling fiber with a low-content heterogeneous structure and a shallow groove with a special-shaped cross-section provided in this comparative example is different from the preparation method in Example 1 in that the doped heterogeneous material is spherical micro-nano boron nitride, and the preparation method includes:

[0098] Step S1, preparation of radiation refrigeration composite material spinning solution:

[0099] The polyester polyurethane containing rich carbon-oxygen bonds prepared in Example 1 was dissolved in N,N-dimethylformamide to obtain a pure polymer solution with a mass fraction of 26%;

[0100] Spherical micro-nano boron nitride with diameters of 200 nm, 500 nm and 1000 nm in a mass ratio of 1:1:1 is placed in N,N-dimethylformamide, and the solvent is ultrasonically treated to obtain a uniform dispersion;

[0101] According to the doping amount of boron nitride being 20% ​​of the polymer mass, the above pure polymer solution is mixed with the boron nitride dispersion, and the mixed solution is subjected to ultrasonic / stirring treatment to obtain a spinning solution with a polyurethane mass fraction of 18-24%.

[0102] Step S2, preparing radiation refrigeration fibers by wet spinning:

[0103] Uniform extrusion of spinning solution: the spinning solution is extruded from the spinneret at a uniform speed, the diameter of the nozzle hole of the spinneret used is 200 μm, and the extrusion rate is 2-12 m / min;

[0104] Phase separation coagulation: the extruded fiber precursor is sequentially passed through a coagulation bath and a water bath for phase separation to form a fiber precursor, the mass fraction of N,N-dimethylformamide in the coagulation bath is 30%, and the temperatures of the coagulation bath and the water bath are 35°C;

[0105] Water washing: The fiber precursor is passed through a hot water bath with a water temperature of 60°C.

[0106] During the phase separation coagulation and water washing process, the total draft ratio of the fiber precursor in the entire spinning process was controlled to be 6, the draft ratio in the phase separation process was 3, and the draft ratio in the water washing process was 2.

[0107] Winding: The washed fibers are wound at a speed of 800-900 m / h and then doffed to obtain pure white radiation cooling fibers doped with spherical boron nitride and having a groove structure on the surface. Finally, the fibers are twisted into yarns and woven into fabrics.

[0108] Table 1 shows the solar reflectivity, infrared emissivity, wicking height and radiative cooling temperature difference data of the fabric of Comparative Example 2. Since polyurethane contains abundant carbon-oxygen bonds, etc., it has absorptivity in the mid-infrared region, but the prepared fiber contains spherical boron nitride inside, and the spherical heterostructure has a weak backscattering effect on light. Therefore, the average absorptivity of the fiber woven fabric in this implementation case in the 8-13μm band is only 93%, and the average reflectivity in the sunlight band is 74%. The fiber surface has a certain groove structure, and the maximum wicking height of the yarn is 2.4cm. In the nighttime radiative cooling performance test, the bottom temperature of the fabric can be about 4.5℃ lower than the ambient temperature.

[0109] Example 2

[0110] The radiation cooling fiber with heterogeneous structure and special-shaped cross section provided in this embodiment uses high and medium infrared absorption polyester polyurethane containing rich carbon-oxygen bonds as the fiber substrate, and the doped heterogeneous material is cellulose acetate, and the mass of cellulose acetate accounts for 20% of the mass of the fiber substrate. According to the test, the radiation cooling fiber exhibits excellent mid-infrared emissivity, good spinning stability and a certain wicking effect.

[0111] The method for preparing the radiation refrigeration fiber with a heterogeneous structure and a special-shaped cross-section provided in this embodiment includes:

[0112] Step S1, preparation of radiation refrigeration composite material spinning solution:

[0113] The polyester polyurethane containing rich carbon-oxygen bonds prepared in Example 1 was dissolved in N,N-dimethylformamide to obtain a pure polymer solution with a mass fraction of 26%;

[0114] Cellulose acetate is placed in N,N-dimethylformamide, and the solvent is ultrasonically treated to obtain a uniform dispersion with a mass fraction of 22%;

[0115] According to the doping amount of cellulose acetate being 20% ​​of the polymer mass, the above pure polymer solution is mixed with cellulose acetate dispersion, and the mixed solution is subjected to ultrasonic / stirring treatment to obtain a spinning solution with a polyurethane mass fraction of 18-24%.

[0116] Step S2, preparing radiation refrigeration fibers by wet spinning:

[0117] Uniform extrusion of spinning solution: the spinning solution is extruded from the spinneret at a uniform speed, the diameter of the nozzle hole of the spinneret used is 200 μm, and the extrusion rate is 2-12 m / min;

[0118] Phase separation coagulation: the extruded fiber precursor is sequentially passed through a coagulation bath and a water bath for phase separation to form a fiber precursor, the mass fraction of N,N-dimethylformamide in the coagulation bath is 30%, and the temperatures of the coagulation bath and the water bath are 35°C;

[0119] Water washing: The fiber precursor is passed through a hot water bath to remove excess solvent on the fiber, and the hot water temperature is 60°C.

[0120] During the phase separation coagulation and water washing process, the total draft ratio of the fiber precursor in the entire spinning process was controlled to be 6, the draft ratio in the phase separation process was 2, and the draft ratio in the water washing process was 3.

[0121] Winding: The washed fibers are wound at a speed of 800-900 m / h and then doffed to obtain pure white radiation cooling fibers doped with boron nitride in a flake form and having a groove structure on the surface. Finally, the fibers are twisted into yarns and woven into fabrics.

[0122] The surface of the obtained radiation cooling fiber has multiple grooves evenly distributed, and its surface morphology is as follows Figure 8 As shown, it has a certain wicking effect, and the wicking height is 3.7cm, which lays a good foundation for moisture transfer (humidity regulation). Fig. 9 As shown in the figure, the average emissivity at 8-13 μm is 94%, which lays a good foundation for radiative cooling. Due to the filling of the incompatible second component, a good heterogeneous structure is formed inside the fiber, which can effectively scatter visible light. The average reflectivity of the fabric prepared by the fiber of this embodiment to sunlight can reach 76%. The test data is shown in the figure. Figure 7 In the nighttime radiant cooling performance test, the temperature at the bottom of the fabric can be about 5°C lower than the ambient temperature.

[0123] Comparative Example 3

[0124] As a control experiment of Example 1, a radiation cooling fiber was prepared by a method basically the same as that of Example 1, with the only difference being that the circular flake-shaped micro-nano boron nitride had a uniform size of 200 nm, and the remaining steps remained the same as those of Example 1.

[0125] Step S1, preparation of radiation refrigeration composite material spinning solution:

[0126] The polyester polyurethane containing rich carbon-oxygen bonds prepared in Example 1 was dissolved in N,N-dimethylformamide to obtain a pure polymer solution with a mass fraction of 26%;

[0127] A circular flake-shaped micro-nano boron nitride with a lateral size of 200 nm is placed in N,N-dimethylformamide, and the solvent is ultrasonically treated to obtain a uniform dispersion;

[0128] According to the doping amount of boron nitride being 20% ​​of the polymer mass, the above pure polymer solution is mixed with the boron nitride dispersion, and the mixed solution is subjected to ultrasonic / stirring treatment to obtain a spinning solution with a polyurethane mass fraction of 18-24%.

[0129] Step S2, preparing radiation refrigeration fibers by wet spinning:

[0130] Uniform extrusion of spinning solution: the spinning solution is extruded from the spinneret at a uniform speed, the diameter of the nozzle hole of the spinneret used is 200 μm, and the extrusion rate is 2-12 m / min;

[0131] Phase separation coagulation: the extruded fiber precursor is sequentially passed through a coagulation bath and a water bath for phase separation to form a fiber precursor, the mass fraction of N,N-dimethylformamide in the coagulation bath is 30%, and the temperatures of the coagulation bath and the water bath are 35°C;

[0132] Water washing: The fiber precursor is passed through a hot water bath with a water temperature of 60°C.

[0133] During the phase separation coagulation and water washing process, the total draft ratio of the fiber precursor in the entire spinning process is controlled to be 6, that is, the draft ratio in the phase separation process is 3, and the draft ratio in the water washing process is 2.

[0134] Winding: The washed fibers are wound at a speed of 800-900 m / h and then doffed to obtain pure white radiation cooling fibers doped with boron nitride in a flake form and without groove structures on the surface. Finally, the fibers are twisted into yarns and woven into fabrics.

[0135] Table 1 shows the solar reflectivity, infrared emissivity, wicking height and radiative cooling temperature difference data of the fabric of Comparative Example 3. Since polyurethane contains abundant carbon-oxygen bonds, etc., it has absorptivity in the mid-infrared region, but the prepared fiber only contains boron nitride filling with a lateral size of 200nm, so that the average reflectivity of the fiber-woven fabric in this implementation case in the solar band is 69%, and the average absorptivity in the 8-13μm band is only 88%, which is significantly worse than Example 1. Although the fiber surface has a certain groove structure, the maximum wicking height of the yarn is 2.9cm, which is lower than Example 1. In addition, in the nighttime radiative cooling performance test, the bottom temperature of the fabric can be about 3.8℃ lower than the ambient temperature, and the effect is not as good as Example 1.

[0136] Example 3

[0137] The radiant refrigeration fiber was prepared by a method substantially the same as that in Example 1, except that polyether polyurethane was used as the fiber substrate, and the remaining steps were the same as those in Example 1.

[0138] Preparation of polyether polyurethane:

[0139] According to the following synthesis route, polytetrahydrofuran and isophorone diisocyanate are added to an N,N-dimethylformamide solution, and reacted at 80°C for 6 hours to obtain a prepolymer B, wherein the molar ratio of polytetrahydrofuran to isophorone diisocyanate is 1:2.1; the chain extender 1,4-butanediol is added to the prepolymer B solution, and reacted at 50°C for 5 hours to form a polyether polyurethane solution with a mass fraction of 30%, wherein the molar ratio of isocyanate to hydroxyl is 1:1.1; the polyester polyurethane solution is washed with water, dried and granulated to obtain a polyether polyurethane masterbatch rich in carbon-oxygen bonds;

[0140]

[0141] Step S1, preparation of radiation refrigeration composite material spinning solution:

[0142] The polyether polyurethane containing abundant carbon-oxygen bonds was dissolved in N,N-dimethylformamide to obtain a pure polymer solution with a mass fraction of 26%.

[0143] Putting flake micro-nano boron nitride with lateral sizes of 200 nm, 500 nm and 1000 nm in a mass ratio of 1:1:1 in N,N-dimethylformamide, and ultrasonically treating the solvent to obtain a uniform dispersion;

[0144] According to the doping amount of boron nitride being 20% ​​of the polymer mass, the above pure polymer solution is mixed with the boron nitride dispersion, and the mixed solution is subjected to ultrasonic / stirring treatment to obtain a spinning solution with a polyurethane mass fraction of 18-24%.

[0145] Step S2, preparing radiation refrigeration fibers by wet spinning:

[0146] Uniform extrusion of spinning solution: the spinning solution is extruded from the spinneret at a uniform speed, the diameter of the nozzle hole of the spinneret used is 200 μm, and the extrusion rate is 2-12 m / min;

[0147] Phase separation coagulation: the extruded fiber precursor is sequentially passed through a coagulation bath and a water bath for phase separation to form a fiber precursor, the mass fraction of N,N-dimethylformamide in the coagulation bath is 30%, and the temperatures of the coagulation bath and the water bath are 35°C;

[0148] Water washing: The fiber precursor is passed through a hot water bath with a water temperature of 60°C.

[0149] During the phase separation coagulation and water washing process, the total draft ratio of the fiber precursor in the entire spinning process is controlled to be 6, that is, the draft ratio in the phase separation process is 3, and the draft ratio in the water washing process is 2.

[0150] Winding: The washed fibers are wound at a speed of 800-900 m / h and then doffed to obtain pure white radiation cooling fibers doped with boron nitride in a flake form and without groove structures on the surface. Finally, the fibers are twisted into yarns and woven into fabrics.

[0151] Table 1 shows the solar reflectivity, infrared emissivity, wicking height and radiative cooling temperature difference data of the fabric of Comparative Example 3. Since polyurethane contains abundant carbon-oxygen bonds, etc., which makes it absorbent in the mid-infrared region, but the prepared fiber only contains boron nitride filling with a lateral size of 200nm, the average reflectivity of the fiber woven fabric in the implementation case is 78% in the solar band, and the average absorptivity in the 8-13μm band is only 95%. Similarly, the surface of the obtained fiber has a certain groove structure, and the maximum wicking height of the yarn is 3.5cm. In the nighttime radiative cooling performance test, the bottom temperature of the fabric can be about 5.5℃ lower than the ambient temperature.

[0152] The solar reflectivity, infrared emissivity, wicking height, and the temperature difference between the bottom of the fabric and the ambient temperature at night of the radiative cooling fibers prepared in the above Examples 1-3 and Comparative Examples 1-3 were tested, and the test results are shown in Table 1.

[0153] Table 1

[0154]

[0155] Further, based on Example 1, poly(hexamethylene carbonate) diol is replaced by polycaprolactone alcohol or polyhexamethylene carbonate diol, or isophorone diisocyanate is replaced by hexamethylene diisocyanate, and the resulting polyester polyurethane is used to prepare radiant cooling fibers by referring to the steps of Example 1. After multiple experiments, the solar emissivity, infrared emissivity, wicking height, and temperature difference between the night and the environment of the obtained radiant cooling fibers are equivalent to those of Example 1; based on Example 3, polytetrahydrofuran is replaced by polypropylene oxide or polyethylene glycol, or isophorone diisocyanate is replaced by hexamethylene diisocyanate, and the resulting polyether polyurethane is used to prepare radiant cooling fibers by referring to the steps of Example 3. After multiple experiments, the solar emissivity, infrared emissivity, wicking height, and temperature difference between the night and the environment of the obtained radiant cooling fibers are equivalent to those of Example 3.

[0156] Although specific embodiments of the present invention are described above, those skilled in the art should understand that these are merely examples and that various changes or modifications may be made to the embodiments without departing from the principles and essence of the present invention. The scope of protection of the present invention is limited only by the appended claims.

Claims

1. A method for preparing a radiation cooling fiber with a heterogeneous structure and a special-shaped cross-section, characterized in that: The following steps are involved: S1. Prepare spinning solution: The polymer matrix material is dissolved in an organic solvent, and inorganic micro-nano sheets or a second component polymer having non-uniform lateral sizes are dispersed therein to obtain a spinning solution; Wherein, the polymer matrix material is polyester polyurethane and / or polyether polyurethane, the polyester polyurethane is obtained by reacting poly(hexamethylene carbonate) glycol, polycaprolactone alcohol or polyhexamethylene carbonate glycol with isophorone diisocyanate or hexamethylene diisocyanate to obtain prepolymer A, and prepolymer A is polymerized with chain extender 1,4-butanediol to obtain polyester polyurethane, the polyether polyurethane is obtained by reacting polypropylene oxide, polytetrahydrofuran or polyethylene glycol with isophorone diisocyanate or hexamethylene diisocyanate to obtain prepolymer B, and prepolymer B is polymerized with chain extender 1,4-butanediol to obtain polyether polyurethane, the refractive index coefficient of the inorganic micro-nano sheet is greater than 1.2, the second component polymer is cellulose or a cellulose derivative, and the organic solvent is N,N-dimethylformamide, N,N-dimethylacetamide, dimethyl sulfoxide, ethyl acetate, acetone, toluene or tetrahydrofuran; S2, wet spinning: The diameter of the nozzle hole of the spinneret is 100-300 μm, the extrusion rate is 2-12 m / min, the spinning solution is uniformly extruded from the spinneret, the extruded fiber precursor is sequentially passed through a coagulation bath and a warm water bath for phase separation at a draft ratio of 2-4 to form a primary fiber, and then the primary fiber is washed in a hot water bath at a draft ratio of 2-6 to obtain a radiation refrigeration fiber with a heterogeneous structure and a special-shaped cross-section; The coagulation bath contains 10-50% by mass of a solvent that is the same as the polymer matrix material to be dissolved, the temperatures of the coagulation bath and the warm water bath are 20-40°C, and the temperature of the hot water bath is 50-90°C.

2. The method for preparing the radiation cooling fiber with heterogeneous structure and special-shaped cross section according to claim 1, characterized in that: In step S1, the specific synthesis steps of polyester polyurethane and polyether polyurethane are respectively as follows: (I) Preparation of polyester polyurethane Adding poly(hexamethylene carbonate) diol, polycaprolactone alcohol or polyhexamethylene carbonate diol and isophorone diisocyanate or hexamethylene diisocyanate to N,N-dimethylformamide solution, reacting at 60-100° C. for 3-6 hours to obtain prepolymer A, wherein the molar ratio of poly(hexamethylene carbonate) diol, polycaprolactone alcohol or polyhexamethylene carbonate diol to isophorone diisocyanate or hexamethylene diisocyanate is 1:(2-2.5); adding chain extender 1,4-butanediol to the prepolymer A solution, reacting at 40-80° C. for 1-6 hours to form a polyester polyurethane solution with a mass fraction of 20-40%, wherein the molar ratio of isocyanate to hydroxyl is 1:(1-1.2); washing the polyester polyurethane solution with water, drying and granulating to obtain polyester polyurethane masterbatch; (II) Preparation of polyether polyurethane Add polypropylene oxide, polytetrahydrofuran or polyethylene glycol and isophorone diisocyanate or hexamethylene diisocyanate to N,N-dimethylformamide solution, react at 60-100°C for 3-6h to obtain prepolymer B, wherein the molar ratio of polypropylene oxide, polytetrahydrofuran or polyethylene glycol to isophorone diisocyanate or hexamethylene diisocyanate is 1:(2-2.5); add the chain extender 1,4-butanediol to the prepolymer B solution, react at 40-80°C for 1-6h to form a polyether polyurethane solution with a mass fraction of 20-40%, wherein the molar ratio of isocyanate to hydroxyl is 1:(1-1.2); wash the polyether polyurethane solution with water, dry and granulate to obtain polyether polyurethane masterbatch.

3. The method for preparing the radiation cooling fiber with heterogeneous structure and special-shaped cross section according to claim 1, characterized in that: In step S1, the specific steps of preparing the spinning solution are: Dissolving the polymer matrix material in any one organic solvent of N,N-dimethylformamide, N,N-dimethylacetamide, dimethyl sulfoxide, ethyl acetate, acetone, toluene or tetrahydrofuran, stirring evenly to obtain a pure polymer solution; Adding the inorganic micro-nano sheets or the second component polymer into the same solvent used to dissolve the polymer matrix material, and ultrasonically treating the solvent to obtain a dispersion; The above pure polymer solution is mixed with the above dispersion and treated by ultrasound / stirring to obtain a spinning solution.

4. The method for preparing the radiation cooling fiber with heterogeneous structure and special-shaped cross section according to claim 1, characterized in that: The mass fraction of the polymer matrix material in the spinning solution is 18-26%, and the doping mass of the inorganic micro-nano sheets or the second component polymer is 5-30% of the mass of the polymer matrix material.

5. The method for preparing the radiation cooling fiber with heterogeneous structure and special-shaped cross section according to claim 1, characterized in that: The polymer matrix material is polyester polyurethane or polyether polyurethane containing carbon oxygen bond, silicon oxygen bond, carbon silicon bond or carbon fluorine bond. The polymer matrix material has an absorption rate greater than 90% in the 8-13 μm mid-infrared region.

6. The method for preparing the radiation cooling fiber with heterogeneous structure and special-shaped cross section according to claim 1, characterized in that: The inorganic micro-nano flakes are one or more of flaky micro-nano boron nitride, flaky micro-nano aluminum nitride, flaky micro-nano silicon nitride, flaky micro-nano titanium dioxide, flaky micro-nano silicon dioxide, and flaky micro-nano aluminum dioxide.

7. The method for preparing the radiation cooling fiber with heterogeneous structure and special-shaped cross section according to claim 1, characterized in that: The lateral size of the inorganic micro-nano sheets ranges from 100 nm to 2500 nm.

8. The method for preparing the radiation cooling fiber with heterogeneous structure and special-shaped cross section according to claim 1, characterized in that: The second component polymer is one or more of cellulose nanofibers, bacterial cellulose, cellulose nanocrystals, cellulose esters, and cellulose ether esters.

9. A radiation cooling fiber, characterized in that: The method is prepared according to any one of claims 1 to 8.

10. A fabric, characterized in that: The radiation refrigeration fiber according to claim 9 is used.

Citation Information

Patent Citations

  • High-heat-conductivity anisotropic polymer-based composite material and preparation method thereof

    CN110228248A

  • Radiation refrigeration fiber, preparation method thereof and application of fiber

    CN110685031A

  • Preparation method of radiation refrigeration fibers and fabric thereof

    CN111455483A

  • Preparation method of cellulose nanocrystal-self-healing polyurethane composite fiber based on waste cotton

    CN118308807A

  • Polyurethane yarn and method for producing the same

    JP2005281901A

Cited By

  • Radiation cooling fiber braided fabric with double-layer porous structure and preparation method of radiation cooling fiber braided fabric

    CN119663536A

  • Micro-gear-shaped special-shaped stretchable conductive anti-radiation fiber as well as preparation and application thereof

    CN120649194A

  • A micro-gear-shaped special-shaped stretchable conductive radiation-proof fiber and its preparation and application

    CN120649194B

  • Spectrum self-adaptive radiation refrigeration fiber and preparation method and application thereof

    CN121760094A

  • Spectrum adaptive radiation refrigeration fiber, and preparation method and application thereof