Preparation method of resin-assisted atomization molded boron nitride-based complex-phase spherical material

By combining boron nitride with other ceramic particles in spray granulation technology using boron nitride frame precursor resin, the binding problem of boron nitride that is difficult to sinter at high temperature and other nitrides or oxides is solved, and efficient preparation is achieved The dense boron nitride matrix composite spherical material improves mechanical strength and thermal stability.

CN118929586AActive Publication Date: 2024-11-12HEBEI UNIV OF TECH

Patent Information

Application Number
CN202411123847.9
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-08-16
Publication Date
2024-11-12
Estimated Expiration
2044-08-16

AI Technical Summary

Technical Problem

The prior art is difficult to effectively combine boron nitride with other nitrides or oxides at high temperatures to prepare composite ceramic microspheres, resulting in limited development of boron nitride-based composite ceramics.

Method used

Using a boron nitride frame precursor resin that can act as a bonding agent at low temperatures, other ceramic particles are agglomerated and connected by spray granulation technology, pyrolyzed at high temperatures to form a boron nitride phase, and with other nitrides or oxides The particles are bonded by nitriding or covalent bonding to form a dense complex spherical material.

Benefits of technology

It realizes the efficient preparation of boron nitride-based composite spherical materials, improves spherical shape, purity and mechanical strength, simplifies the process flow, reduces costs and safety risks, and is suitable for large-scale production.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118929586A_ABST
    Figure CN118929586A_ABST
Patent Text Reader

Abstract

The invention relates to a preparation method of a resin-assisted atomization molded boron nitride-based complex-phase spherical material, which comprises the following steps: uniformly mixing an aqueous solution of an aldehyde group-containing organic matter, an amino-containing compound, a boron-oxygen-containing compound and water under a heating condition to obtain high-fluidity uniform liquid resin; adding nitride powder or nano oxide into the uniform liquid resin, and uniformly stirring to obtain mixed slurry which contains the nitride powder or nano oxide and has the solid content of 10-30 wt% and the viscosity of 500-3000 mPa.S; and carrying out atomized particle drying molding on the mixed slurry, carrying out hot drying treatment, and carrying out high-temperature heat treatment in a protective atmosphere environment, so that the resin component is converted into a boron nitride phase after being subjected to high-temperature pyrolysis and in-situ nitridation reaction, thereby obtaining the boron nitride-based complex-phase spherical material. According to the method, a precursor sphere is formed through a resin adhesive, a BN phase is formed through high-temperature pyrolysis and nitridation is carried out, and the problem of high-temperature sintering of BN and other nitrides is solved.
Need to check novelty before this filing date? Find Prior Art

Description

Technical field:

[0001] The invention relates to the technical field of synthesis of high-end powder materials of advanced nitride ceramics and composite ceramics thereof, and in particular to a method for preparing a resin-assisted atomization-molded boron nitride-based composite spherical material. Background technology:

[0002] Ceramic microspheres have important application potential in materials science due to their high thermal conductivity, mechanical strength, wear resistance and chemical stability. They can significantly improve the thermal conductivity of electronic packaging and the automotive industry, enhance the strength and wear resistance of composite materials, and be used as catalyst carriers. 3D printing bionic materials in the biomedical field and coating materials in high temperature and corrosive environments can also benefit from the excellent properties of ceramic microspheres. The development of new ceramic microspheres and their composite materials will promote technological progress and innovation in related industries.

[0003] At present, the research and development of boron nitride-based composite phase ceramic microsphere particles are relatively small, although spherical ceramic particles have high application potential and advantages in many fields. In fact, the preparation of boron nitride and other nitrides (such as Si3N4 or AlN) or oxides into composite microspheres faces many challenges, mainly because of the failure to find an effective bonding strategy or adhesive raw materials. Due to the very high chemical inertness of the surface of BN particles and other nitride or oxide particles, it is difficult to carry out effective mass transfer bonding at high temperatures, making it difficult to prepare and develop composite phase microsphere ceramic particles containing boron nitride components, which greatly limits the development of boron nitride-based ceramic microsphere particles. Therefore, it is particularly important to develop new methods to overcome these difficulties and prepare nitride composite ceramic microspheres containing BN components with excellent performance to open up the wide application of boron nitride and its composite ceramics. This will not only fill the current technical gap, but also provide significantly broader convenience and broad practicality for the application of nitride ceramics.

[0004] In view of the above problems, the present invention proposes an innovative method, using a precursor resin that can act as a spray particle adhesive at low temperature and can be nitrided at high temperature to form a boron nitride framework that connects nitride particles to each other. With the help of this resin, the problem of high-temperature chemical inertness of boron nitride particles and difficulty in compounding with other ceramics is overcome, and the industrial synthesis and output of nitride composite ceramic microspheres are significantly promoted, which will help to improve the application of boron nitride and its composite ceramic microspheres. Summary of the invention:

[0005] The present invention aims to provide a method for preparing a resin-assisted atomization-molded boron nitride-based multiphase spherical material. By means of spray granulation technology, the resin is used as a binder to agglomerate and connect other ceramic particles to form a spherical precursor, and the resin is pyrolyzed at high temperature to form a boron nitride phase, and through the pyrolysis nitridation process, other nitride or oxide particles in the precursor sphere are nitrided to form bonds or covalent bonds with boron nitride on their particle edges / external surfaces, thereby forming dense boron nitride-based multiphase spherical particles with unchanged morphology.

[0006] The technical solution for achieving the purpose of the present invention is as follows:

[0007] In a first aspect, the present invention provides a method for preparing a multiphase spherical material based on boron nitride by resin-assisted atomization molding, the preparation method comprising the following steps:

[0008] (1) mixing an aldehyde-containing organic aqueous solution, an amino compound, a boron oxide compound, and water under heating conditions to obtain a uniform liquid resin with high fluidity; the viscosity of the uniform liquid resin is greater than the viscosity of water and is not greater than 50 mPa·s;

[0009] (2) adding nitride powder or nano-oxide to the above uniform liquid resin, stirring evenly, to obtain a mixed slurry containing nitride powder or nano-oxide with a solid content of 10wt%-30wt% and a viscosity of 500-3000mPa·S;

[0010] (3) atomizing the mixed slurry to form particles by drying, and then performing a heat drying treatment at 100-500° C. to obtain a composite phase spherical precursor particle powder having a spherical morphology;

[0011] (4) The composite phase spherical precursor particle powder is heat treated in a protective atmosphere environment within a temperature range of 1100-1800° C., so that the resin component is transformed into a boron nitride phase after high-temperature pyrolysis and in-situ nitridation reaction, thereby obtaining a boron nitride-based composite phase spherical material.

[0012] Furthermore, in step (1), the ratio of the amount of additional water added (in milliliters) to the amount of the aldehyde-formylating organic aqueous solution (in milliliters) is in the range of 0.5-5; the molar ratio of the amino compound to the boron oxide compound is 1:(0.2-2); the heating temperature is 45°C to 95°C, and the mixture is stirred evenly for 0.2 to 96 hours until a uniform liquid resin is obtained.

[0013] The solid content in step (2) refers to the ratio of the mass of the nitride powder or nano-oxide to the mass of the total mixture.

[0014] Furthermore, in step (3), the mixed liquid resin whose temperature is maintained in the range of 25°C to 90°C is blown into an atomizing drying granulator with air as hot air drying airflow in the temperature range of 120°C to 300°C at a creeping feed rate of 1mL / min-50mL / min for atomizing particle drying and forming to obtain a fluffy white powder with a little moisture, and then further heat-dried in a hot air flow oven at 100°C to 500°C for 1-48 hours to obtain a composite phase spherical precursor particle powder with spherical morphology characteristics.

[0015] Preferably, the heating / cooling rate range of the heat drying treatment in step (3) is 1-20°C / min, and the heat drying gas flow is air, nitrogen, or a mixture of nitrogen and air with an air content of no more than 5% by volume.

[0016] Furthermore, the aldehyde-containing organic aqueous solution in step (1) is a solution formed by dissolving formaldehyde or acetaldehyde in a water solvent; wherein the content of formaldehyde or acetaldehyde in water is not less than 30 wt.%;

[0017] The boron-oxygen compound is at least one of boron trioxide, boric acid or borax.

[0018] Furthermore, the amino-containing compound in step (1) is a nitrogen-containing compound containing an amino group, which is at least one of a guanidine-containing compound, an azole-containing nitrogen-containing compound, and a triazine-containing nitrogen-containing compound; the guanidine-containing compound is at least one of guanidine carbonate, cyanoguanidine, aminoguanidine, and aminoguanidine bicarbonate.

[0019] The azole-containing nitrogen-containing compound is 3-amino-1,2,4-triazole, and the triazine-containing nitrogen-containing compound is melamine;

[0020] When the system contains triazine nitrogen-containing compounds or azole nitrogen-containing compounds, a crosslinking inhibitor is added to the system to prevent the system from agglomerating and maintain a uniform liquid resin state.

[0021] Furthermore, the nitride powder is at least one of boron nitride nanosheets, boron nitride nanoparticles, amorphous boron nitride powder, boron nitride micrometers or nanometer fibers, commercial boron nitride powder, aluminum nitride micrometers or nanometer powders, and silicon nitride micrometers or nanometer powders; the nano oxide is at least one of titanium oxide, silicon dioxide, aluminum oxide, lanthanum oxide, molybdenum oxide, cerium oxide, zirconium oxide, yttrium oxide, or magnesium oxide.

[0022] Furthermore, the particle plane size distribution range of the commercial boron nitride powder is 5 to 30 microns; the average particle size of the aluminum nitride micron powder is 1 to 10 microns; and the average particle size of the silicon nitride micron powder is 1 to 10 microns.

[0023] Furthermore, in the step (4), the heating / cooling rate of the heat treatment is 5-100°C / min, the air flow rate is 10-2000ml / min, and the protective atmosphere is nitrogen, ammonia+nitrogen or ammonia;

[0024] Wherein, the atmosphere for heat treatment in the temperature range of 1500-1800°C is nitrogen;

[0025] The atmosphere for the heat treatment within the temperature range of 1100-1400° C. is ammonia or ammonia+nitrogen.

[0026] In the second aspect, the present invention provides a resin-assisted atomization formed boron nitride-based complex phase spherical material, which is obtained by the preparation method. The boron nitride-based complex phase spherical material is a composite phase spherical particle of boron nitride and aluminum nitride, a composite phase spherical particle of boron nitride and silicon nitride, a composite phase spherical particle of boron nitride and boron nitride, or a composite phase spherical particle of boron nitride and oxide, and its boron nitride phase is a hexagonal boron nitride phase.

[0027] The particle size distribution range of the boron nitride-based multiphase spherical material of the present invention extends from several microns to more than one hundred microns, and the spherical particles have high sphericity, high purity, and firm and dense multiphase connection.

[0028] The spray dryer involved in the present invention is an industrial-grade commonly used atomizing drying granulator, and there is no transformation or modification of the equipment.

[0029] Compared with the prior art, the present invention has the following beneficial effects:

[0030] The resin provided by the present invention can be directly transformed into a boron nitride (BN) phase at high temperature. In the high temperature process, the directly carried out nitridation reaction can realize a strong nitridation bonding action on the edge or surface of the original nitride particles, so that the obtained complex phase other nitride particles or nano oxides can be well densely combined with the BN phase components to form a spherical structure of the complex phase components with a high-strength bonding interface.

[0031] The method of the present invention creatively introduces the BN component, which is difficult to sinter into a whole with other nitrides, into the spherical precursor in the form of a resin precursor with high bonding ability. During the high-temperature pyrolysis-nitridation process, these resin precursors can form a stable combination, thereby solving the technical problem of not being able to composite multiple types of nitrides into balls in the past.

[0032] The method of the present invention has a simple process flow, does not require complicated process steps, and significantly simplifies the preparation process. The raw materials used are low in cost, easy to obtain, and have significant economic benefits. The required equipment is simple, does not require special design and modification, and is suitable for large-scale production. In the high-temperature pyrolysis process, the method of the present invention has high safety and reduces the potential safety hazards in high-temperature operations.

[0033] The product obtained by the present invention has high sphericity and high crystallinity, and the complex phase components are stable and will not change. These characteristics enable the present invention to provide a high raw material basis for the production of complex phase nitride bulk ceramics and the formation of complex phase nitride coatings, with high economic value and strong universality.

[0034] The method of the present invention effectively solves the problem that BN and other nitrides are difficult to sinter and connect at high temperatures. During the high-temperature in-situ nitridation or pyrolysis process, the resin is converted into a stable BN phase, which serves as a connecting framework for other nitride particles, ensuring the close bonding of BN and other nitride particles during high-temperature sintering, and finally forming a dense spherical sphere. This not only improves the mechanical strength and thermal stability of the sphere, but also solves the problem that it is difficult to maintain a spherical structure at high temperatures in traditional methods.

[0035] The resin provided by the present invention has the characteristics of flexible and controllable composition, which is convenient for supporting the preparation of highly spherical and controllable particle size nitride complex phase spherical. The obtained product has the characteristics of high crystallinity, low porosity, high strength and high density. The synthesis process is simple and easy to operate, the production steps are simple, the energy consumption is saved, and it has significant economic benefits. Description of the drawings:

[0036] In order to more clearly introduce the technical solutions and product types of the present invention, the drawings required for use in the description of the embodiments are briefly elaborated and illustrated below. It should be emphasized that these illustration examples are only part of the embodiments of the present invention. For ordinary technicians in this field, without paying creative work, these are likely to extend and multiply to other similar and related illustration examples. In the event that similar and similar illustrations are used as new creative embodiments, they are deemed to be infringements of the present invention.

[0037] Figure 1 The powder XRD diffraction patterns of the nitride complex phase spherical products formed by boron nitride and silicon nitride respectively obtained at 1100° C. and 1500° C. in nitrogen in Example 1;

[0038] Figure 2 This is a SEM image of a nitride composite spherical product formed by boron nitride and silicon nitride obtained at 1100° C. in nitrogen in Example 1;

[0039] Figure 3This is a SEM image of a nitride composite spherical product formed by boron nitride and silicon nitride obtained at 1500° C. in nitrogen in Example 1;

[0040] Figure 4 The powder XRD diffraction patterns of the homogeneous nitride composite spherical products formed by boron nitride and boron nitride nanosheets respectively obtained at 1100° C. and 1500° C. in nitrogen in Example 2;

[0041] Figure 5 This is a SEM image of a spherical product of a homogeneous nitride composite formed by boron nitride and boron nitride nanosheets obtained at 1100° C. in nitrogen in Example 2;

[0042] Figure 6 This is a SEM image of a spherical product of a homogeneous nitride composite formed by boron nitride and boron nitride nanosheets obtained at 1500° C. in nitrogen in Example 2;

[0043] Figure 7 Powder XRD diffraction patterns of boron nitride and boron nitride nanospheres obtained in nitrogen at 1500° C. in Examples 3 and 4, and spherical products of homogeneous nitride complex phase composites formed with boron nitride commercial bulk powder;

[0044] Figure 8 This is a SEM image of a spherical product of a homogeneous nitride composite formed by boron nitride and boron nitride nanospheres obtained at 1500° C. in nitrogen in Example 3;

[0045] Fig. 9 This is a SEM image of a spherical product of a homogeneous nitride composite formed by boron nitride and boron nitride commercial bulk powder obtained at 1500° C. in nitrogen in Example 4;

[0046] Fig.10 The powder XRD diffraction patterns of the pure boron nitride microsphere particle powder products obtained at 1100° C. and 1500° C. in nitrogen in Example 5;

[0047] Fig.11 The SEM images of the pure boron nitride microsphere particle powder product obtained at 1100° C. and 1500° C. in nitrogen in Example 5;

[0048] Fig.12 This is a SEM image of the pure boron nitride microsphere particle powder product obtained at 1100° C. in ammonia in Example 6;

[0049] Fig.13 This is a SEM image of the pure boron nitride microsphere particle powder product obtained at a nitrogen temperature of 1100° C. in Example 7;

[0050] Fig.14 XRD diffraction patterns of nitride complex phase spherical products formed by boron nitride and aluminum nitride obtained at 1100° C. and 1500° C. in nitrogen in Example 8;

[0051] Fig.15 This is a SEM image of a nitride composite spherical product formed by boron nitride and aluminum nitride obtained at 1100° C. in nitrogen in Example 8;

[0052] Fig.16 This is a SEM image of the nitride complex spherical product formed by boron nitride and aluminum nitride obtained at 1500°C in nitrogen in Example 8. Specific implementation method:

[0053] In order to better help technical professionals in the field understand the present invention, the details of the present invention will be further described in detail in conjunction with actual examples and the method mechanism of the present invention will be further analyzed and explained. It should be emphasized that the following examples are only used to more clearly illustrate the present invention and should not be construed as any limitation to the scope of protection of the present invention. Professionals in the technical field can make various improvements and adjustments based on the content of the present invention, and these improvements and adjustments should still be included in the scope of protection of the present invention.

[0054] Unless otherwise defined, the professional terms used in the present invention are consistent with the meanings commonly understood by those skilled in the art. Various raw materials, reagents, instruments, equipment and some consumable materials used in the present invention can be purchased from the market or can be prepared by existing methods.

[0055] The present invention will be further described below in conjunction with embodiments:

[0056] The present invention is a method for preparing a multiphase spherical material based on boron nitride by resin-assisted atomization molding, which includes the following four steps:

[0057] Step (1): mixing an aldehyde-containing organic aqueous solution, an amino compound, a boron oxide compound, and water under heating conditions to obtain a uniform liquid resin with high fluidity; the viscosity of the uniform liquid resin is greater than the viscosity of water and is not greater than 50 mPa·S;

[0058] The amino compound is at least one of guanidine carbonate, cyanoguanidine, aminoguanidine, aminoguanidine bicarbonate, etc.; the boron-oxygen compound is at least one of boron trioxide, boric acid or borax, etc.;

[0059] The heating temperature is 45°C to 95°C, and the mixture is stirred evenly for 0.2 to 20 hours until a uniform liquid resin is obtained.

[0060] Preferably, the aldehyde-containing organic matter aqueous solution is a solution formed by dissolving formaldehyde or acetaldehyde in a water solvent; wherein the content of formaldehyde or acetaldehyde in water is not less than 30 wt.%.

[0061] The reaction mechanism for forming a uniform liquid resin with high fluidity during this step is: assuming that the amino compound is R-NH2 and the organic compound containing an aldehyde group is R-CHO, the two undergo a condensation reaction. The nitrogen atom in the amino group (-NH2) of the amino compound is a nucleophilic reagent with a lone pair of electrons. When it encounters the carbon atom in the aldehyde group (-CHO), it can form an unstable combination and lose a molecule of water to form an imine bond (C=N). Therefore, in this reaction, a large number of imine bond intermediates and water are first generated. Subsequently, this intermediate containing multiple imine bonds undergoes an esterification reaction with the hydroxyl group in the boric acid, and a water byproduct is produced, forming a cross-linked structure containing BO bridge bonds, and forming a resin containing a BO connection network with a low degree of cross-linking. Since the degree of cross-linking of the resin is not high, it exhibits a certain fluidity. By adjusting the amount of water, the resin can be prepared into a resin colloid with high fluidity.

[0062] Step (2): adding nitride powder or nano-oxide into a uniform liquid resin and stirring the mixture to obtain a mixed liquid resin;

[0063] Among them, the nitride powder is boron nitride, aluminum nitride or silicon nitride powder, etc.; the nano oxide is at least one of titanium oxide, silicon dioxide, aluminum oxide, lanthanum oxide, molybdenum oxide, cerium oxide, zirconium oxide, yttrium oxide or magnesium oxide, etc.

[0064] After the two are uniformly stirred at a temperature range of 25-95° C. for 0.1-10 hours, a mixed liquid resin containing corresponding particles uniformly dispersed in the uniform liquid resin is obtained. The mixed liquid resin is still in a liquid state, similar to an emulsion, and is called a mixed slurry.

[0065] During this step, the uniform liquid resin is a low-crosslinked, high-fluidity resin that can react with the surface of these nitride powders or nano-oxides, so that these nitride powders or nano-oxides form a relatively uniform, unified mixed phase in the resin glue without any signs of stratification, agglomeration, and phase separation, thereby achieving highly dispersed, unified mixing.

[0066] Step (3): atomizing the mixed liquid resin into particles and drying them, and then performing a heat drying treatment at 100-500° C. to obtain a composite spherical precursor particle powder having a spherical morphology;

[0067] Specifically, a mixed liquid resin whose temperature is maintained in the range of 25-90°C is blown into an atomizing drying granulator with air as a hot air drying airflow in the temperature range of 120-300°C at a peristaltic feeding rate of 1-50mL / min for atomizing particle drying and forming to obtain a fluffy white powder with a little moisture. After the powder is heat-dried in a hot air flow oven at 100-500 degrees Celsius for 1-48 hours, a complex phase spherical precursor particle powder with spherical morphology characteristics is obtained.

[0068] In this step, the uniformly dispersed nitride powder or nano-oxide forms a bond with the resin molecules, so that the nitride powder or nano-oxide is uniformly dispersed in the mist droplets formed during the spraying process. In the hot air flow, the mist droplets are rapidly dehydrated and dried to form spherical particles with the lowest energy shape. These spheres are organic / inorganic polymer composite structures with the solidified resin as the connecting framework and the nitride powder or nano-oxide as the filling phase, that is, a multi-phase spherical precursor particle powder with spherical morphology characteristics is formed.

[0069] The further heat drying process of the resin is to strengthen and enhance the curing of the resin in the spherical particles. The curing mechanism is: under heating conditions, each monomer in the low-crosslinked resin is further crosslinked to form a high-crosslinked structure. The residual amino and aldehyde groups in each monomer will react with the reaction sites of the adjacent monomers to generate more imine bonds. The hydroxyl group of the boric acid still reacts with the imine intermediate to form a new boron oxygen bridge (BO), so that the monomers are connected to each other through the BO bridge. Through multiple crosslinking reactions, multiple monomers are connected together, resulting in the formation of a stable high-crosslinked three-dimensional network structure of solid resin. The high-crosslinked three-dimensional network structure of the solid resin contains a large number of boron oxygen (BO) bridge bonds and forms a small amount of BN bonds.

[0070] Step (4): The composite spherical precursor particle powder is heat treated in a protective atmosphere at a temperature range of 1100-1800°C, so that the resin is transformed into a boron nitride phase after high-temperature pyrolysis and in-situ nitridation reaction (see Figure 10-13 ), and obtain a boron nitride-based composite spherical material (see Figure 2 , 3 , 5, 6, 8, 9, 15 and 16).

[0071] Under nitrogen at high temperature in the range of 1500-1800℃, the cured resin in the precursor sphere will be thermally decomposed to generate small molecular waste gas containing hydrogen, carbon, nitrogen and oxygen and leave the spherical reaction zone. Since the BO bonds will be nitrided to BN bonds at the same time, the newly formed BN components in the surrounding will be firmly connected to these filled boron nitride, aluminum nitride or silicon nitride particles in combination with the already formed BN bonds, ensuring that the spherical nitride composite particles with unchanged structure are formed at the BN connection interface, and at the same time ensuring the stability of the crystal phase of aluminum nitride particles, silicon nitride particles and boron nitride particles (see Figure 1 , Figure 4 and Figure 7 The strong diffraction calibration peak of the XRD indicates that the high crystalline characteristics of the aluminum nitride particles, silicon nitride particles and boron nitride particles therein are not greatly weakened).

[0072] Under high temperature ammonia in the temperature range of 1100-1400℃, the cured resin will undergo thermal decomposition and be corroded by ammonia. At the same time, the oxygen-containing part will generate water and separate from the spherical body. Similarly, the formed BN bonds maintain the invariance of the spherical structure arrangement of each nitride particle, and a nitride complex phase spherical particle product (at this time, the addition amount of nitride or nano-oxide is not 0) or a boron nitride spherical particle product (at this time, the addition amount of nitride or nano-oxide is 0) can also be obtained.

[0073] Example 1

[0074] 21g of cyanoguanidine, 30mL of water and 15g of boric acid were added to 20mL of formaldehyde solution with a concentration of 37wt.%, and after heating and stirring at 95°C for 0.2 hours, 15g of silicon nitride powder (with a particle size statistical distribution range of 1-10 microns) was added, and after uniform stirring at 65°C for 5 hours, a mixed liquid resin with uniform silicon nitride dispersion was obtained. The mixed liquid resin at 65°C was pumped into the cavity of the hot air flow blast of the spray drying granulation at a feed rate of 5mL / min through a peristaltic pump, and the heat flow in the cavity was set to 200°C. Spherical powder was collected in the collection tower of the atomization granulation equipment, and then heat-dried in 150°C hot air for 6 hours to obtain a composite spherical precursor particle powder with spherical morphology. Finally, the composite spherical precursor particle powder is subjected to high-temperature pyrolysis and nitridation reaction in a high-temperature atmosphere furnace with a nitrogen flow (flow rate of 10 ml / min) at 1100°C or 1500°C. After 6 hours of constant temperature insulation, it is cooled to room temperature at the same cooling rate (10°C / min) as the heating process. The sample is taken out from the high-temperature atmosphere furnace. The taken out sample is the obtained product of the composite spherical material of hexagonal boron nitride and silicon nitride (BN / Si3N4).

[0075] In this embodiment, the powder XRD diffraction patterns of the nitride composite spherical products were obtained at 1100°C and 1500°C in nitrogen respectively. Figure 1 As shown, the respective SEM images are shown in Figure 2 and Figure 3 As shown in the figure, it can be seen that this embodiment can obtain a boron nitride-based spherical composite material.

[0076] Example 2

[0077] After replacing the silicon nitride in Example 1 with boron nitride nanosheet powder, the remaining steps are the same as in Example 1 to obtain a homogeneous composite spherical material of hexagonal boron nitride and boron nitride nanosheets (BN / BNNSs), which is a powdery particle, such as Figure 4-6 shown.

[0078] Example 3

[0079] The boron nitride nanosheets in Example 2 are replaced by boron nitride nanospheres to obtain a homogeneous composite spherical material formed by corresponding hexagonal boron nitride and boron nitride nanospheres.

[0080] Example 4

[0081] The boron nitride nanospheres in Example 3 are replaced with commercial boron nitride powder materials to obtain a homogeneous multiphase spherical material formed by corresponding hexagonal boron nitride and large-particle boron nitride bulk materials.

[0082] Example 5

[0083] In Example 1, no nitride powder was added, that is, the weight of the nitride powder was changed to 0g, and spherical particles of hexagonal boron nitride were obtained. SEM images of nitride composite spherical products were obtained at 1100°C and 1500°C in nitrogen respectively. Fig.11 shown.

[0084] Example 6

[0085] After the nitrogen in Example 5 was changed to ammonia at 1100°C, the same boron nitride spherical particles as those in Example 5 at 1100°C under nitrogen were obtained. The SEM image of the particles is shown in FIG. Fig.12 shown.

[0086] Example 7

[0087] The 30 mL of water in Example 5 was changed to 10 mL, and the other steps remained unchanged, to obtain a composite spherical material with controllable enlargement of spherical particles.

[0088] When the solid content of the nitride or oxide particles in Examples 5-7 is 0wt.%, the spherical material obtained is a pure boron nitride spherical particle powder product. However, the pure boron nitride microsphere particles obtained by the method of the present invention have the characteristics of very low crystallinity. Even after pyrolysis at a temperature higher than 1600°C, the spherical particles are still composed of highly isotropic low-crystalline staggered boron nitride; at the same time, due to the high content of aldehyde components that can form a resin with high viscosity with amino groups, the particle size of the final spherical particles is relatively large. After the spheres are heat treated at a higher temperature, the crystallinity tends to remain low and the surface remains highly smooth and round, and the internal components are more uniformly isotropic, and the particle size is micron-level. Low-crystalline hexagonal boron nitride microsphere particles can be used as a reinforcing agent for ceramic composites to enhance the toughness and crack resistance of ceramic materials, while maintaining good mechanical strength and heat resistance. They are very suitable for the reinforced structure of high-temperature composite phase ceramics, the filling phase of flexible protective coatings under high-temperature extreme environments, and the structural flexible components in high-temperature electrical insulation composite materials. Compared with the general synthesis method of high-crystallization hexagonal boron nitride spherical particles, which usually results in high-temperature, low-crystallization hexagonal boron nitride spherical particles are more effective in high-temperature toughness and crack resistance than high-crystallization relatively hexagonal boron nitride spherical particles.

[0089] Example 8

[0090] The silicon nitride in Example 1 was replaced by aluminum nitride, and other conditions and operations remained unchanged to obtain a composite spherical material of hexagonal boron nitride and aluminum nitride (see Fig.15 and Fig.16 ), but the sample obtained at 1500℃ contained obvious aluminum oxide impurities (see Fig.14 The XRD patterns are shown in Figure 2).

[0091] Example 9

[0092] Similar multiphase spherical materials can be obtained by replacing the cyanoguanidine in Examples 1-4 and 8 with one or a mixture of guanidine carbonate, aminoguanidine, aminoguanidine bicarbonate, 3-amino-1,2,4-triazole or melamine.

[0093] Example 10

[0094] After the 30mL of water in Examples 1-4 and 8-9 is changed to 15, 20, 40, 75 or 100mL, other operations remain unchanged and similar multiphase spherical materials can be obtained. The slight difference is that when the amount of water is in the range of 40, 75 or 100mL, the stirring temperature is between 45 and 80°C. The difference is that: the particle size of the spherical particles shows a trend of gradually decreasing with the increase of the amount of water; when the temperature is less than 65°C, the reaction time needs to be extended to ensure the reaction formation of the resin. This process can last up to 20 hours. In Example 1, since the temperature is a relatively high temperature of 95°C, 0.2 hours is acceptable. In fact, the reaction time of 0.2-20 hours is completely controllable.

[0095] Embodiment 11

[0096] In Example 1, the amount of cyanoguanidine is between 4.1-40g, or the amount of boric acid is between 3.1-31g, or it is changed to diboron trioxide and its amount is between 4-34g, or it is changed to borax and its amount is between 19.1-190g, or the concentration of formaldehyde solution is changed to 30wt.%, or it is changed to an aqueous solution of acetaldehyde; changing the amount of boron-oxygen compound added and the mass of aldehyde-containing organic matter can obtain similar multiphase spherical materials. The difference is that after changing to acetaldehyde, when the amount of boron-oxygen raw material is low, the temperature range of heat drying treatment in air is 400-500℃, and the heat drying treatment time is increased to 36-48 hours, so as to remove some excessive carbon impurities in advance.

[0097] Example 12

[0098] The nitride in Example 11 can be replaced by boron nitride nanoparticles, amorphous boron nitride powder, boron nitride micrometer or nanofiber, commercial boron nitride large-particle powder (5-30 micrometers), aluminum nitride micrometer (1-10 micrometers) or nanometer powder, or silicon nitride nanometer powder, and nanometer oxide powder, and similar composite spherical materials can be obtained, except that the aluminum oxide impurities obtained from aluminum nitride nanoparticles will increase: Wherein, when the nitride is silicon nitride and boron nitride nanosheets with relatively good crystallinity and commercial boron nitride, the stirring temperature can be within the range of 65-95°C, and the temperature increase promotes the resin reaction activity, and the reaction temperature can be completed in 0.1-1 hour at the shortest. The corresponding nitride composite phase microsphere particles and composite phase microsphere particles of boron nitride and oxide are obtained.

[0099] Embodiment 13

[0100] The hot drying air flow in the hot drying treatment in Example 12 was changed to ordinary nitrogen or a mixture of nitrogen and air with an air content not higher than 5% by volume, and the heating / cooling rate range was changed to 1, 5, 15 and 20°C / min; and the subsequent high-temperature pyrolysis heating program was changed to 5, 15, 40, 60 and 100°C / min, respectively, to obtain a similar product.

[0101] Embodiment 14

[0102] After the high-temperature pyrolysis temperature in Example 13 was set to 1600 and 1800°C, the air flow was adjusted to 20, 200, 800, 1400 and 2000 ml / min, respectively, the heating rate was in the range of 5-100°C, and the heat treatment time was 4 hours and 1 hour, respectively, to obtain similar products.

[0103] Embodiment 15

[0104] After the high-temperature pyrolysis temperature in Example 14 was changed to 1100, 1200 and 1400°C, respectively, and the protective atmosphere was changed to ammonia or ammonia + nitrogen, respectively, the target temperature duration was 12, 8 and 6 hours, respectively, and similar products were obtained. The difference was that the aluminum oxide impurities in the boron nitride / aluminum nitride composite phase were significantly reduced.

[0105] Example 16

[0106] The solid content of the nitride powder in Example 1 was changed, and the amount of silicon nitride powder added was adjusted to any amount of 9.56-36 g, to obtain a product similar to Example 1. When the amount of silicon nitride powder added was higher than 20 g, the particle size of the spherical particles tended to increase significantly.

[0107] Embodiment 17

[0108] When the atomization granulation temperature in Example 1 is within the range of 120-200°C, when the temperature is selected within the range of 100-400°C, the drying process generally takes 36-48 hours to completely evaporate the water, and similar products are obtained in the same way.

[0109] Without departing from the basic principles, basic raw materials and basic routes of the present invention, any non-inventive technology and process that replaces, simplifies, replaces, modifies, improves, modifies and adds experimental steps and raw materials to synthesize boron nitride spherical products or nitride multiphase spherical particle products similar to those produced by the present invention, as well as any act of applying the boron nitride spherical products or nitride multiphase spherical particle products prepared by the technology of the present invention to any field, shall be deemed to be an infringement of the protection scope of the present invention.

[0110] Any matters not described in the present invention are applicable to the prior art.

Claims

1. A method for preparing a composite spherical material based on boron nitride by resin-assisted atomization molding, characterized in that: The preparation method comprises the following steps: (1) mixing an aldehyde-containing organic aqueous solution, an amino compound, a boron oxide compound, and water under heating conditions to obtain a uniform liquid resin with high fluidity; the viscosity of the uniform liquid resin is greater than the viscosity of water and is not greater than 50 mPa·s; (2) adding nitride powder or nano-oxide to the above uniform liquid resin, stirring evenly, to obtain a mixed slurry containing nitride powder or nano-oxide with a solid content of 10wt%-30wt% and a viscosity of 500-3000mPa·S; (3) atomizing the mixed slurry to form particles by drying, and then performing a heat drying treatment at 100-500° C. to obtain a composite phase spherical precursor particle powder having a spherical morphology; (4) The composite phase spherical precursor particle powder is heat treated in a protective atmosphere environment within a temperature range of 1100-1800° C., so that the resin component is transformed into a boron nitride phase after high-temperature pyrolysis and in-situ nitridation reaction, thereby obtaining a boron nitride-based composite phase spherical material.

2. The preparation method according to claim 1, characterized in that: In step (1), the ratio of the amount of additional water added (in milliliters) to the amount of the aldehyde-formylating organic aqueous solution (in milliliters) is in the range of 0.5-5; the molar ratio of the amino compound to the boron oxide compound is 1:(0.2-2); the heating temperature is 45°C to 95°C, and the mixture is stirred evenly for 0.2 to 96 hours until a uniform liquid resin is obtained; the solid content in step (2) refers to the ratio of the mass of the nitride powder or nano-oxide to the mass of the total mixture.

3. The preparation method according to claim 1, characterized in that: In step (3), the mixed liquid resin is kept at a temperature in the range of 25°C to 90°C and is blown into an atomizing drying granulator with air as a hot air drying airflow at a temperature range of 120°C to 300°C at a creeping feed rate of 1mL / min-50mL / min for atomizing particle drying and forming to obtain a fluffy white powder with a little moisture, and then heat-dried in a hot air flow oven at 100°C to 500°C for 1-48 hours to obtain a composite phase spherical precursor particle powder with spherical morphology characteristics; Preferably, the heating / cooling rate range of the heat drying treatment in step (3) is 1-20°C / min, and the heat drying gas flow is air, nitrogen, or a mixture of nitrogen and air with an air content of no more than 5% by volume.

4. The preparation method according to claim 1, characterized in that: The aqueous solution of aldehyde-containing organic matter in step (1) is a solution formed by dissolving formaldehyde or acetaldehyde in a water solvent; wherein the content of formaldehyde or acetaldehyde in water is not less than 30 wt.%; The boron-oxygen compound is at least one of boron trioxide, boric acid or borax.

5. The preparation method according to claim 1, characterized in that: The amino compound in step (1) is a nitrogen-containing compound containing an amino group, and is at least one of a guanidine-containing compound, an azole-containing nitrogen-containing compound, and a triazine-containing nitrogen-containing compound; the guanidine-containing compound is at least one of guanidine carbonate, cyanoguanidine, aminoguanidine, and aminoguanidine bicarbonate; The azole-containing nitrogen-containing compound is 3-amino-1,2,4-triazole, and the triazine-containing nitrogen-containing compound is melamine; When the system contains triazine nitrogen-containing compounds or azole nitrogen-containing compounds, a crosslinking inhibitor is added to the system to prevent the system from agglomerating and maintain a uniform liquid resin state.

6. The preparation method according to claim 1, characterized in that: The nitride powder is at least one of boron nitride nanosheets, boron nitride nanoparticles, amorphous boron nitride powder, boron nitride micrometer or nanometer fibers, commercial boron nitride powder, aluminum nitride micrometer or nanometer powder, silicon nitride micrometer or nanometer powder; the nano oxide is at least one of titanium oxide, silicon dioxide, aluminum oxide, lanthanum oxide, molybdenum oxide, cerium oxide, zirconium oxide, yttrium oxide or magnesium oxide.

7. The preparation method according to claim 6, characterized in that: The particle plane size distribution range of the commercial boron nitride powder is 5 to 30 microns; the average particle size of the aluminum nitride micron powder is 1 to 10 microns; and the average particle size of the silicon nitride micron powder is 1 to 10 microns.

8. The preparation method according to claim 1, characterized in that: In the step (4), the heating / cooling rate of the heat treatment is 5-100°C / min, the air flow rate is 10-2000ml / min, and the protective atmosphere is nitrogen, ammonia+nitrogen or ammonia; Wherein, the atmosphere for heat treatment in the temperature range of 1500-1800°C is nitrogen; The atmosphere for the heat treatment within the temperature range of 1100-1400° C. is ammonia or ammonia+nitrogen.

9. A resin-assisted atomization forming boron nitride-based complex phase spherical material, characterized in that: The boron nitride-based composite spherical material is obtained by the preparation method described in any one of claims 1 to 8, and is a composite phase spherical particle of boron nitride and aluminum nitride, a composite phase spherical particle of boron nitride and silicon nitride, a composite phase spherical particle of boron nitride and boron nitride, or a composite phase spherical particle of boron nitride and oxide, and its boron nitride phase is a hexagonal boron nitride phase.

10. The multiphase spherical material according to claim 9, characterized in that: The particle size distribution of the boron nitride-based composite spherical materials ranges from a few microns to more than one hundred microns.

Citation Information

Patent Citations

  • Spherical boron nitride powder and in-situ synthesis preparation method thereof

    CN115520841A

  • High-thermal-conductivity powder filler with core-shell structure and preparation method of high-thermal-conductivity powder filler

    CN116515324A

  • Preparation method of boron nitride spherical particles and boron nitride spherical particles

    CN116692789A

  • Method for preparing hexagonal nitride quasi-spherical particles through centrifugal stirring, granulation forming and high-temperature pyrolysis

    CN117963854A

  • Curing agent composition for thermosetting resin, and thermosetting resin composition, inorganic reinforced composite resin composition and molding including the same

    JP2020138989A

Cited By

  • Azole borate crystal and preparation method thereof, and boron nitride material prepared by pyrolysis of azole borate precursor

    CN119824546A