Preparation method of graphite-based Yb2O3-TiB2-SiC ceramic coating material

By directly covering SiC, TiB2 and Yb2O3 powders on the graphite substrate and pressurized sintering, the complexity and high cost problems caused by the difference in thermal expansion coefficient in the preparation of ceramic coatings are solved, and efficient preparation and good ceramic coatings are achieved. High temperature oxidation resistance.

CN118930320AActive Publication Date: 2024-11-12ZHENGZHOU UNIV
View PDF 3 Cites 0 Cited by

Patent Information

Application Number
CN202410998735.1
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-07-24
Publication Date
2024-11-12
Estimated Expiration
2044-07-24

AI Technical Summary

Technical Problem

In the existing ceramic coating preparation methods, the difference in thermal expansion coefficient between the matrix material and the ceramic coating leads to complex preparation process, long time, low efficiency and high cost, which affects practical application.

Method used

Using the preparation method of graphite-based Yb2O3-TiB2-SiC ceramic coating material, the SiC powder, TiB2 powder and Yb2O3 powder are mixed at a certain mass ratio, and sintered at high temperature under pressurized conditions, and directly coated on graphite On the substrate, the preparation process is simplified.

Benefits of technology

It realizes simple and efficient preparation of ceramic coatings, ensures flat surfaces and uniform composition distribution, eliminates the problem of performance instability caused by mismatch of thermal expansion coefficients, and improves high-temperature oxidation resistance.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118930320A_ABST
    Figure CN118930320A_ABST
Patent Text Reader

Abstract

The invention relates to the technical field of graphite-based ceramic coating materials, in particular to a preparation method of a graphite-based Yb2O3-TiB2-SiC ceramic coating material. The method comprises the following steps: uniformly mixing SiC powder, TiB2 powder and Yb2O3 powder, coating a graphite substrate with the mixture, sintering, applying pressure in the sintering process, controlling the sintering pressure to be 30MPa, and obtaining the graphite-based Yb2O3-TiB2-SiC ceramic coating material after the sintering process is finished. According to the method, sintering is carried out under the pressure applying condition, a SiC bottom layer does not need to be prepared between the graphite matrix and the ceramic coating, the problem that the performance of the ceramic coating is unstable due to mismatching of thermal expansion coefficients between the graphite matrix and the ceramic coating can be solved, the obtained ceramic coating and the matrix are well combined, the surface of the ceramic coating is flat, and the service life of the ceramic coating is prolonged. Components are uniformly distributed, no obvious defect exists, and the performance is stable; and meanwhile, the preparation method is simpler and more efficient, the thickness of the coating is controllable, and the application prospect is wide.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the technical field of graphite-based ceramic coating materials, and in particular to a method for preparing a graphite-based Yb2O3-TiB2-SiC ceramic coating material. Background Art

[0002] Ceramic coating is a general term for various inorganic protective layers, which have the advantages of wear resistance, corrosion resistance, high temperature resistance, high hardness, high strength and good biocompatibility. Ceramic coating can provide special functional properties to the substrate to overcome the defects of the substrate material and improve the efficiency of the material. Therefore, ceramic coating is widely used in aerospace, automobile manufacturing, energy, chemical industry, electronics and biomedicine. In view of the needs of the industrial engineering field, it is urgent to prepare ceramic coatings with excellent performance.

[0003] Due to the difference in thermal expansion coefficient between the substrate material and the ceramic coating, in the existing preparation method, an inner coating is often prepared between the substrate material and the ceramic coating to ensure the stability of the ceramic coating; for example, Ren et al. (Xuanru Ren, et al., Preparation of oxidation protective Hf 0.2 Ta 0.8 B 2-x -SiC coating by in-situ reaction method on SiC-coated carbon / carbon composite, Journal of Alloys and Compounds, 2015, 618: 390-395.) A layer of Hf0.2Ta0.8B2-x outer coating was prepared on the surface of a C / C substrate with a SiC inner coating by an in-situ reaction method; Chinese invention patent: "CN111960830A A SiC / HfB2-SiC-La2O3 / SiC ultra-high temperature oxidation resistant composite coating on a graphite substrate", a layer of SiC bottom layer was prepared between the graphite substrate and the ceramic coating, etc.

[0004] However, preparing an inner coating between the substrate material and the ceramic coating makes the preparation process more complicated, time-consuming and inefficient, and also increases the preparation cost, which brings inconvenience to practical applications. Summary of the invention

[0005] The purpose of the present invention is to provide a method for preparing a graphite-based Yb2O3-TiB2-SiC ceramic coating material to solve the problem that the existing preparation methods all use an inner coating method to deal with the difference in thermal expansion coefficients between the base material and the ceramic coating, thereby resulting in long material preparation time, low efficiency and high cost, and inconvenience for practical application.

[0006] To achieve the above object, the present invention adopts the following technical scheme: a method for preparing a graphite-based Yb2O3-TiB2-SiC ceramic coating material, comprising the following steps:

[0007] S1. Mix SiC powder, TiB2 powder and Yb2O3 powder in a certain mass ratio to obtain a uniformly mixed raw material powder;

[0008] S2, pre-treating the graphite substrate;

[0009] S3. The raw material powder obtained in S1 is coated on the pretreated graphite substrate in S2, and high-temperature sintering is performed under pressure to obtain a graphite-based Yb2O3-TiB2-SiC ceramic coating material.

[0010] Furthermore, in the S1, the particle sizes of SiC powder, TiB2 powder and Yb2O3 powder are all 4-8 μm; the purity of SiC powder, TiB2 powder and Yb2O3 powder is ≥99.9%.

[0011] Furthermore, in the S1, the mass ratio of SiC powder, TiB2 powder and Yb2O3 powder is 2:3:0.4.

[0012] Furthermore, in the above-mentioned S1, the mixed powder is mixed uniformly by wet ball milling to form a slurry, and the slurry is dried and sieved to obtain a uniformly mixed raw material powder.

[0013] Furthermore, the mass ratio of the ball mill to the raw material powder is 2:1, the ball composition is ZrO2, and the diameter is 3 mm; the ball milling medium is anhydrous ethanol; the ball milling speed is 90 r / min, and the ball milling time is 24 h.

[0014] Furthermore, during the screening process, a 30-mesh stainless steel screen is used to separate the grinding balls in the slurry, and the separated slurry is placed in an 80° C. constant temperature drying oven and dried for 12 hours. A 200-mesh stainless steel screen is used to screen the dried powder to obtain a uniformly mixed raw material powder.

[0015] Furthermore, in said S2, the method for pretreating the graphite substrate powder is: grinding the surface of the graphite substrate with sandpaper, and performing ultrasonic cleaning and drying operations after grinding.

[0016] Furthermore, the specification of the graphite substrate is a Φ18mm×3mm disc; the graphite substrate is polished with 200-mesh and 800-mesh sandpapers respectively, and the polishing time of the two types of sandpapers on the graphite substrate is 2 minutes; the frequency of ultrasonic cleaning is 40kHz, and the ultrasonic time is 5 minutes; drying is carried out in a constant temperature drying oven, the drying temperature is 80°C, and the drying time is 2 hours.

[0017] Furthermore, in the S3, the temperature control program of the sintering process is: the heating rate below 1000°C is 50°C / min; the heating rate from 1000°C to the maximum temperature is 30°C / min; the holding time after heating to the maximum temperature is 20 minutes; then the temperature is reduced to 1000°C at a rate of 50°C / min, and then cooled to room temperature with the furnace; the maximum temperature is ≥1800°C.

[0018] Furthermore, in S3, the pressure applied during the sintering process is 30 MPa.

[0019] Beneficial effects of the present invention:

[0020] 1. The method of the present invention realizes the preparation of Yb2O3-TiB2-SiC single ceramic coating on a graphite substrate under pressure, and the preparation process is simpler and more efficient;

[0021] 2. The Yb2O3-TiB2-SiC ceramic coating obtained by the method of the present invention has a smooth surface, uniform component distribution, no obvious defects, and good bonding with the substrate, thereby eliminating the problem of unstable performance of the ceramic coating caused by the mismatch of thermal expansion coefficients between the graphite substrate and the ceramic coating, and ensuring the stability of the ceramic coating;

[0022] 3. The Yb2O3-TiB2-SiC ceramic coating obtained by the method of the present invention has good anti-oxidation performance at high temperatures. In addition, the thickness of the coating can be adjusted to further improve the anti-oxidation performance of the material, and has broad application prospects. BRIEF DESCRIPTION OF THE DRAWINGS

[0023] Figure 1 is the X-ray diffraction pattern of the Yb2O3-TiB2-SiC ceramic coating prepared in Example 1 of the present invention;

[0024] Figure 2 is a surface morphology photograph (100 μm) of the Yb2O3-TiB2-SiC ceramic coating prepared in Example 1 of the present invention;

[0025] Figure 3 is a surface morphology photograph (1 μm) of the Yb2O3-TiB2-SiC ceramic coating prepared in Example 1 of the present invention;

[0026] Figure 4 is a cross-sectional morphology photograph of the Yb2O3-TiB2-SiC ceramic coating prepared in Example 1 of the present invention;

[0027] Figure 5 is a surface morphology photograph of the Yb2O3-TiB2-SiC ceramic coating prepared in Comparative Example 1 of the present invention;

[0028] Figure 6 The surface morphology of the Yb2O3-TiB2-SiC ceramic coating prepared in Example 1 of the present invention after oxidation at 1300°C for 24 hours;

[0029] Figure 7 This is the cross-sectional morphology of the Yb2O3-TiB2-SiC ceramic coating prepared in Example 1 of the present invention after oxidation at 1300°C for 24 hours;

[0030] Figure 8 It is a macroscopic photograph of the sample prepared in Comparative Example 2 of the present invention. DETAILED DESCRIPTION

[0031] The technical solutions in the embodiments of the present invention will be described clearly and completely below in conjunction with the accompanying drawings in the embodiments of the present invention.

[0032] Example 1

[0033] A method for preparing a ceramic coating comprises the following steps:

[0034] S1. Use raw materials TiB2, SiC and Yb2O3, calculate and weigh them according to the mass ratio of 2:3:0.4; wherein the particle size of TiB2 powder, SiC powder and Yb2O3 powder is 4-8μm, and the purity is ≥99.9%. After weighing the powder, add the raw material powder, zirconia grinding balls with a diameter of 3mm and anhydrous ethanol into a ball mill according to the mass ratio of 1:2:7, and roll ball mill for 24 hours at a speed of 90r / min; the powder after ball milling is separated from the grinding balls through a 30-mesh stainless steel sieve, and the slurry after screening is placed in a constant temperature drying oven at 80℃ and dried for 12 hours. The dried powder is screened through a 200-mesh stainless steel sieve to obtain a uniformly mixed dry powder.

[0035] S2. Use a graphite disc with a size of Φ18mm×3mm as the substrate; first, manually grind and polish the graphite disc on 200-mesh SiC sandpaper for 2 minutes, rinse off the residual particles on the graphite surface with clean water, then use 800-mesh SiC sandpaper to grind and polish for 2 minutes, rinse off the residual particles on the surface, and then ultrasonically clean it at a frequency of 40kHz for 5 minutes. After removing impurities, put it in a constant temperature drying oven at 80℃ and dry it for 12 hours.

[0036] S3. The dry powder obtained in S1 and S2 and the treated graphite matrix are loaded into a Φ20 mm special mold for spark plasma sintering. The powder and the mold are separated by clean carbon paper. 1.5 g of powder is weighed to wrap the graphite matrix in the center, and the surface of the powder is flattened after each step. After the mold is installed, spark plasma sintering is performed, and the sintering setting pressure is 30 MPa.

[0037] The sintering program temperature system is as follows: during the heating process, the heating rate below 1000°C is 50°C / min; the heating rate from 1000 to 1800°C is 30°C / min, and after keeping at 1800°C for 20 minutes, the temperature is lowered to 1000°C at a rate of 50°C / min, and finally cooled to room temperature with the furnace; after taking out, the carbon paper is removed by grinding and polishing with sandpaper to obtain a Yb2O3-TiB2-SiC ceramic coating sample.

[0038] like Figure 1 As shown, the prepared Yb2O3-TiB2-SiC ceramic coating sample has a phase composition of Yb2O3, TiB2 and SiC and has no other impurity diffraction peaks, indicating that the coating was successfully prepared.

[0039] Figure 2 , 3 and Figure 4 The surface and cross-sectional morphologies of the coating samples are shown respectively. The coating surface is flat, the composition is evenly distributed, there are no obvious defects, and it is well bonded to the substrate. In addition, during the coating preparation process, its composition and thickness are controllable.

[0040] Antioxidant Experimental Study:

[0041] The material obtained in this example was oxidized in a static air environment at 1300°C for 24 hours, and the weight per unit area increased by 0.92 mg / cm 2 , showing good antioxidant properties.

[0042] like Figure 6 As shown in the figure, from the surface morphology of the oxidized coating, it can be seen that a dense oxide layer is formed on the surface of the oxidized coating sample. The TiO2 with light gray contrast and the Yb2Si2O7 with bright white contrast are tightly embedded in the SiO2 with dark gray contrast. They have a pinning effect on the oxide layer, which is beneficial to improve the high temperature stability of the oxide layer.

[0043] like Figure 7 As shown, from the cross-sectional morphology image of the coating sample after oxidation, it can be seen that the coating and the oxide layer are relatively complete, without obvious defects, and show good high-temperature stability; it should be noted that the coating thickness of the material of the present invention is controllable, and the high-temperature oxidation resistance of the material can be further improved by increasing the thickness.

[0044] Example 2

[0045] In S3, sintering is performed at 1900°C, and other conditions are the same as those in Example 1.

[0046] The obtained coating was basically consistent with that in Example 1 after testing, and the coating was successfully prepared.

[0047] Comparative Example 1

[0048] A method for preparing a ceramic coating comprises the following steps:

[0049] S1. Use raw materials TiB2, SiC and Yb2O3, calculate and weigh them according to the mass fraction ratio of 2:3:0.4; the particle size of TiB2 powder, SiC powder and Yb2O3 powder is 4-8μm, and the purity is ≥99.9%. After weighing the powder, add the raw material powder, 3mm diameter zirconium oxide grinding balls and anhydrous ethanol in a ball mill according to the mass ratio of 1:2:7, and roll ball mill for 24 hours at a speed of 90r / min. The ball-milled powder is separated by a 30-mesh stainless steel sieve, and the sieved slurry is placed in a constant temperature drying oven at 80℃ and dried for 5 hours. The dried powder is sieved by a 200-mesh stainless steel sieve to obtain a uniformly mixed dry powder.

[0050] S2. Use a graphite disc with a size of Φ18mm×3mm as the substrate; first, manually grind and polish the graphite disc on 200-mesh SiC sandpaper for 2 minutes, rinse off the residual particles on the graphite surface with clean water, then use 800-mesh SiC sandpaper to grind and polish for 2 minutes, rinse off the residual particles on the surface, and then ultrasonically clean it at a frequency of 40kHz for 5 minutes. After removing impurities, put it in a constant temperature drying oven at 80℃ and dry it for 2 hours.

[0051] S3. The dry powder obtained in S1 and S2 and the treated graphite substrate are loaded into a Φ20 mm special mold for spark plasma sintering, and the powder and the mold are separated by clean carbon paper; 1.5 g of powder is weighed to wrap the graphite substrate in the center, and the surface of the powder is flattened after each step to ensure the uniformity of the coating; after the mold is installed, spark plasma sintering is adopted, and the sintering setting pressure is 30 MPa.

[0052] The temperature program of the sintering process is as follows: during the heating process, 50°C / min is used below 1000°C; 30°C / min is used from 1000 to 1700°C; the holding time at 1700°C is 20 minutes; during the cooling process, the temperature is reduced to 1000°C at a rate of 50°C / min, and then the program ends and the sample is cooled to room temperature with the furnace. After being taken out, it is polished with sandpaper to remove the carbon paper to obtain a Yb2O3-TiB2-SiC ceramic coating sample.

[0053] Depend on Figure 5As shown, the Yb2O3-TiB2-SiC ceramic coating sample prepared by spark plasma sintering at 1700℃ for 20min has a low density and many holes on the surface. When the carbon paper is removed, the coating is easily ground off over a large area to expose the graphite matrix, and the integrity of the coating is destroyed.

[0054] Combining Example 1, Example 2 and Comparative Example 1, it can be clearly seen that the ceramic coating of the present invention cannot be prepared when the temperature is low.

[0055] Comparative Example 2

[0056] No pressure is applied during the sintering process in S3, and other conditions are the same as in Example 1.

[0057] The experimental results are as follows Figure 8 As shown, the coating powder was only loosely attached to the graphite substrate, and the Yb2O3-TiB2-SiC ceramic coating was not successfully prepared.

[0058] The present invention is not limited to the above-mentioned optimal implementation mode. Anyone can derive other various forms of products under the inspiration of the present invention. However, no matter what changes are made in the shape or structure, all technical solutions that are the same or similar to those of the present application fall within the protection scope of the present invention.

Claims

1. A method for preparing a graphite-based Yb2O3-TiB2-SiC ceramic coating material, characterized in that: The following steps are involved: S1. Mix SiC powder, TiB2 powder and Yb2O3 powder in a certain mass ratio to obtain a uniformly mixed raw material powder; S2, pre-treating the graphite substrate; S3. The raw material powder obtained in S1 is coated on the pretreated graphite substrate in S2, and high-temperature sintering is performed under pressure to obtain a graphite-based Yb2O3-TiB2-SiC ceramic coating material.

2. The method for preparing a graphite-based Yb2O3-TiB2-SiC ceramic coating material according to claim 1, characterized in that: In the S1, the particle sizes of SiC powder, TiB2 powder and Yb2O3 powder are all 4-8 μm; the purity of SiC powder, TiB2 powder and Yb2O3 powder is ≥99.9%.

3. The method for preparing a graphite-based Yb2O3-TiB2-SiC ceramic coating material according to claim 1, characterized in that: In the S1, the mass ratio of SiC powder, TiB2 powder and Yb2O3 powder is 2:3:0.

4.

4. The method for preparing a graphite-based Yb2O3-TiB2-SiC ceramic coating material according to claim 1, characterized in that: In the above-mentioned S1, the mixed powders are mixed uniformly by wet ball milling to form slurry, and the slurry is dried and sieved to obtain uniformly mixed raw material powder.

5. The method for preparing a graphite-based Yb2O3-TiB2-SiC ceramic coating material according to claim 4, characterized in that: The mass ratio of the ball mill to the raw material powder is 2:1, the ball composition is ZrO2, and the diameter is 3mm; the ball milling medium is anhydrous ethanol; the ball milling speed is 90r / min, and the ball milling time is 24h.

6. The method for preparing a graphite-based Yb2O3-TiB2-SiC ceramic coating material according to claim 4, characterized in that: During the screening process, a 30-mesh stainless steel screen is used to separate the grinding balls in the slurry, and the separated slurry is placed in a constant temperature drying oven at 80° C. and dried for 12 hours. A 200-mesh stainless steel screen is used to screen the dried powder to obtain a uniformly mixed raw material powder.

7. The method for preparing a graphite-based Yb2O3-TiB2-SiC ceramic coating material according to claim 1, characterized in that: In the above-mentioned S2, the method for pre-treating the graphite substrate powder is: using sandpaper to polish the surface of the graphite substrate, and then performing ultrasonic cleaning and drying operations after polishing.

8. The method for preparing a graphite-based Yb2O3-TiB2-SiC ceramic coating material according to claim 7, characterized in that: The specification of the graphite substrate is a Φ18mm×3mm disc; the graphite substrate is polished using 200-mesh and 800-mesh sandpapers respectively, and the polishing time of the two types of sandpapers on the graphite substrate is 2 minutes; the frequency of ultrasonic cleaning is 40kHz, and the ultrasonic time is 5 minutes; drying is carried out in a constant temperature drying oven, the drying temperature is 80°C, and the drying time is 2 hours.

9. The method for preparing a graphite-based Yb2O3-TiB2-SiC ceramic coating material according to claim 1, characterized in that: In the S3, the temperature control program of the sintering process is: the heating rate below 1000°C is 50°C / min; the heating rate from 1000°C to the maximum temperature is 30°C / min; the holding time after heating to the maximum temperature is 20 minutes; then the temperature is reduced to 1000°C at a rate of 50°C / min, and then cooled to room temperature with the furnace; the maximum temperature is ≥1800°C.

10. The method for preparing a graphite-based Yb2O3-TiB2-SiC ceramic coating material according to claim 1, characterized in that: In the above-mentioned S3, the pressure applied during the sintering process is 30 MPa.

Citation Information

Patent Citations

  • Method for preparing carborundum-coke ytterbium silicate composite coating on surface of carbon / carbon composite material

    CN101805212A

  • Method for preparing HfB2-SiC oxidation resisting coating on surface of carbon-based material

    CN110590404A

  • Environmental barrier coating, environmental barrier component with the same, and method of manufacturing environmental barrier coating

    JP2019214750A