Double-layer coated lithium iron manganese phosphate-solid-state battery and preparation method thereof

Through the preparation method of double-layer coated lithium iron manganese phosphate-solid-state batteries, the problems of low safety and conductivity of lithium-ion batteries are solved, and efficient rate performance and discharge capacity are achieved, which is suitable for large-scale production.

CN118929603APending Publication Date: 2024-11-12GTC-POWER ZHUHAI TECH CO LTD
View PDF 0 Cites 3 Cited by

Patent Information

Application Number
CN202410863430.X
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-06-29
Publication Date
2024-11-12

AI Technical Summary

Technical Problem

Safety issues of lithium-ion batteries, especially the risks of short circuit, liquid leakage, spontaneous combustion and explosion of liquid electrolytes, and the low conductivity and Li+ diffusion coefficient of lithium manganese iron phosphate materials limit their development.

Method used

The preparation method of double-layer coated lithium manganese iron phosphate-solid-state battery is used to coat LiMnxFe1-xPO4 material by glucose as a carbon source, and Li6PS5Cl is deposited on its surface to form a double-layer coated LiMn0.4Fe0.6PO4 positive electrode material, and Li6PS5Cl is used as Solid electrolyte improves electrical conductivity and inhibits the growth and aggregation of crystal particles.

Benefits of technology

It achieves excellent rate performance, high discharge capacity, good chemical and electrochemical stability of lithium-ion batteries, and is suitable for large-scale production.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure BDA0004919597700000091
    Figure BDA0004919597700000091
  • Figure BDA0004919597700000101
    Figure BDA0004919597700000101
Patent Text Reader

Abstract

The invention relates to the technical field of lithium ion batteries, in particular to a double-layer coated lithium iron manganese phosphate-solid-state battery and a preparation method thereof. According to the preparation method, glucose is used as a carbon source to coat a LiMnxFe1-xPO4 material, then further deposition and coating are carried out through Li6PS5Cl to obtain the double-layer coated LiMn0. 4Fe0. 6PO4 positive electrode material, that is, the surface of the positive electrode material is respectively coated with a carbon coating layer and a solid electrolyte coating layer, and the material of the carbon coating layer takes glucose as the carbon source, and the material of the solid electrolyte coating layer is coated with a solid electrolyte coating layer. The conductive performance of the lithium manganese iron phosphate material can be effectively improved, and ferrous oxalate (FeC2O4. 2H2O) is adopted as an iron source, so that the obtained lithium manganese iron phosphate positive electrode material is high in crystallinity and large in bonding force, impurities are not suitable to be introduced in the preparation process, growth and agglomeration of crystal particles can be inhibited, and the service life of the lithium manganese iron phosphate positive electrode material is prolonged. And the prepared lithium ion battery has excellent rate capability and relatively high discharge gram capacity.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention relates to the technical field of lithium ion batteries, and in particular to a double-layer coated lithium manganese iron phosphate-solid-state battery and a preparation method thereof. Background Art

[0002] The supply of fossil resources required for traditional cars is becoming increasingly tight, and the energy crisis is imminent. In this context, lithium-ion batteries have become the focus of people's attention, and pure electric vehicles are also very popular. In order to further promote pure electric vehicles, improving the energy density of power lithium-ion batteries carried by pure electric vehicles has become a top priority in current research. Power batteries with high energy density can not only increase the cruising range of pure electric vehicles, but also extend the overall life of the battery to a certain extent.

[0003] As the energy density of lithium-ion batteries increases, the energy released will also increase once the battery explodes, causing more serious harm. In recent years, accidents caused by spontaneous combustion and explosion of lithium-ion power batteries have become common, and the safety of lithium-ion batteries has become a focus of attention. Since the electrolytes used in lithium-ion batteries are mainly liquid types, liquid electrolytes still have safety hazards such as short circuits, leakage, spontaneous combustion and even explosions. When the battery encounters collisions, punctures, etc., it is very easy to explode. Therefore, there is an urgent need to develop a new electrolyte system. Sulfide solid electrolytes have good ionic conductivity, so they have become a research hotspot for various companies and institutions represented by Toyota.

[0004] Sulfide electrolytes are derived from oxide solid electrolytes. The oxygen element in the oxide body is replaced by sulfur to form a sulfide solid electrolyte. The electronegativity of sulfur is smaller than that of oxygen, and its binding force on lithium ions is small, which is conducive to the migration of lithium ions. However, sulfide electrolytes have the defects of narrow electrochemical window and poor interface stability with positive and negative electrodes. They are also very sensitive to moisture and can react with trace amounts of water in the air to release toxic hydrogen sulfide gas.

[0005] In addition, although lithium manganese iron phosphate (LiMn x Fe 1-x PO4) has the advantages of good kinetics of LiFePO4 and high energy density of LiMnPO4, but it has lower conductivity and lower Li + The defect of diffusion coefficient has caused great obstacles to its development. Therefore, the electrochemical performance of lithium manganese iron phosphate needs to be further improved. Summary of the invention

[0006] In order to overcome the shortcomings of the prior art, the first purpose of the present invention is to provide a method for preparing a double-layer coated lithium iron manganese phosphate-solid-state battery, which can effectively improve the conductivity of the lithium iron manganese phosphate material, and can also inhibit the growth and agglomeration of crystal particles, so that the prepared lithium-ion battery has excellent rate performance and higher discharge gram capacity.

[0007] In order to overcome the shortcomings of the prior art, the second object of the present invention is to provide a double-layer coated lithium manganese iron phosphate-solid-state battery.

[0008] In order to achieve the first object of the above invention, the technical solution adopted by the present invention is as follows:

[0009] The present invention provides a method for preparing a double-layer coated lithium manganese iron phosphate-solid-state battery, comprising the following steps:

[0010] S1. Synthesis of precursor: lithium carbonate, manganese carbonate, ferrous oxalate and diammonium phosphate are used as reaction raw materials, glucose is used as carbon source and ethanol is used as solvent, the above materials are ground and mixed, the obtained slurry is filtered and initially dried, and then placed in a blast drying oven to obtain powder, and the obtained powder is placed in a vacuum oven to dry to obtain a precursor;

[0011] S2. Calcination of the precursor: The precursor synthesized in step S1 is placed in a tube furnace and calcined to obtain LiMn coated with glucose as a carbon source. x Fe 1-x PO4 material;

[0012] S3, using ALD technology to deposit Li6PS5Cl on the LiMn x Fe 1-x PO4 material surface, finally obtained double-layer coated LiMn 0.4 Fe 0.6 PO4 positive electrode material;

[0013] S4, double-layer coated LiMn obtained in step S3 0.4 Fe 0.6 PO4 positive electrode material is used as the positive electrode of the battery, the negative electrode of the battery is selected, and Li6PS5Cl is used as the solid electrolyte to prepare the double-layer coated lithium manganese iron phosphate-solid-state battery.

[0014] The present invention uses ferrous oxalate (FeC2O4·2H2O) as an iron source to make the obtained lithium iron manganese phosphate positive electrode material have high crystallinity and strong bonding force, and it is not easy to introduce impurities during the preparation process. The use of Li6PS5Cl as a solid electrolyte can make the prepared lithium ion battery have high conductivity, good chemical stability and electrochemical stability.

[0015] The present invention discloses a method for preparing a double-layer coated lithium manganese iron phosphate solid-state battery, wherein glucose is used as a carbon source to coat LiMn x Fe 1-x PO4 material, and then further deposited and coated with Li6PS5Cl to obtain a double-layer coated LiMn 0.4 Fe 0.6 The PO4 positive electrode material, that is, the surface of the positive electrode material is respectively coated with a carbon coating layer and a solid electrolyte coating layer, and the material of the carbon coating layer uses glucose as a carbon source, which can effectively improve the conductivity of the lithium manganese iron phosphate material, and can also inhibit the growth and agglomeration of crystal particles, so that the prepared lithium ion battery has excellent rate performance and higher discharge gram capacity.

[0016] Furthermore, in step S1, the molar ratio of lithium carbonate, manganese carbonate, ferrous oxalate and diammonium hydrogen phosphate is (0.5-1.5):(0.1-0.7):(0.3-0.9):(0.5-2).

[0017] Furthermore, in step S1, the mass ratio of the total mass of the reaction raw materials to the amount of glucose used is (2-3):1.

[0018] Furthermore, in the step S1, the mass ratio of the total mass of the reaction raw materials to the amount of the ethanol used is 1:(30-40).

[0019] Furthermore, in the step S1, the grinding and mixing of the materials is performed by ball milling for 18 hours to 22 hours.

[0020] Furthermore, in step S1, the slurry is filtered and initially dried, and then placed in a forced air drying oven at 60° C. to 70° C. to dry for 0.8 h to 1.2 h to obtain a powder.

[0021] Furthermore, in the step S1, the obtained powder is placed in a vacuum oven at 100° C. to 110° C. and dried for 3 h to 5 h to obtain a precursor.

[0022] Furthermore, in step S2, the calcination procedure is: first, in an air atmosphere, heating the temperature to 380°C to 420°C at a heating rate of 4°C / min to 6°C / min, pre-calcining for 280min to 320min, then heating the temperature to 580°C to 620°C at a heating rate of 9°C / min to 11°C / min, and calcining for 700min to 740min.

[0023] Furthermore, in step S4, the negative electrode is at least one of metallic lithium, graphite or silicon carbon.

[0024] In order to achieve the second purpose of the above invention, the technical solution adopted by the present invention is as follows:

[0025] The present invention provides a double-layer coated lithium iron manganese phosphate-solid-state battery, which is prepared by the preparation method of the double-layer coated lithium iron manganese phosphate-solid-state battery described above.

[0026] Compared with the prior art, the present invention has the following beneficial effects:

[0027] (1) A method for preparing a double-layer coated lithium manganese iron phosphate-solid-state battery of the present invention, wherein glucose is used as a carbon source to coat LiMn x Fe 1-x PO4 material, and then further deposited and coated with Li6PS5Cl to obtain a double-layer coated LiMn 0.4 Fe 0.6 PO4 positive electrode material, that is, the surface of the positive electrode material is respectively coated with a carbon coating layer and a solid electrolyte coating layer, and the material of the carbon coating layer uses glucose as a carbon source, which can effectively improve the conductivity of the lithium iron manganese phosphate material, and by using ferrous oxalate (FeC2O4·2H2O) as an iron source, the obtained lithium iron manganese phosphate positive electrode material can have high crystallinity and strong bonding force, and it is not easy to introduce impurities during the preparation process, and the growth and agglomeration of crystal particles can be suppressed, so that the prepared lithium ion battery has excellent rate performance and high discharge gram capacity.

[0028] (2) The method for preparing a double-layer coated lithium manganese iron phosphate-solid-state battery of the present invention has the characteristics of being simple and suitable for large-scale production.

[0029] (3) The double-layer coated lithium manganese iron phosphate-solid-state battery of the present invention has excellent rate performance, high discharge gram capacity, high conductivity, good chemical stability and electrochemical stability. DETAILED DESCRIPTION

[0030] In order to make the technical problems, technical solutions and beneficial effects to be solved by the present invention more clearly understood, the present invention is further described in detail below in conjunction with the embodiments. It should be understood that the specific embodiments described herein are only used to explain the present invention and are not used to limit the present invention.

[0031] The terms used in the embodiments of the present invention are only for the purpose of describing specific embodiments, and are not intended to limit the present invention. The singular forms "a", "said", "the", "first", "second" and "third" used in the embodiments of the present invention and the appended claims are also intended to include plural forms, unless the context clearly indicates other meanings.

[0032] In an embodiment of the present invention, a method for preparing a double-layer coated lithium manganese iron phosphate-solid-state battery comprises the following steps:

[0033] S1. Synthesis of precursor: lithium carbonate, manganese carbonate, ferrous oxalate and diammonium phosphate are used as reaction raw materials, glucose is used as carbon source and ethanol is used as solvent, the above materials are ground and mixed, the obtained slurry is filtered and initially dried, and then placed in a blast drying oven to obtain powder, and the obtained powder is placed in a vacuum oven to dry to obtain a precursor;

[0034] S2. Calcination of the precursor: The precursor synthesized in step S1 is placed in a tube furnace and calcined to obtain LiMn coated with glucose as a carbon source. x Fe 1-x PO4 material;

[0035] S3, using ALD technology to deposit Li6PS5Cl on the LiMn x Fe 1-x PO4 material surface, finally obtained double-layer coated LiMn 0.4 Fe 0.6 PO4 positive electrode material;

[0036] S4, double-layer coated LiMn obtained in step S3 0.4 Fe 0.6 PO4 positive electrode material is used as the positive electrode of the battery, the negative electrode of the battery is selected, and Li6PS5Cl is used as the solid electrolyte to prepare the double-layer coated lithium manganese iron phosphate-solid-state battery.

[0037] The present invention uses ferrous oxalate (FeC2O4·2H2O) as an iron source to make the obtained lithium iron manganese phosphate positive electrode material have high crystallinity and strong bonding force, and it is not easy to introduce impurities during the preparation process. The use of Li6PS5Cl as a solid electrolyte can make the prepared lithium ion battery have high conductivity, good chemical stability and electrochemical stability.

[0038] A method for preparing a double-layer coated lithium manganese iron phosphate-solid-state battery in the embodiment, wherein glucose is used as a carbon source to coat LiMn x Fe 1-x PO4 material, and then further deposited and coated with Li6PS5Cl to obtain a double-layer coated LiMn 0.4 Fe 0.6 The PO4 positive electrode material, that is, the surface of the positive electrode material is respectively coated with a carbon coating layer and a solid electrolyte coating layer, and the material of the carbon coating layer uses glucose as a carbon source, which can effectively improve the conductivity of the lithium manganese iron phosphate material, and can also inhibit the growth and agglomeration of crystal particles, so that the prepared lithium ion battery has excellent rate performance and higher discharge gram capacity.

[0039] In some embodiments, in step S1, the molar ratio of lithium carbonate, manganese carbonate, ferrous oxalate and diammonium hydrogen phosphate is (0.5-1.5):(0.1-0.7):(0.3-0.9):(0.5-2).

[0040] In some embodiments, in step S1, the mass ratio of the total mass of the reaction raw materials to the amount of glucose used is (2-3):1.

[0041] In some embodiments, in step S1, the mass ratio of the total mass of the reaction raw materials to the amount of the ethanol used is 1:(30-40).

[0042] In some embodiments, in step S1, the grinding and mixing of the materials is performed by ball milling for 18 hours to 22 hours.

[0043] In some embodiments, in step S1, the slurry is filtered and initially dried, and then placed in a forced air drying oven at 60° C. to 70° C. to dry for 0.8 h to 1.2 h to obtain a powder.

[0044] In some embodiments, in step S1, the obtained powder is placed in a vacuum oven at 100° C. to 110° C. and dried for 3 h to 5 h to obtain a precursor.

[0045] In some embodiments, in step S2, the calcination procedure is: first increase the temperature to 380°C to 420°C in an air atmosphere at a heating rate of 4°C / min to 6°C / min, pre-calculate for 280min to 320min, then increase the temperature to 580°C to 620°C at a heating rate of 9°C / min to 11°C / min, and calcine for 700min to 740min.

[0046] In some embodiments, in step S4, the negative electrode is at least one of metallic lithium, graphite or silicon carbon.

[0047] In an embodiment of the present invention, a double-layer coated lithium iron manganese phosphate-solid-state battery is prepared by the preparation method of a double-layer coated lithium iron manganese phosphate-solid-state battery described above.

[0048] The following describes the invention in conjunction with specific embodiments.

[0049] Example 1

[0050] A method for preparing a double-layer coated lithium manganese iron phosphate-solid-state battery of this embodiment is characterized by comprising the following steps:

[0051] S1. Synthesis of precursor: lithium carbonate, manganese carbonate, ferrous oxalate and diammonium hydrogen phosphate are used as reaction raw materials, 20% glucose by mass is used as carbon source, and ethanol is used as solvent. The above materials are ball milled and mixed for 20 hours by a ball mill. The obtained slurry is filtered and initially dried, and then placed in a 65°C forced air drying oven for 1 hour to obtain a powder. The obtained powder is placed in a vacuum oven at 105°C and dried for 4 hours to obtain a precursor; in this embodiment, the molar ratio of lithium carbonate, manganese carbonate, ferrous oxalate and diammonium hydrogen phosphate is 1:0.4:0.6:1; in this embodiment, the mass ratio of the total mass of the reaction raw materials to the amount of glucose used is 2.5:1; in this embodiment, the mass ratio of the total mass of the reaction raw materials to the amount of ethanol used is 1:35;

[0052] S2. Calcination of the precursor: The precursor synthesized in step S1 is placed in a tube furnace for calcination. The calcination procedure is: firstly, the temperature is raised to 400°C at a heating rate of 5°C / min in an air atmosphere for pre-calcination for 300min, then the temperature is raised to 600°C at a heating rate of 10°C / min, and calcined for 720min to obtain LiMn coated with glucose as a carbon source. x Fe 1-x PO4 material;

[0053] S3, using ALD technology to deposit Li6PS5Cl on the LiMn x Fe 1-x PO4 material surface, finally obtained double-layer coated LiMn 0.4 Fe 0.6 PO4 positive electrode material;

[0054] S4, double-layer coated LiMn obtained in step S3 0.4 Fe 0.6 PO4 positive electrode material is used as the positive electrode of the battery, metallic lithium is selected as the negative electrode of the battery, and Li6PS5Cl is used as the solid electrolyte to obtain the double-layer coated lithium manganese iron phosphate-solid-state battery.

[0055] Example 2

[0056] A method for preparing a double-layer coated lithium manganese iron phosphate-solid-state battery of this embodiment is characterized by comprising the following steps:

[0057] S1. Synthesis of precursor: lithium carbonate, manganese carbonate, ferrous oxalate and diammonium hydrogen phosphate are used as reaction raw materials, 20% glucose by mass is used as carbon source, and ethanol is used as solvent. The above materials are ball milled and mixed for 18 hours by a ball mill. The obtained slurry is filtered and initially dried, and then placed in a 60°C forced air drying oven for 1.2 hours to obtain a powder. The obtained powder is placed in a vacuum oven at 100°C and dried for 5 hours to obtain a precursor; in this embodiment, the molar ratio of lithium carbonate, manganese carbonate, ferrous oxalate and diammonium hydrogen phosphate is 0.5:0.1:0.3:0.5; in this embodiment, the mass ratio of the total mass of the reaction raw materials to the amount of glucose used is 2:1; in this embodiment, the mass ratio of the total mass of the reaction raw materials to the amount of ethanol used is 1:30;

[0058] S2. Calcination of the precursor: The precursor synthesized in step S1 was placed in a tube furnace for calcination. The calcination procedure was as follows: first, the temperature was raised to 380°C at a heating rate of 4°C / min in an air atmosphere for pre-calcination for 320 min, then the temperature was raised to 580°C at a heating rate of 9°C / min, and calcined for 740 min to obtain LiMn coated with glucose as a carbon source. x Fe 1-x PO4 material;

[0059] S3, using ALD technology to deposit Li6PS5Cl on the LiMn x Fe 1-x PO4 material surface, finally obtained double-layer coated LiMn 0.4 Fe 0.6 PO4 positive electrode material;

[0060] S4, double-layer coated LiMn obtained in step S3 0.4 Fe 0.6 PO4 positive electrode material is used as the positive electrode of the battery, graphite is selected as the negative electrode of the battery, and Li6PS5Cl is used as the solid electrolyte to prepare the double-layer coated lithium manganese iron phosphate-solid-state battery.

[0061] Example 3

[0062] A method for preparing a double-layer coated lithium manganese iron phosphate-solid-state battery of this embodiment is characterized by comprising the following steps:

[0063] S1. Synthesis of precursor: lithium carbonate, manganese carbonate, ferrous oxalate and diammonium hydrogen phosphate are used as reaction raw materials, 20% glucose by mass is used as carbon source, and ethanol is used as solvent. The above materials are ball milled and mixed for 22 hours by a ball mill. The obtained slurry is filtered and initially dried, and then placed in a 70°C forced air drying oven for 0.8 hours to obtain a powder. The obtained powder is placed in a vacuum oven at 110°C and dried for 3 hours to obtain a precursor; in this embodiment, the molar ratio of lithium carbonate, manganese carbonate, ferrous oxalate and diammonium hydrogen phosphate is 1.5:0.7:0.9:2; in this embodiment, the mass ratio of the total mass of the reaction raw materials to the amount of glucose used is (2-3):1; in this embodiment, the mass ratio of the total mass of the reaction raw materials to the amount of ethanol used is 1:40;

[0064] S2. Calcination of the precursor: The precursor synthesized in step S1 was placed in a tube furnace for calcination. The calcination procedure was as follows: first, the temperature was raised to 420°C at a heating rate of 6°C / min in an air atmosphere for pre-calcination for 280 min, then the temperature was raised to 620°C at a heating rate of 11°C / min, and calcined for 700 min to obtain LiMn coated with glucose as a carbon source. x Fe 1-x PO4 material;

[0065] S3, using ALD technology to deposit Li6PS5Cl on the LiMn x Fe 1-x PO4 material surface, finally obtained double-layer coated LiMn 0.4 Fe 0.6 PO4 positive electrode material;

[0066] S4, double-layer coated LiMn obtained in step S3 0.4 Fe 0.6 PO4 positive electrode material is used as the positive electrode of the battery, silicon carbon is selected as the negative electrode of the battery, and Li6PS5Cl is used as the solid electrolyte to prepare the double-layer coated lithium manganese iron phosphate-solid-state battery.

[0067] Comparative Example 1

[0068] The difference between Comparative Example 1 and Example 1 is that in step S1, glucose is not added, that is, there is no carbon source coating layer, and a single-layer coated lithium manganese iron phosphate positive electrode material is obtained; the remaining steps and condition parameters are the same as those in Example 1.

[0069] Comparative Example 2

[0070] The difference between Comparative Example 2 and Example 1 is that the entire S3 step is not performed, that is, Li6PS5Cl deposition is not performed, that is, the solid electrolyte coating layer is missing, and the obtained LiMn x Fe 1-xPO4 material; the remaining steps and condition parameters are the same as those in Example 1.

[0071] Comparative Example 3

[0072] The difference between Comparative Example 3 and Example 1 is that in step S1, glucose is not added, that is, the carbon source coating layer is missing, and the entire S3 step is not performed, that is, Li6PS5Cl deposition is not performed, that is, the solid electrolyte coating layer is missing, and the LiMn without any coating layer is obtained. x Fe 1-x PO4 material; the remaining steps and condition parameters are the same as those in Example 1.

[0073] Experimental test:

[0074] (1) Charge and discharge cycle test

[0075] The solid-state lithium-ion batteries prepared in Examples 1-3 and Comparative Examples 1-3 were subjected to charge and discharge cycle tests. The solid-state lithium batteries of each embodiment and comparative example were charged and discharged at 0.1C, wherein the 0.1C charge and discharge cycle test was performed under the condition that the charge and discharge cut-off voltage was 2.75-4.3V. The test results are shown in Table 1.

[0076] Table 1. Charge and discharge test results of solid-state lithium-ion batteries of Examples 1-3 and Comparative Examples 1-3

[0077]

[0078]

[0079] From the test data in Table 1, it can be seen that when the double-layer coated LiMn prepared by the method of the present invention 0.4 Fe 0.6 When the PO4 positive electrode material is used as the positive electrode of the battery and metallic lithium is used as the negative electrode of the battery to assemble the all-solid-state battery, the capacity retention rate of the solid-state battery after 100 cycles at 0.1C is 90%. In addition, compared with Example 1, since Example 2 uses graphite as the negative electrode of the battery and Example 3 uses silicon carbon as the negative electrode of the battery, the capacity of the solid-state batteries of Examples 2 and 3 after 100 cycles at 0.1C is lower than that of Example 1.

[0080] In addition, since Comparative Example 1 uses a single-layer coated lithium iron manganese phosphate positive electrode material as the positive electrode of the battery and metal lithium as the negative electrode of the battery to assemble an all-solid-state battery, the 0.1C specific capacity of the solid-state battery is only 89 mAh / g, which is only 72% of that of Example 1, and the capacity retention rate of 100 cycles at 0.1C is 85%. Comparative Examples 2 and 3 are respectively coated with only glucose or electrolyte layers, and the 0.1C specific capacity and the capacity retention rate of 100 cycles at 0.1C are lower than those using double-layer coated LiMn 0.4Fe 0.6 This shows that the present invention effectively improves the conductivity of lithium iron manganese phosphate material by double-layer coating of lithium iron manganese phosphate and uses glucose as a carbon source, and can also inhibit the growth and agglomeration of crystal particles, so that the lithium ion battery prepared by the present invention has excellent rate performance and high discharge capacity.

[0081] The above description is only a preferred embodiment of the present application and is not intended to limit the present application. Any modifications, equivalent substitutions and improvements made within the spirit and principles of the present application should be included in the protection scope of the present application.

Claims

1. A method for preparing a double-layer coated lithium manganese iron phosphate-solid-state battery, characterized in that: The following steps are involved: S1. Synthesis of precursor: lithium carbonate, manganese carbonate, ferrous oxalate and diammonium phosphate are used as reaction raw materials, glucose is used as carbon source and ethanol is used as solvent, the above materials are ground and mixed, the obtained slurry is filtered and initially dried, and then placed in a blast drying oven to obtain powder, and the obtained powder is placed in a vacuum oven to dry to obtain a precursor; S2. Calcination of the precursor: The precursor synthesized in step S1 is placed in a tube furnace and calcined to obtain LiMn coated with glucose as a carbon source. x Fe 1-x PO4 material; S3, using ALD technology to deposit Li6PS5Cl on the LiMn x Fe 1-x PO4 material surface, finally obtained double-layer coated LiMn 0.4 Fe 0.6 PO4 positive electrode material; S4, double-layer coated LiMn obtained in step S3 0.4 Fe 0.6 PO4 positive electrode material is used as the positive electrode of the battery, the negative electrode of the battery is selected, and Li6PS5Cl is used as the solid electrolyte to prepare the double-layer coated lithium manganese iron phosphate-solid-state battery.

2. The method for preparing a double-layer coated lithium manganese iron phosphate-solid-state battery according to claim 1, characterized in that: In the step S1, the molar ratio of the lithium carbonate, manganese carbonate, ferrous oxalate and diammonium hydrogen phosphate is (0.5-1.5):(0.1-0.7):(0.3-0.9):(0.5-2).

3. The method for preparing a double-layer coated lithium manganese iron phosphate-solid-state battery according to claim 1, characterized in that: In the step S1, the mass ratio of the total mass of the reaction raw materials to the amount of the glucose used is (2-3):

1.

4. The method for preparing a double-layer coated lithium manganese iron phosphate-solid-state battery according to claim 1, characterized in that: In the step S1, the mass ratio of the total mass of the reaction raw materials to the amount of the ethanol used is 1:(30-40).

5. The method for preparing a double-layer coated lithium manganese iron phosphate-solid-state battery according to claim 1, characterized in that: In the step S1, the grinding and mixing of the materials is performed by ball milling for 18 hours to 22 hours.

6. The method for preparing a double-layer coated lithium manganese iron phosphate-solid-state battery according to claim 1, characterized in that: In the step S1, the slurry is filtered and initially dried, and then placed in a 60° C. to 70° C. forced air drying oven for 0.8 h to 1.2 h to obtain a powder.

7. The method for preparing a double-layer coated lithium manganese iron phosphate-solid-state battery according to claim 1, characterized in that: In the step S1, the obtained powder is placed in a vacuum oven at 100° C. to 110° C. and dried for 3 h to 5 h to obtain a precursor.

8. The method for preparing a double-layer coated lithium manganese iron phosphate-solid-state battery according to claim 1, characterized in that: In step S2, the calcination procedure is: first, in an air atmosphere, heating the temperature to 380°C to 420°C at a heating rate of 4°C / min to 6°C / min, pre-calcining for 280min to 320min, then heating the temperature to 580°C to 620°C at a heating rate of 9°C / min to 11°C / min, and calcining for 700min to 740min.

9. The method for preparing a double-layer coated lithium manganese iron phosphate-solid-state battery according to claim 1, characterized in that: In the step S4, the negative electrode is at least one of metallic lithium, graphite or silicon carbon.

10. A double-layer coated lithium manganese iron phosphate-solid-state battery, characterized in that: It is prepared by the preparation method of a double-layer coated lithium manganese iron phosphate-solid-state battery as described in any one of claims 1 to 9.

Citation Information

Cited By

  • Composite positive electrode material and preparation method and application thereof

    CN119275276A

  • PVD (Physical Vapor Deposition) modified positive electrode material as well as preparation method and application thereof

    CN120089675A

  • Lithium manganese iron phosphate battery pack and processing method thereof

    CN120199912A