Preparation method of bifunctional catalyst and application of bifunctional catalyst in high-density fuel synthesis
By introducing metal on NbOPO4 support, the MOx/NbOPO4 dual-function catalyst was prepared, and the problems of poor catalyst performance and slow reaction rate in the prior art were solved, and high-efficiency one-pot solvent-free method was achieved to synthesize high-density polycycloalkane fuel, reducing energy Consumption and cost.
Patent Information
- Application Number
- CN202410986819.3
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-07-23
- Publication Date
- 2024-11-12
- Estimated Expiration
- 2044-07-23
AI Technical Summary
In the prior art, when synthesizing high-density polycycloalkane fuels from biomass derivatives, the catalyst performance is poor, the reaction rate is slow, and additional solvent is required, resulting in high energy consumption and high cost.
Prepare MOx/NbOPO4 bifunctional catalysts, and form MOx/NbOPO4 catalysts with different metal impregnation amounts, which are used for the one-pot solvent-free method to synthesize high-density polycycloalkane fuels, catalyzed alkylation and hydrodeoxygenation reaction.
A highly efficient catalytic lignin derivatives in one pot solvent-free reaction is achieved, and high-density polycycloalkane fuel is obtained, with a fast reaction rate and high catalytic activity, reducing energy consumption and cost.
Smart Images

Figure CN118925761A_ABST
Abstract
Description
Technical Field
[0001] The present invention belongs to the field of organic catalytic synthesis, and specifically relates to MO with controllable metal and acid centers. x / NbOPO 4 A method for preparing a bifunctional catalyst and its use in one-pot solvent-free synthesis of high-density fuels. Background Art
[0002] "One generation of power, one generation of equipment", the fuel performance level determines the performance level of the engine and the aircraft. As new aircraft develop towards higher, faster and farther directions, higher requirements are placed on the fuel used as the power of aircraft, and high energy density hydrocarbon fuels are urgently needed. In addition, under the condition of a certain aircraft tank volume, the greater the fuel mass that can be carried by increasing the fuel density, this is also one of the most effective technical ways to achieve aircraft endurance; at the same time, increasing the fuel density is conducive to the miniaturization of aircraft, or reducing the volume of the fuel tank, providing ample space for electronic equipment and other components.
[0003] However, with the continuous exploitation of oil resources, the rapid development of various industries, the substantial increase in demand for liquid fuels, and a series of problems caused by fossil fuels, the development of new economical and energy-saving liquid fuels is an urgent problem to be solved. The research on the use of renewable biomass raw materials to replace fossil raw materials to synthesize high-density fuels has gradually received widespread attention. Biomass-derived biojet fuel can reduce carbon emissions by up to 80% throughout the life cycle of the fuel. Biomass derivatives have unsaturated carbon-carbon bonds and / or oxygen-containing groups with no more than one ring, so multi-step reactions are required to obtain hydrocarbons with multiple rings. First, carbon-carbon (CC) coupling is required to construct a polycyclic oxygenated fuel precursor; secondly, the polycyclic oxygenated fuel precursor is subjected to a hydrodeoxygenation reaction to remove oxygen and saturate the C=C bond to obtain polycyclic alkanes. Perhydrofluorene is a tricyclic hydrocarbon with a density of 1.012 g / mL at 20°C. It is a high-performance high-density fuel and can also be used as an additive to increase the density of existing aerospace fuels.
[0004] At present, the research on the one-pot synthesis of alkanes from biomass derivatives mainly focuses on straight-chain alkanes and monocyclic or bicyclic alkanes, while there are few studies on the catalysis of tricyclic and higher alkanes. 4 One-pot production of diesel series branched C hydrocarbons using furfural and 2-methylfuran as raw materials via hydroxyalkylation and hydrodeoxygenation over a catalyst 15Straight-chain alkanes, but additional solvent cyclohexane is required to disperse the oxygen-containing intermediates during the hydrodeoxygenation reaction, the reaction time is as long as 17 hours, and the density of straight-chain alkanes is lower than that of cycloalkanes. Reference Fuel, 2023, 334, 126634. Bicyclic and tricyclic alkanes were prepared by a one-pot method using Pt / Hβ catalyst to catalyze the alkylation and hydrodeoxygenation of phenol and cyclohexanol. However, the proportion of bicyclic alkanes obtained is relatively high, which will reduce the final fuel density to a certain extent, and the entire reaction system needs to be carried out in cyclohexane solvent, and the reaction time is as long as 16 hours. Although these one-pot reaction routes can simplify the reaction process and improve energy efficiency, the use of a large amount of additional solvents still leads to relatively high energy consumption. Obviously, the catalysts prepared in these documents have poor performance, resulting in a slow overall reaction rate.
[0005] The synthesis of polycyclic fuels from biomass platform molecules is mainly obtained through a two-step process. The first step is to increase the carbon number of the target molecule through CC coupling reaction to obtain an oxygenated fuel intermediate, and then the second step is to use a hydrogenation catalyst and an acid catalyst to generate a polycyclic alkane series fuel from the oxygenated intermediate during the hydrodeoxygenation process. 4 -IB catalyzes the CC coupling of phenol and benzyl alcohol to obtain oxygenated fuel intermediates, and then introduces Ru / C during the hydrodeoxygenation process. 4 -IB and Ru / C synergistic catalytic system, a one-pot solvent-free sequential synthesis method for obtaining a fuel mainly composed of perhydrofluorene and dicyclohexylmethane from lignin derivatives was developed. The literature (Sustainable Energy Fuels, 2022, 6, 1616-1624.) reported that after the aldol condensation product was obtained by vanillin and cyclohexanone under the catalysis of sulfated titanium dioxide nanofibers, it was purified by column chromatography, and Pd / C and HY catalysts were introduced in the hydrodeoxygenation process, and cyclohexane was used as solvent to further convert it into a mixture of perhydrofluorene and dicyclohexylmethane. Patent CN115920934A reported NbOPO 4 The catalyst has excellent acidity for catalyzing alkylation reactions. However, to obtain polycyclic alkane fuel, the reactor needs to be reopened after the alkylation reaction is completed, and the Ru / C catalyst is added to the reactor. 4 Only by physically mixing with Ru / C can the hydrodeoxygenation reaction be completed to obtain polycycloalkane fuel.
[0006] The two-step catalytic reaction to produce polycycloalkane jet fuel is cumbersome and requires different catalysts at different reaction stages, which is costly. In addition, the acid catalyst and metal catalyst are added in batches to the reaction vessel to catalyze the CC coupling and hydrodeoxygenation processes, which results in energy waste and difficulty in catalyst separation. In addition, the reaction must be carried out in a solvent.
[0007] The present invention is proposed to solve the above-mentioned problems. Summary of the invention
[0008] In order to solve the above-mentioned deficiencies and shortcomings of the prior art, the present invention prepares MO x / NbOPO 4 Bifunctional catalyst; using the catalyst, high-density polycyclic alkane fuel can be synthesized in one pot without solvent. The raw material is phenolic compounds and / or aromatic alcohol compounds extracted from biomass lignin.
[0009] The technical solution of the present invention is as follows:
[0010] The first aspect of the present invention discloses a method for preparing a bifunctional catalyst, comprising the following steps:
[0011] (1) uniformly mixing a niobium source, tartaric acid and water to obtain a niobium tartrate aqueous solution;
[0012] (2) dissolving diammonium hydrogen phosphate in water;
[0013] (3) mixing the solutions obtained in step (1) and step (2), and adjusting the pH value with an acid;
[0014] (4) adding an aqueous solution of hexadecyltrimethylammonium bromide to the mixed solution of step (3);
[0015] (5) subjecting the mixed solution obtained in step (4) to hydrothermal crystallization in a high-pressure hydrothermal autoclave for a period of time, and then filtering the solid to obtain the solid and drying it;
[0016] (6) mixing the metal salt solution uniformly;
[0017] (7) mixing the solid dried in step (5) into the metal salt solution in step (6) at a certain temperature and mixing for a period of time;
[0018] (8) The solid obtained by separating the mixture in step (7) is dried and then calcined to obtain the bifunctional catalyst.
[0019] Preferably, the niobium source in step (1) is niobium hydroxide, and the mass ratio of the niobium source to tartaric acid is 1:(1-5); and in step (3), phosphoric acid is used to adjust the pH value so that the pH value is not greater than 2, preferably the pH value is equal to 1.
[0020] Preferably, the concentration of the aqueous solution of hexadecyltrimethylammonium bromide (CTAB) in step (4) is 5wt%-10wt%, and the mass ratio of hexadecyltrimethylammonium bromide to niobium hydroxide is 7:25. The main purpose of adding hexadecyltrimethylammonium bromide is to form pores in the catalyst; other surfactants can also be used as catalyst pores.
[0021] Preferably, the hydrothermal crystallization time of the mixed solution in step (5) is 12-26 hours at a temperature of 100-200° C.; and the drying is performed at 60-120° C. for 6-24 hours.
[0022] Preferably, the metal salt solution in step (6) is a metal salt solution of one or more of Pt, Pd, Ir, Ru, Rh, Au, Ni, Cu, Zn, Co, and Fe.
[0023] Preferably, the mixing temperature in step (7) is 25-100° C. and the mixing time is 1-10 h; wherein the amount of metal salt solution added is 0.5-6.0 wt % of the metal to the solid matter.
[0024] Preferably, the calcination temperature in step (8) is 350-650° C. and the calcination time is 3-10 h.
[0025] The second aspect of the present invention discloses the use of the bifunctional catalyst prepared by the preparation method for catalyzing a one-pot solvent-free reaction of lignin derivatives to obtain polycycloalkane fuel.
[0026] Preferably, the lignin derivative is a phenolic compound and / or an aromatic alcohol compound. The phenolic compounds mainly include phenol, anisole, guaiacol, etc., and the aromatic alcohols mainly include benzyl alcohol, diphenyl ether, etc.
[0027] Preferably, the one-pot solvent-free reaction to obtain polycycloalkane fuel includes alkylation reaction and hydrodeoxygenation reaction; the alkylation reaction conditions are: temperature 100-160°C, time 1-10h, speed>300rpm; the hydrodeoxygenation reaction conditions are: temperature 100-200°C, time 1-10h, speed>600rpm; no solvent is added during the entire reaction process. The bifunctional catalyst is used to catalyze the one-pot solvent-free reaction of lignin derivatives to obtain polycycloalkane fuel, which actually includes two steps of catalytic alkylation reaction and catalytic hydrodeoxygenation reaction. The catalyst of the present invention can catalyze both alkylation reaction and hydrodeoxygenation reaction, and plays a bifunctional role. The obtained polycycloalkane fuel is perhydrofluorene, dicyclohexylmethane or a mixture thereof.
[0028] Beneficial effects of the present invention:
[0029] 1. The preparation method of the present invention comprises the following steps: 4 The metal is introduced into the carrier process, using NbOPO 4 .nH 2 O was used as a carrier to impregnate metal salt solution to prepare MO with different metal impregnation amounts. x / NbOPO 4 Catalyst (MO x / NbOPO 4 means MOx Loaded on carrier NbOPO 4 Characterization shows that the catalyst MO x / NbOPO 4 MO exists 2 , MO-Nb and other active MO x The strong interaction between metal and acid sites makes the active metal sites preferentially loaded on the B acid sites. The applicant found that 3wt% RuO x / NbOPO 4 Catalyst (3wt% here means the numerator is the mass of metal Ru, the denominator is NbOPO 4 Each Ru site on the NbOPO 2 matches approximately 2.53 B acid sites. 4 and oriented distribution of RuO x The clear division of labor produces a strong synergistic effect, thus developing an ordered and enriched active site for catalyzing the one-pot solvent-free reaction of lignin derivatives platform molecules such as phenol and benzyl alcohol to obtain high-density polycyclic hydrocarbon fuels with high catalytic activity. (Note: 3wt% MO x / NbOPO 4 Catalyst, here 3wt% Here the numerator A is the mass of metal M, and the denominator is NbOPO 4 quality).
[0030] 2. The bifunctional catalyst obtained by the preparation method of the present invention is in the form of nanosheets, and the carrier NbOPO 4 Rich in surface defects and directional anchoring of MO x The platform molecules used to catalyze lignin derivatives such as phenol and benzyl alcohol can generate a mixture of perhydrofluorene and / or dicyclohexylmethane in one pot without solvent to obtain high-density polycycloalkane fuel; the reaction process is alkylation reaction and hydrodeoxygenation reaction, and the catalyst can catalyze both alkylation reaction and hydrodeoxygenation reaction, playing a dual-functional role.
[0031] 3. The preparation method of the present invention is based on the preparation of NbOPO in patent CN115920934A 4 Innovation and improvement based on NbOPO 4 It has excellent acidity and is used to catalyze alkylation reactions. 4 .nH 2 O is the carrier impregnated with metal salt solution to prepare MO with different metal impregnation amounts. x / NbOPO 4 The bifunctional catalyst of the present invention provides hydrogenation and acid sites on a single catalyst at the same time, and plays the role of two catalytic active sites in one reaction container, that is, a bifunctional role; its rich The acid accelerates the alkylation of oxygenated reactants to form fuel intermediates; in the hydrodeoxygenation step, part of the MO x In situ reduction to M metal, synergistic acid sites rapidly convert oxygen-containing intermediates into polycyclic alkanes such as perhydrofluorene and dicyclohexylmethane, thereby increasing the reaction rate. The bifunctional catalyst of the present invention has excellent metal-acid balance, catalyzes the one-pot solvent-free reaction of lignin derivatives (phenol and benzyl alcohol) to obtain high-density fuels such as perhydrofluorene with high yield and short reaction time, exhibits excellent catalytic activity, and plays a bifunctional catalytic role. BRIEF DESCRIPTION OF THE DRAWINGS
[0032] Figure 1 The 3wt%RuO prepared by x / NbOPO 4 Scanning electron microscope (SEM) photograph.
[0033] Figure 2 The 3wt%RuO prepared by x / NbOPO 4 Transmission electron microscope (TEM) photograph.
[0034] Figure 3 The NbOPO prepared by 4 and 1-4wt%RuO x / NbOPO 4 X-ray diffraction (XRD) pattern.
[0035] Figure 4 The NbOPO4 and 1-4wt%RuO prepared by the method are x / NbOPO 4 The infrared spectrum of pyridine reflecting B acid and L acid.
[0036] Figure 5 The 1-4wt% RuO prepared by the implementation x / NbOPO 4 The hydrogen temperature-programmed desorption test (H 2 -TPD). DETAILED DESCRIPTION
[0037] The present invention is described in detail below in conjunction with some specific embodiments. These embodiments are only used to illustrate the present invention and are not intended to limit the scope of the present invention. The embodiments in the examples are only preferred embodiments, but the present invention is not limited to the preferred embodiments.
[0038] Example 1: Preparation of bifunctional catalyst. x / NbOPO 4 For example, the mass of metal Ru is NbOPO 4The mass percentages are 1wt%, 2wt%, 3wt% and 4wt%. The steps are as follows:
[0039] (1) Under continuous magnetic stirring, 8.9 g of niobium hydroxide was slowly dissolved in an aqueous solution containing 18.75 g of tartaric acid; the solution was then transferred to a 100 mL volumetric flask; 0.66 g of diammonium hydrogen phosphate was dissolved in 10 mL of deionized water; 20 mL of tartaric acid solution was added to the diammonium hydrogen phosphate solution under vigorous stirring; the pH value was adjusted to about 1 with phosphoric acid; an aqueous solution of hexadecyltrimethylammonium bromide (CTAB) (the aqueous solution was prepared by dissolving 0.5 g of CTAB in 7.5 mL of distilled water, with a concentration of 6.25 wt%) was dropped into the mixed solution; the obtained solution was stirred at 45° C. for 10 h, and then hydrothermally crystallized at 160° C. for 24 h in an autoclave; after cooling, the solid was filtered, washed with distilled water, and dried at 105° C. for 5 h to remove moisture to obtain NbOPO 4 .nH 2 O powder;
[0040] Repeat the above steps to obtain NbOPO 4 .nH 2 O powder, and then calcined at 500 ° C for 5 h to obtain calcined NbOPO 4 ;
[0041] (2) Weigh 1 g of ruthenium chloride and dissolve it in water, then transfer the solution to a 100 mL volumetric flask. The concentration of the ruthenium chloride solution is 0.01 g / mL. Take 5 mL of the 0.01 g / mL ruthenium chloride solution and add it to the NbOPO obtained in step (1). 4 .nH 2 O powder, add 15 mL of deionized water, heat in a water bath at 65 ° C and stir for 3 h; then dry in a drying oven at 105 ° C for 10 h, and heat the obtained dry powder to 500 ° C at a rate of 5 ° C / min in an air atmosphere for calcination, and keep it for 5 h to remove the organic solvent; thus, 2 wt% RuO x / NbOPO 4 (2wt% here is metal Ru in NbOPO 4 The mass percentage of RuO is 2%. The same below) catalyst; by changing the volume of the 0.01 g / mL ruthenium chloride solution, the impregnation amount was changed to obtain 1wt% RuO x / NbOPO 4 、3wt%RuO x / NbOPO 4 and 4wt%RuO x / NbOPO 4 .
[0042] Figure 1 and Figure 2 The prepared 3wt%RuO x / NbOPO 4 Scanning electron microscope (SEM) and transmission electron microscope (TEM) images. Figure 1 It can be seen that the SEM images show that 3wt%RuO x / NbOPO 4 Uniform circular layered nanosheets with dense packing and random orientation; Figure 2 It can be seen that the TEM image shows that RuO x The presence of nanoparticles and the corresponding average particle size of about 2 nm, RuO x Preferential loading to the edge of the layered nanosheets, i.e., NbOPO 4 There are many defect sites around it, which can serve as preferential nucleation sites, thus forming a significant RuO x / NbOPO 4 Particles on the surface.
[0043] Figure 3 The prepared NbOPO 4 and 1-4wt%RuO x / NbOPO 4 X-ray diffraction pattern (XRD) of the sample. Figure 3 It can be seen that with the increase of Ru impregnation amount, the 4 Compared with the diffraction peak, the crystallinity is slightly increased, and the degree of deviation from 2θ=28.4° to a lower angle is gradually increasing. This may be due to the increasing content of Ru-O-Nb bonds and the increasing degree of interaction between Ru-O-Nb bonds. 2 The diffraction peaks of the RuO nanoparticles were determined by 2θ=35.1°(101) and 54.2°(211) (PDF#40-1290), indicating that the Ru particles have been successfully deposited on the support surface and that the main forms of Ru are RuO 2 and Ru-O-Nb; with the increase of Ru impregnation amount, RuO 2 The diffraction peaks become increasingly obvious.
[0044] Figure 4 and Figure 5 The prepared NbOPO 4 and 1-4wt%RuO x / NbOPO 4 Pyridine Fourier transform infrared spectrum (Py-IR) and hydrogen programmed temperature desorption test (H 2 -TPD). Figure 4 1wt%RuO calculated from Py-IR data x / NbOPO 4, 2wt%RuO x / NbOPO 4 、3wt%RuO x / NbOPO 4 and 4wt%RuO x / NbOPO 4 The B acid content was 58.13 μmol gcat -1 、36.41μmol gcat -1 、23.46μmol gcat -1 and 20.22 μmol gcat -1 ;according to Figure 5 H 2 - 1wt%RuO calculated from TPD data x / NbOPO 4 , 2wt%RuO x / NbOPO 4 、3wt%RuO x / NbOPO 4 and 4wt%RuO x / NbOPO 4 The number of accessible metal centers was 39.50 μmol gcat -1 、48.23μmol gcat -1 、59.37μmol gcat -1 and 60.89 μmol gcat -1 This indicates that with the increase of loading, the B acid sites gradually decrease while the metal content gradually increases.
[0045] Table 1 is the quantitative data of the metal acid sites of the bifunctional catalyst prepared in the embodiment. The applicant found that as a bifunctional catalyst, the conversion rate of benzyl alcohol in the alkylation process, the selectivity of the oxygen-containing intermediate benzylphenol, and the conversion rate of benzylphenol in the hydrodeoxygenation process, the selectivity of perhydrofluorene and even the product distribution are closely related to the synergistic effect of the metal and acid center. Metal-acid balance (MAB), that is, the ratio of surface metal sites to B acid sites (nRu / nBAS, taking metal Ru as an example), can determine the alkylation, hydrodeoxygenation activity and product distribution in a one-pot solvent-free conversion process. Only the concentration of B acid sites was used in calculating MAB because they are mainly responsible for the alkylation process of phenol and benzyl alcohol and the alcohol dehydration process of the hydrodeoxygenation process. In order to study the effect of MAB on the catalytic reaction activity of the catalyst, MAB was adjusted by changing the loading amount of metal Ru; the result was that the loading amount of metal Ru increased from 1wt% to 4wt%, and MAB varied between 0.68 and 3.01, so as to quantitatively study RuO x / NbOPO 4The synergistic effect of the catalyst on the one-pot solvent-free conversion of benzyl alcohol and phenol into polycyclic alkane fuels. For this reaction system, there is no rate-limiting step, and the alkylation reaction and hydrodeoxygenation reaction are completed sequentially, so the metal Ru and acid balance of the bifunctional catalyst needs to reach a suitable MAB. The applicant unexpectedly discovered that a low Ru loading is not enough to provide enough metal sites for effective hydrodeoxygenation, and more Ru particles will block the channels and pores of the acidic carrier, resulting in the inhibition of the alkylation reaction; because with the increase of metal loading, the metal sites gradually increase, while the B acid sites gradually decrease. Therefore, a suitable MAB can play a bifunctional role in catalysis.
[0046] Table 1 1-4wt%RuO x / NbOPO 4 Catalyst B acid content, metal content and nRu / nBAS
[0047] serial number catalyst B acid content (μmol / g) Metal content (μmol / g) nRu / nBAS 1 <![CDATA[1wt%RuO x / NbOPO 4 ]]> 58.13 39.50 0.68 2 <![CDATA[2wt%RuO x / NbOPO 4 ]]> 36.41 48.23 1.32 3 <![CDATA[3wt%RuO x / NbOPO 4 ]]> 23.46 59.37 2.53 4 <![CDATA[4wt%RuO x / NbOPO 4 ]]> 20.22 60.89 3.01
[0048] According to the steps of Example 1, 3 wt% PtO x / NbOPO 4 and 3wt%NiO x / NbOPO 4 Bifunctional catalyst.
[0049] As a comparison, 3 wt% RuO x / S-NbOPO 4 The steps are: NbOPO obtained in step (1) of Example 1 4 .nH 2 O powder was calcined at 500 °C for 5 h to obtain calcined NbOPO 4 ; 7.5 mL of 0.01 g / mL ruthenium chloride solution was added, and then 15 mL of deionized water was added, and the mixture was heated in a water bath at 65°C and stirred for 3 h; then dried in a drying oven at 105°C for 10 h; the obtained dried powder was calcined at 500°C in an air atmosphere, and the temperature was increased at a rate of 5°C / min and maintained for 5 h to remove the organic solvent; thus, 3 wt% RuO x / S-NbOPO 4 catalyst.
[0050] Example 2: The above catalyst was used to catalyze the one-pot solvent-free reaction of lignin-derived molecules phenol and benzyl alcohol to prepare high-density fuel. The reaction was carried out in a 50 mL stainless steel batch reactor. The steps are as follows: 139.8 mmol phenol, 34.8 mmol benzyl alcohol and 0.6 g of the above catalyst were added to the reactor, and the catalyst accounted for 3.5 wt% of the reactants; the temperature was raised to 130 ° C and the alkylation reaction was carried out at a stirring speed of 800 rpm in an air atmosphere for 2 hours; then N 2Purge 3 times to ensure the airtightness of the device and then use H 2 Purge 3 times and fill with 6MPa H 2 , in H 2 The temperature was raised to 160°C under the atmosphere and the stirring speed was 800 rpm for hydrodeoxygenation reaction for 1 hour. After the reaction was completed, the reaction mixture was extracted with a syringe, and a filter head containing an organic filter membrane was installed to squeeze the extracted solution into a chromatographic vial to perform chromatographic analysis on the product. The product was subjected to reduced pressure distillation to obtain a fuel sample, and its fuel performance was tested. The results are shown in Table 2 below.
[0051] Table 2 Hydrodeoxygenation of phenol and benzyl alcohol in one-pot solvent-free reaction catalyzed by different catalysts
[0052] Serial number catalyst Yield of perhydrofluorene and dicyclohexylmethane 1 <![CDATA[1wt%RuO x / NbOPO 4 ]]> 3.8 2 <![CDATA[2wt%RuO x / NbOPO 4 ]]> 45.9 3 <![CDATA[3wt%RuO x / NbOPO 4 ]]> 78.3 4 <![CDATA[4wt%RuO x / NbOPO 4 ]]> 58.2 5 <![CDATA[3wt%RuO x / S-NbOPO 4 ]]> 18.0 6 <![CDATA[3wt%PtO x / NbOPO 4 ]]> 51.0 7 <![CDATA[3wt%NiO x / NbOPO 4 ]]> 30.0 8 <![CDATA[NbOPO 4 ]]> 0 9 <![CDATA[NbOPO 4 +Ru / C]]> 6.1 10 <![CDATA[NbOPO 4 +Ru / C]]> 82.0
[0053] [Note] In Table 2, catalyst No. 8 is NbOPO 4 The calcined NbOPO was obtained by calcining at 500℃ for 5h. 4 Catalyst No. 9: NbOPO 4 +Ru / C is the yield of the catalyst of patent CN115920934A under the experimental conditions. Catalyst No. 10 NbOPO4+Ru / C is the yield of the catalyst of patent CN115920934A after alkylation reaction and hydrodeoxygenation reaction at 180°C for 6-10h.
[0054] It can be seen from Table 2 that RuO x / NbOPO 4 Better activity than other MOs x / NbOPO 4 Activity: 3wt%RuO x / NbOPO 4 The best activity.
[0055] It can also be seen from Table 2 that 3wt%RuO x / S-NbOPO 4 Ratio of 3wt%RuO x / NbOPO 4 The activity decreased significantly, which may be due to the reaction of Ru with calcined NbOPO during the impregnation process. 4 This is due to the weak interaction between the carrier and the catalyst. This indicates that the bifunctional catalyst prepared by the preparation method of the present invention has excellent activity.
[0056] It can also be seen from Table 2 that only NbOPO 4 The catalyst cannot undergo hydrodeoxygenation to obtain the final product, polycycloalkane fuel; Ru / C catalyst needs to be added after the alkylation reaction is completed. 4Only by physically mixing with Ru / C can the hydrodeoxygenation reaction be completed to obtain multi-cycloalkane fuel; and the final fuel yield is still low (6.1%) under the experimental conditions (alkylation reaction at 130℃ for 2h; hydrodeoxygenation reaction at 160℃, 6MPa for 1h). To obtain a higher fuel yield, Ru / C catalyst is added after the alkylation reaction is completed, and the hydrodeoxygenation reaction is carried out at a higher temperature of 180℃ for 6-10h to overcome the energy barrier of the hydrodeoxygenation reaction; that is, when the molar ratio of phenol to benzyl alcohol is 4:1, after the alkylation reaction at 130℃ for 2h, Ru / C catalyst is added, and the hydrodeoxygenation reaction is carried out at 180℃ for 6-10h to obtain a higher yield of perhydrofluorene and dicyclohexylmethane (82.0%). This shows that only NbOPO 4 The catalyst has no bifunctional effect, and the MO of the present invention x / NbOPO 4 The catalyst has a bifunctional effect.
[0057] 3wt%RuO x / NbOPO 4 After the final product was subjected to vacuum distillation, the fuel composition was 76% perhydrofluorene, 11% dicyclohexylmethane, 3% other two-ring products, and 10% other three-ring products. The measured fuel density was 0.9594 g / mL.
[0058] The above is only used to introduce the specific implementation methods of the present invention in detail, but the technical solution proposed by the present invention is not limited to the above method. Without departing from the basic principles of the present technology, equivalent modifications and changes made by those skilled in the art to the technology proposed by the present invention should be included in the scope of the claims of the present invention.
Claims
1. A method for preparing a bifunctional catalyst, It is characterized in that The steps include: (1) uniformly mixing a niobium source, tartaric acid and water to obtain a niobium tartrate aqueous solution; (2) dissolving diammonium hydrogen phosphate in water; (3) mixing the solutions obtained in step (1) and step (2), and adjusting the pH value with an acid; (4) adding an aqueous solution of hexadecyltrimethylammonium bromide to the mixed solution of step (3); (5) subjecting the mixed solution obtained in step (4) to hydrothermal crystallization in a high-pressure hydrothermal autoclave for a period of time, and then filtering the solid to obtain the solid and drying it; (6) mixing the metal salt solution uniformly; (7) mixing the solid dried in step (5) into the metal salt solution in step (6) at a certain temperature and mixing for a period of time; (8) The solid separated from the mixture in step (7) is dried and then calcined to obtain the bifunctional catalyst.
2. The preparation method according to claim 1, It is characterized in that The niobium source in step (1) is niobium hydroxide, and the mass ratio of the niobium source to tartaric acid is 1:(1-5); and in step (3), phosphoric acid is used to adjust the pH value so that the pH value is not greater than 2.
3. The preparation method according to claim 2, It is characterized in that The concentration of the aqueous solution of cetyltrimethylammonium bromide (CTAB) in step (4) is 5wt%-10wt%, and the mass ratio of cetyltrimethylammonium bromide to niobium hydroxide is 7:
25.
4. The preparation method according to claim 1, It is characterized in that In step (5), the mixed solution is hydrothermally crystallized for 12-26 hours at a temperature of 100-200° C.; and dried at 60-120° C. for 6-24 hours.
5. The preparation method according to claim 1, It is characterized in that The metal salt solution in step (6) is a metal salt solution of one or more of Pt, Pd, Ir, Ru, Rh, Au, Ni, Cu, Zn, Co, and Fe.
6. The preparation method according to claim 1, It is characterized in that The mixing temperature in step (7) is 25-100° C. and the mixing time is 1-10 h. The amount of metal salt solution added is 0.5-6.0 wt % of the metal to the solid matter.
7. The preparation method according to claim 1, It is characterized in that The calcination temperature in step (8) is 350-650° C. and the calcination time is 3-10 h.
8. Use of the bifunctional catalyst prepared by the preparation method according to any one of claims 1 to 7 for catalyzing a one-pot solvent-free reaction of lignin derivatives to obtain polycycloalkane fuels.
9. The use according to claim 8, It is characterized in that The lignin derivatives are phenolic compounds and / or aromatic alcohol compounds.
10. The use according to claim 8, It is characterized in that The one-pot solvent-free reaction to obtain polycyclic alkane fuel includes alkylation reaction and hydrodeoxygenation reaction; the alkylation reaction conditions are: temperature 100-160°C, time 1-10h, speed>300rpm; the hydrodeoxygenation reaction conditions are: temperature 100-200°C, time 1-10h, speed>600rpm.
Citation Information
Patent Citations
Ru-Ni / NbOPO4 bimetallic catalyst as well as preparation method and application thereof
CN113649036A
Method for preparing 1, 14-tetradecane glycol from biomass derivative
CN114230437A
Cycloalkane fuel and preparation method thereof
CN115418246A
Preparation method of niobium phosphate catalyst and application of niobium phosphate catalyst in high-density fuel synthesis
CN115920934A
Ni-Nb-P non-supported catalyst, preparation method and application thereof
CN118268011A