Hydrophobic paper cup stand and preparation method thereof
By modifying starch and polylactic acid, hot-pressing and spraying waterproofing agents, the problem of paper cup holder losing strength when contacting water is solved, and the preparation of hydrophobic paper cup holder is realized. It has excellent hydrophobic properties and strength, avoids beverage leakage, and is characterized by green and environmental protection and rapid degradation.
Patent Information
- Application Number
- CN202411248801.X
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-09-06
- Publication Date
- 2024-11-08
- Estimated Expiration
- Not applicable · inactive patent
AI Technical Summary
Existing paper cup holders lose strength and rot when exposed to water, causing the drink to leak and fail to effectively fix or package the drink, causing economic and emotional losses to merchants and consumers.
Starch is modified by γ-aminopropyltriethoxysilane and succinic anhydride, starch derivatives are prepared, and blended with polylactic acid to form modified polylactic acid fibers, and heat-pressed with pulp fibers. Finally spray waterproofing agent to enhance hydrophobicity.
The prepared hydrophobic paper cup holder has excellent hydrophobic properties and a certain strength, which can effectively prevent water immersion and avoid beverage leakage. It also has the characteristics of green and environmental protection and rapid degradation.
Smart Images

Figure BDA0005031659890000081 
Figure BDA0005031659890000091
Abstract
Description
Technical Field
[0001] The invention relates to the technical field of pulp molding, in particular to a hydrophobic paper cup holder and a preparation method thereof. Background Art
[0002] Paper tray, also known as pulp molding, is an environmentally friendly paper product made from carton scraps, newsprint, wood pulp, etc., which is crushed and mixed into a slurry with a certain concentration, then pressed and formed by CNC molds and dried. Due to its good shockproof, impactproof and corrosion-resistant characteristics, it has been widely used in packaging in the electronics, mechanical parts, porcelain and other industries since its inception.
[0003] In recent years, with the rise of the coffee and milk tea industries in China, in order to fix and package the drinks and reduce costs, paper trays have been processed into cup holders and applied to the coffee, milk tea and other beverage industries. However, the current paper cup holders will completely lose their strength or even rot once they come into contact with water, which will undoubtedly make them lose their fixing and packaging functions, causing the drinks to leak, which will cause certain economic and emotional consumption for both merchants and consumers.
[0004] In summary, the present invention provides a hydrophobic paper cup holder and a preparation method thereof, which have certain practical application significance. Summary of the invention
[0005] The object of the present invention is to provide a hydrophobic paper cup holder and a preparation method thereof, so as to solve the problems raised in the above background technology.
[0006] In order to solve the above technical problems, the present invention provides the following technical solutions:
[0007] A method for preparing a hydrophobic paper cup holder comprises the following steps:
[0008] Step 1: (1) modifying starch with γ-aminopropyltriethoxysilane and succinic anhydride to obtain a starch derivative; (2) mixing, plasticizing and extruding the starch derivative and polylactic acid to obtain a modified polylactic acid;
[0009] Step 2: mixing the modified polylactic acid and polylactic acid, and electrospinning to obtain modified polylactic acid fibers;
[0010] Step 3: (1) mixing pulp fiber, modified polylactic acid fiber, filler, adhesive, and deionized water to obtain slurry; (2) injecting the slurry into a molding machine, hot pressing and drying to obtain a paper cup holder;
[0011] Step 4: Spray the waterproofing agent onto the paper coaster and dry it to obtain a hydrophobic paper coaster.
[0012] Furthermore, the preparation method of the modified polylactic acid is as follows: (1) dispersing starch in dimethylformamide at 40 to 50° C. to obtain a 20 to 30 wt % starch suspension; (2) adding γ-aminopropyltriethoxysilane and succinic anhydride to dimethylformamide, stirring and reacting at 40 to 50° C. for 1 to 3 hours, heating to 60 to 70° C., adding starch suspension and catalyst thereto, continuing stirring and reacting for 2 to 8 hours, terminating the reaction, filtering, washing, and drying to obtain a starch derivative; (3) adding the starch derivative and polylactic acid into a mixer and mixing them evenly, and then plasticizing and extruding them through a twin-screw extruder to obtain a modified polylactic acid.
[0013] Furthermore, the raw materials for preparing the starch derivative include the following components: by weight, 3 to 6 parts of γ-aminopropyltriethoxysilane, 5 to 10 parts of succinic anhydride, 15 to 20 parts of starch, 1 to 2 parts of a catalyst, and 100 parts of dimethylformamide.
[0014] Furthermore, the mass ratio of the starch derivative to the polylactic acid is 1:(5-10), and the polylactic acid used in the present invention is all L-polylactic acid.
[0015] Furthermore, the extrusion temperature of the twin-screw extruder is 140-185° C., and the screw speed is 100-150 r / min.
[0016] Furthermore, the preparation method of the modified polylactic acid fiber is as follows: (1) adding modified polylactic acid and polylactic acid into dichloromethane, stirring and dissolving until the solution is stable and transparent, and preparing a spinning solution of 20 to 40 wt%; (2) injecting the spinning solution into an electrospinning machine, electrospinning, and washing to obtain the modified polylactic acid fiber.
[0017] Furthermore, the mass ratio of the modified polylactic acid to the polylactic acid is (1-3):1.
[0018] Furthermore, the relevant parameters of the electrospinning are: voltage of 5 to 15 KV, jet speed of 3 to 5 mL / h, and jet distance of 80 to 120 mm.
[0019] Furthermore, the slurry includes the following components: by weight, 50-60 parts of pulp fiber, 20-30 parts of modified polylactic acid fiber, 5-15 parts of filler, 20-30 parts of adhesive, and 200 parts of deionized water.
[0020] Furthermore, the filler includes but is not limited to any one of calcium carbonate, montmorillonite and silicon dioxide.
[0021] Furthermore, the adhesive is a water-based adhesive.
[0022] Furthermore, the relevant parameters of the hot pressing molding are: hot pressing temperature is 100-130° C., hot pressing pressure is 5-20 MN, and hot pressing time is 30-60 s.
[0023] Furthermore, the preparation method of the waterproofing agent is: adding tetraethyl silicate, hydrochloric acid and ethanol into a reaction container, stirring and mixing at room temperature for 12 to 24 hours, then adding fluorosilane and sodium dodecylbenzene sulfonate, and continuing to stir and mix for 3 to 6 hours to obtain the waterproofing agent.
[0024] Furthermore, the raw materials for preparing the waterproofing agent include the following components: by weight, 15 to 20 parts of tetraethyl silicate, 4 to 6 parts of hydrochloric acid, 60 to 80 parts of ethanol, 1 to 2 parts of fluorosilane, and 0.2 to 0.5 parts of sodium dodecylbenzene sulfonate.
[0025] Furthermore, the fluorosilane includes but is not limited to any one of (3,3,3-trifluoropropyl)methyldimethoxysilane, (3,3,3-trifluoropropyl)methyldiethoxysilane, and 1,3,5-trimethyl-1,3,5-tris(3,3,3-trifluoropropyl)-cyclotrisiloxane.
[0026] Furthermore, the spraying thickness is 0.2 to 0.5 mm.
[0027] Polylactic acid is a biodegradable hydrophobic material. The present invention is designed to spin it into polylactic acid fibers, and then mix it with pulp fibers to obtain a hydrophobic paper cup holder. However, in actual experiments, it is found that the paper cup holder directly processed from polylactic acid fibers and pulp fibers has a certain degree of hydrophobicity, but due to the brittleness of polylactic acid itself, the paper cup holder also shows obvious brittleness and structural instability. Therefore, the present invention obtains modified polylactic acid by modifying starch and then blending it with polylactic acid for extrusion.
[0028] By improving the compatibility between starch and polylactic acid, and then improving the interfacial bonding force between starch and polylactic acid, modified polylactic acid with excellent mechanical properties is obtained; then the modified polylactic acid and polylactic acid are mixed and spun to obtain modified polylactic acid fibers; the modified polylactic acid fibers are mixed and processed with pulp fibers to finally obtain a degradable paper cup holder with excellent hydrophobicity and a certain strength.
[0029] In order to further enhance the hydrophobicity of the paper cup holder, the scheme prepares silica sol under hydrochloric acid conditions, and modifies it with fluorosilane (fluorine has excellent hydrophobic properties) to obtain a waterproof agent; and immerses the paper cup holder in the waterproof agent to form a waterproof film on its surface to enhance the hydrophobicity of the paper cup holder. The reason why the silica sol is prepared under hydrochloric acid conditions is that the silica sol prepared under such conditions has better dispersibility and adhesion, and the scheme further adds sodium dodecylbenzene sulfonate to improve the dispersibility of the silica sol. Under the combined effect, the agglomeration of silica is greatly avoided, and the ability of the waterproof agent is improved.
[0030] Compared with the prior art, the beneficial effects achieved by the present invention are:
[0031] (1) The present invention enhances the hydrophobicity and mechanical properties of polylactic acid by using starch to enhance the polylactic acid, and finally spins the modified polylactic acid fiber with polylactic acid; the modified polylactic acid fiber is mixed with pulp fiber to prepare a degradable paper cup holder with good hydrophobicity and not easy to be damaged;
[0032] (2) In order to further enhance the hydrophobicity of the paper cup holder, the present invention sprays a layer of waterproof agent on the surface of the paper cup holder, and the waterproof agent can form a waterproof film on the surface of the paper cup holder, which can effectively prevent water from entering;
[0033] (3) The present invention comprehensively prepares a paper cup holder with excellent hydrophobic properties and certain strength, which can effectively prevent water from entering, and greatly avoids the drink spilling caused by the decrease in the strength of the cup holder due to water intrusion; in addition, the paper cup holder is green and environmentally friendly, can be quickly degraded, and will not cause significant damage to the environment. DETAILED DESCRIPTION
[0034] The following is a preferred implementation of the embodiment of the present invention. Obviously, the described embodiment is only a part of the embodiment of the present invention, not all of the embodiments. For ordinary technicians in this technical field, all other embodiments obtained by ordinary technicians in this field without creative work without departing from the principle of the embodiment of the present invention are within the scope of protection of the present invention.
[0035] Example 1: A method for preparing a hydrophobic paper cup holder:
[0036] Step 1: Preparation of modified polylactic acid: (1) Disperse 20 parts of corn starch into 60 parts of dimethylformamide at 45° C. to obtain a 25 wt% starch suspension; (2) Add 5 parts of γ-aminopropyltriethoxysilane and 8 parts of succinic anhydride to 40 parts of dimethylformamide, stir and react at 45° C. for 2 hours, then heat to 65° C., add starch suspension and 1.3 parts of concentrated sulfuric acid, continue stirring and react for 6 hours, terminate the reaction, filter, wash and dry to obtain a starch derivative; (3) Add the starch derivative and left-handed polylactic acid in a mass ratio of 1:7 into a mixer and mix them evenly, then plasticize and extrude them through a twin-screw extruder at an extrusion temperature of 175° C. and a screw speed of 150 r / min to obtain a modified polylactic acid;
[0037] Step 2: Preparation of modified polylactic acid fiber: (1) adding modified polylactic acid and L-polylactic acid into dichloromethane at a mass ratio of 2:1, stirring and dissolving until the solution is stable and transparent, and preparing a 30wt% spinning solution; (2) injecting the spinning solution into an electrospinning machine, electrospinning at a voltage of 10KV, a jet speed of 4mL / h, and a jet distance of 100mm, and then washing the spun silk with water to obtain modified polylactic acid fiber;
[0038] Step 3: (1) 55 parts of pulp fiber, 30 parts of modified polylactic acid fiber, 8 parts of silica, 25 parts of waterborne polyurethane, and 200 parts of deionized water are mixed uniformly to obtain a slurry; (2) the slurry is injected into a molding machine, hot-pressed for 45 seconds at a temperature of 120° C. and a pressure of 8MN to form the slurry, and then dried to a moisture content of 4% to obtain a paper cup holder;
[0039] Step 4: (1) adding 20 parts of tetraethyl silicate, 5 parts of hydrochloric acid (0.01 mol / L), and 80 parts of ethanol into a reaction container, stirring and mixing at room temperature for 24 hours, then adding 2 parts of (3,3,3-trifluoropropyl)methyldimethoxysilane and 0.4 parts of sodium dodecylbenzenesulfonate, and continuing to stir and mix for 5 hours to obtain a waterproofing agent;
[0040] (2) Spray the waterproof agent onto the paper cup holder with a spraying thickness of 0.3 mm to obtain a hydrophobic paper cup holder.
[0041] Example 2: A method for preparing a hydrophobic paper cup holder:
[0042] Step 1: Preparation of modified polylactic acid: (1) Dispersing 20 parts of corn starch into 60 parts of dimethylformamide at 45° C. to obtain a 25 wt% starch suspension; (2) Adding 3 parts of γ-aminopropyltriethoxysilane and 5 parts of succinic anhydride to 40 parts of dimethylformamide, stirring and reacting at 45° C. for 2 hours, heating to 65° C., adding the starch suspension and 1.3 parts of concentrated sulfuric acid, continuing to stir and react for 6 hours, terminating the reaction, filtering, washing, and drying to obtain a starch derivative;
[0043] (3) adding the starch derivative and L-polylactic acid in a mass ratio of 1:10 into a mixer and mixing them evenly, and then plasticizing and extruding them through a twin-screw extruder at an extrusion temperature of 175° C. and a screw speed of 150 r / min to obtain modified polylactic acid;
[0044] Step 2: Preparation of modified polylactic acid fiber: (1) adding modified polylactic acid and L-polylactic acid into dichloromethane at a mass ratio of 1:1, stirring and dissolving until the solution is stable and transparent, and preparing a 30wt% spinning solution; (2) injecting the spinning solution into an electrospinning machine, electrospinning at a voltage of 10KV, a jet speed of 4mL / h, and a jet distance of 100mm, and then washing the spun silk with water to obtain modified polylactic acid fiber;
[0045] Step 3: (1) 55 parts of pulp fiber, 30 parts of modified polylactic acid fiber, 8 parts of silica, 25 parts of waterborne polyurethane, and 200 parts of deionized water are mixed uniformly to obtain a slurry; (2) the slurry is injected into a molding machine, hot-pressed for 45 seconds at a temperature of 120° C. and a pressure of 8MN to form the slurry, and then dried to a moisture content of 4% to obtain a paper cup holder;
[0046] Step 4: (1) adding 20 parts of tetraethyl silicate, 5 parts of hydrochloric acid (0.01 mol / L), and 80 parts of ethanol into a reaction container, stirring and mixing at room temperature for 24 hours, then adding 1 part of (3,3,3-trifluoropropyl)methyldimethoxysilane and 0.4 parts of sodium dodecylbenzenesulfonate, and continuing to stir and mix for 5 hours to obtain a waterproofing agent;
[0047] (2) Spray the waterproof agent onto the paper cup holder with a spraying thickness of 0.3 mm to obtain a hydrophobic paper cup holder.
[0048] Example 3: A method for preparing a hydrophobic paper cup holder:
[0049] Step 1: Preparation of modified polylactic acid: (1) Disperse 20 parts of corn starch into 60 parts of dimethylformamide at 45° C. to obtain a 25 wt% starch suspension; (2) Add 6 parts of γ-aminopropyltriethoxysilane and 10 parts of succinic anhydride to 40 parts of dimethylformamide, stir and react at 45° C. for 2 hours, then heat to 65° C., add starch suspension and 1.3 parts of concentrated sulfuric acid, continue stirring and react for 6 hours, terminate the reaction, filter, wash and dry to obtain a starch derivative; (3) Add the starch derivative and left-handed polylactic acid into a mixer at a mass ratio of 1:5 and mix them evenly, then plasticize and extrude them through a twin-screw extruder at an extrusion temperature of 175° C. and a screw speed of 150 r / min to obtain a modified polylactic acid;
[0050] Step 2: Preparation of modified polylactic acid fiber: (1) adding modified polylactic acid and L-polylactic acid into dichloromethane at a mass ratio of 3:1, stirring and dissolving until the solution is stable and transparent, and preparing a 30wt% spinning solution; (2) injecting the spinning solution into an electrospinning machine, electrospinning at a voltage of 10KV, a jet speed of 4mL / h, and a jet distance of 100mm, and then washing the spun silk with water to obtain modified polylactic acid fiber;
[0051] Step 3: (1) 55 parts of pulp fiber, 30 parts of modified polylactic acid fiber, 8 parts of silica, 25 parts of waterborne polyurethane, and 200 parts of deionized water are mixed uniformly to obtain a slurry; (2) the slurry is injected into a molding machine, hot-pressed for 45 seconds at a temperature of 120° C. and a pressure of 8MN to form the slurry, and then dried to a moisture content of 4% to obtain a paper cup holder;
[0052] Step 4: (1) adding 20 parts of tetraethyl silicate, 5 parts of hydrochloric acid (0.01 mol / L), and 80 parts of ethanol into a reaction container, stirring and mixing at room temperature for 24 hours, then adding 2 parts of (3,3,3-trifluoropropyl)methyldimethoxysilane and 0.4 parts of sodium dodecylbenzenesulfonate, and continuing to stir and mix for 5 hours to obtain a waterproofing agent;
[0053] (2) Spray the waterproof agent onto the paper cup holder with a spraying thickness of 0.3 mm to obtain a hydrophobic paper cup holder.
[0054] Based on Example 1, a control experiment was carried out, specifically Comparative Examples 1 to 4, as described below:
[0055] Comparative Example 1: Comparative Example 1 is based on Example 1, with the following modifications: corn starch is not used to modify polylactic acid, and other processes remain unchanged, specifically: a method for preparing a hydrophobic paper cup holder:
[0056] Step 1: Preparation of polylactic acid fiber: (1) adding L-polylactic acid to dichloromethane, stirring and dissolving until the solution is stable and transparent, and preparing a 30 wt% spinning solution; (2) injecting the spinning solution into an electrospinning machine, and electrospinning under the conditions of a voltage of 10 KV, a jet speed of 4 mL / h, and a jet distance of 100 mm, and then washing the spun silk with water to obtain polylactic acid fiber;
[0057] Step 2: (1) 55 parts of pulp fiber, 30 parts of polylactic acid fiber, 8 parts of silica, 25 parts of waterborne polyurethane, and 200 parts of deionized water are mixed uniformly to obtain a slurry; (2) the slurry is injected into a molding machine, hot-pressed for 45 seconds at a temperature of 120° C. and a pressure of 8MN to form the slurry, and then dried to a moisture content of 4% to obtain a paper cup holder;
[0058] Step 3: (1) adding 20 parts of tetraethyl silicate, 5 parts of hydrochloric acid (0.01 mol / L), and 80 parts of ethanol into a reaction container, stirring and mixing at room temperature for 24 hours, then adding 2 parts of (3,3,3-trifluoropropyl)methyldimethoxysilane and 0.4 parts of sodium dodecylbenzenesulfonate, and continuing to stir and mix for 5 hours to obtain a waterproofing agent;
[0059] (2) Spray the waterproof agent onto the paper cup holder with a spraying thickness of 0.3 mm to obtain a hydrophobic paper cup holder.
[0060] Comparative Example 2: Comparative Example 2 is based on Example 1, with the following modifications: directly mixing corn starch and polylactic acid, plasticizing and extruding, and other processes remain unchanged, specifically: a method for preparing a hydrophobic paper cup holder:
[0061] Step 1: Preparation of modified polylactic acid: corn starch and L-polylactic acid are added into a mixer at a mass ratio of 1:7 and mixed evenly, and then plasticized and extruded through a twin-screw extruder at an extrusion temperature of 175°C and a screw speed of 150r / min to obtain modified polylactic acid;
[0062] Step 2: Preparation of modified polylactic acid fiber: (1) adding modified polylactic acid and L-polylactic acid into dichloromethane at a mass ratio of 2:1, stirring and dissolving until the solution is stable and transparent, and preparing a 30wt% spinning solution; (2) injecting the spinning solution into an electrospinning machine, electrospinning at a voltage of 10KV, a jet speed of 4mL / h, and a jet distance of 100mm, and then washing the spun silk with water to obtain modified polylactic acid fiber;
[0063] Step 3: (1) 55 parts of pulp fiber, 30 parts of modified polylactic acid fiber, 8 parts of silica, 25 parts of waterborne polyurethane, and 200 parts of deionized water are mixed uniformly to obtain a slurry; (2) the slurry is injected into a molding machine, hot-pressed for 45 seconds at a temperature of 120° C. and a pressure of 8MN to form the slurry, and then dried to a moisture content of 4% to obtain a paper cup holder;
[0064] Step 4: (1) adding 20 parts of tetraethyl silicate, 5 parts of hydrochloric acid (0.01 mol / L), and 80 parts of ethanol into a reaction container, stirring and mixing at room temperature for 24 hours, then adding 2 parts of (3,3,3-trifluoropropyl)methyldimethoxysilane and 0.4 parts of sodium dodecylbenzenesulfonate, and continuing to stir and mix for 5 hours to obtain a waterproofing agent;
[0065] (2) Spray the waterproof agent onto the paper cup holder with a spraying thickness of 0.3 mm to obtain a hydrophobic paper cup holder.
[0066] Comparative Example 3: Comparative Example 3 is based on Example 1, with the following modifications: no waterproofing agent is sprayed on the paper cup holder, and other processes remain unchanged, specifically: a method for preparing a hydrophobic paper cup holder:
[0067] Step 1: Preparation of modified polylactic acid: (1) Dispersing 20 parts of corn starch into 60 parts of dimethylformamide at 45° C. to obtain a 25 wt% starch suspension; (2) Adding 5 parts of γ-aminopropyltriethoxysilane and 8 parts of succinic anhydride to 40 parts of dimethylformamide, stirring and reacting at 45° C. for 2 hours, heating to 65° C., adding the starch suspension and 1.3 parts of concentrated sulfuric acid, continuing to stir and react for 6 hours, terminating the reaction, filtering, washing, and drying to obtain a starch derivative;
[0068] (3) adding the starch derivative and L-polylactic acid in a mass ratio of 1:7 into a mixer and mixing them evenly, and then plasticizing and extruding them through a twin-screw extruder at an extrusion temperature of 175° C. and a screw speed of 150 r / min to obtain modified polylactic acid;
[0069] Step 2: Preparation of modified polylactic acid fiber: (1) adding modified polylactic acid and L-polylactic acid into dichloromethane at a mass ratio of 2:1, stirring and dissolving until the solution is stable and transparent, and preparing a 30wt% spinning solution; (2) injecting the spinning solution into an electrospinning machine, electrospinning at a voltage of 10KV, a jet speed of 4mL / h, and a jet distance of 100mm, and then washing the spun silk with water to obtain modified polylactic acid fiber;
[0070] Step 3: (1) 55 parts of pulp fiber, 30 parts of modified polylactic acid fiber, 8 parts of silica, 25 parts of waterborne polyurethane, and 200 parts of deionized water are mixed uniformly to obtain a slurry; (2) the slurry is injected into a molding machine, hot-pressed for 45 seconds at a temperature of 120° C. and a pressure of 8MN to form the slurry, and then dried to a moisture content of 4% to obtain a paper cup holder;
[0071] Comparative Example 4: Comparative Example 4 is based on Example 1, with the following adjustments: no modified polylactic acid fiber is added, no waterproofing agent is sprayed, and other processes remain unchanged, specifically: a method for preparing a hydrophobic paper cup holder:
[0072] Step 1: (1) 55 parts of pulp fiber, 8 parts of silica, 25 parts of waterborne polyurethane, and 200 parts of deionized water are mixed uniformly to obtain a slurry; (2) the slurry is injected into a molding machine, hot-pressed for 45 seconds at a temperature of 120° C. and a pressure of 8MN to form the slurry, and then dried to a moisture content of 4% to obtain a hydrophobic paper cup holder.
[0073] In the above embodiments, all raw materials are from the following sources: corn starch is commercially available; dimethylformamide, γ-aminopropyltriethoxysilane, succinic anhydride, L-polylactic acid, tetraethyl silicate, (3,3,3-trifluoropropyl)methyldimethoxysilane, and sodium dodecylsulfonate are all 99% pure and were purchased from Shanghai Jinjinle Industrial Co., Ltd.; water-based polyurethane item number: JBL-58155, purchased from Guangzhou Jiabaili Waterproof Engineering Co., Ltd.
[0074] Performance test: (1) The hydrophobic paper cup holders prepared in the embodiment and the comparative example were tested for waterproof performance using a JIC-1 wetting angle measuring instrument;
[0075] (2) The degradation rate of the paper cup holder is tested by the soil burial method; the degradation rate testing method is as follows: firstly, the paper cup holder is weighed m0, then buried in the soil, taken out after 10 weeks, placed in a dryer for two days, and then weighed m1 to calculate the degradation rate; the degradation rate (%) = (m0-m1) / m0×100%.
[0076] The specific test results are shown in Table 1 below:
[0077] Table 1
[0078]
[0079]
[0080] Conclusion: From the data in Table 1 above, it can be seen that Example 3 is the best example; the modified polylactic acid fiber prepared by modifying starch and then polylactic acid can effectively enhance the hydrophobicity and degradation rate of the paper cup holder; further spraying a waterproofing agent can significantly improve the hydrophobicity of the paper cup holder, although it will slightly affect the degradation rate of the paper cup holder. Finally, it is shown that the present invention prepares a paper cup holder with excellent hydrophobic properties.
[0081] Finally, it should be noted that the above is only a preferred embodiment of the present invention, but the protection scope of this application is not limited thereto. Any changes or substitutions that can be easily thought of by any technician familiar with the technical field within the spirit and principle of the present invention and within the technical scope disclosed in this application should be included in the protection scope of this application; in the absence of conflict, the embodiments of this application and the features in the embodiments can be combined with each other. Therefore, the protection scope of this application shall be based on the protection scope of the claims.
Claims
1. A method for preparing a hydrophobic paper cup holder, Features: The following steps are involved: Step 1: (1) modifying starch with γ-aminopropyltriethoxysilane and succinic anhydride to obtain a starch derivative; (2) mixing, plasticizing and extruding the starch derivative and polylactic acid to obtain a modified polylactic acid; Step 2: mixing the modified polylactic acid and polylactic acid, and electrospinning to obtain modified polylactic acid fibers; Step 3: (1) mixing pulp fiber, modified polylactic acid fiber, filler, adhesive and deionized water to obtain slurry; (2) injecting the slurry into a molding machine, hot pressing and drying to obtain a paper cup holder; Step 4: Spray the waterproofing agent onto the paper coaster and dry it to obtain a hydrophobic paper coaster.
2. A method for preparing a hydrophobic paper cup holder according to claim 1, Features: The preparation method of the modified polylactic acid is as follows: (1) dispersing starch in dimethylformamide at 40 to 50° C. to obtain a 20 to 30 wt % starch suspension; (2) adding γ-aminopropyltriethoxysilane and succinic anhydride to dimethylformamide, stirring and reacting at 40 to 50° C. for 1 to 3 hours, heating to 60 to 70° C., adding starch suspension and catalyst thereto, continuing stirring and reacting for 2 to 8 hours, terminating the reaction, filtering, washing, and drying to obtain a starch derivative; (3) adding the starch derivative and polylactic acid into a mixer and mixing them evenly, and then plasticizing and extruding them through a twin-screw extruder to obtain a modified polylactic acid; Among them, the raw materials for preparing starch derivatives include the following components: by weight, 3 to 6 parts of γ-aminopropyltriethoxysilane, 5 to 10 parts of succinic anhydride, 15 to 20 parts of starch, 1 to 2 parts of catalyst, and 100 parts of dimethylformamide; among them, the mass ratio of starch derivatives to polylactic acid is 1:(5 to 10).
3. A method for preparing a hydrophobic paper cup holder according to claim 2, Features: The extrusion temperature of the twin-screw extruder is 140-185° C., and the screw speed is 100-150 r / min.
4. The method for preparing a hydrophobic paper cup holder according to claim 1, Features: The preparation method of the modified polylactic acid fiber is as follows: (1) adding modified polylactic acid and polylactic acid into dichloromethane, stirring and dissolving, and preparing a spinning solution with a concentration of 20 to 40 wt %; (2) injecting the spinning solution into an electrostatic spinning machine, electrostatically spinning, and washing to obtain the modified polylactic acid fiber; Among them, the mass ratio of modified polylactic acid and polylactic acid is (1-3):
1.
5. The method for preparing a hydrophobic paper cup holder according to claim 4, Features: The relevant parameters of the electrospinning are: voltage of 5 to 15 KV, jet speed of 3 to 5 mL / h, and jet distance of 80 to 120 mm.
6. The method for preparing a hydrophobic paper cup holder according to claim 1, Features: The slurry comprises the following components: by weight, 50-60 parts of pulp fiber, 20-30 parts of modified polylactic acid fiber, 5-15 parts of filler, 20-30 parts of adhesive and 200 parts of deionized water.
7. The method for preparing a hydrophobic paper cup holder according to claim 1, Features: The relevant parameters of the hot pressing molding are as follows: the hot pressing temperature is 100-130° C., the hot pressing pressure is 5-20 MN, and the hot pressing time is 30-60 s.
8. The method for preparing a hydrophobic paper cup holder according to claim 1, Features: The preparation method of the waterproofing agent is as follows: tetraethyl silicate, hydrochloric acid and ethanol are added into a reaction container, stirred and mixed for 12 to 24 hours at room temperature, and then fluorosilane and sodium dodecylbenzene sulfonate are added, and the stirring and mixing is continued for 3 to 6 hours to obtain the waterproofing agent; Among them, the raw materials for preparing the waterproofing agent include the following components: by weight, 15 to 20 parts of tetraethyl silicate, 4 to 6 parts of hydrochloric acid, 60 to 80 parts of ethanol, 1 to 2 parts of fluorosilane, and 0.2 to 0.5 parts of sodium dodecylbenzene sulfonate; the fluorosilane includes any one of (3,3,3-trifluoropropyl)methyldimethoxysilane, (3,3,3-trifluoropropyl)methyldiethoxysilane, and 1,3,5-trimethyl-1,3,5-tris(3,3,3-trifluoropropyl)-cyclotrisiloxane.
9. The method for preparing a hydrophobic paper cup holder according to claim 1, Features: The spraying thickness is 0.2-0.5 mm. 10 . The hydrophobic paper cup holder prepared according to the method for preparing a hydrophobic paper cup holder according to any one of claims 1 to 9.
Citation Information
Cited By
Preparation method and application of modified starch for improving permeability resistance of medical paper
CN121270728A