Foaming floating ball and manufacturing method thereof
By using recyclable materials such as EVA particles and additives such as synthetic rubber, foam floats with pressure resistance and good resilience, the problems of easy breakage and difficult degradation of traditional floats are solved, and environmental protection and performance are achieved. promote.
Patent Information
- Application Number
- CN202411162373.9
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-08-23
- Publication Date
- 2024-11-12
AI Technical Summary
Traditional fishing floats are prone to breakage, have poor rebound performance and are difficult to degrade, resulting in environmental pollution and fishing yield.
Foaming floats are made of recyclable materials such as EVA particles, synthetic rubber, PE granules and calcium bicarbonate. The elasticity is increased by adding synthetic rubber, PE granules increases hardness, calcium bicarbonate increases wear resistance, and the float body is added Wear-resistant rings and luminous layers are provided.
The pressure resistance and good rebound of the float ball are achieved, damage is avoided, environmental protection is improved, and it replaces the traditional plastic float ball that is difficult to degrade.
Smart Images

Figure CN118931027A_ABST
Abstract
Description
Technical Field
[0001] The invention relates to the technical field of foaming floats, in particular to a foaming float and a manufacturing method thereof. Background Art
[0002] A float is a solid or hollow sphere that floats on the surface of a liquid due to its shape and material properties. The float is usually made of a material that is less dense than the liquid, such as plastic, rubber or certain metals, to ensure that it can float in the liquid.
[0003] Traditional fishing floats include hollow hard plastic floats, PVC (polyvinyl chloride), EPS (polystyrene) foam floats, etc. Traditional hard plastic floats (hollow) are easily broken after being bumped during use. According to statistics, the annual breakage rate is about 30%, and water leaks in after being broken, which does not play a buoyant role. The nets cannot float up normally, but sink instead, affecting the catch. In work scenarios where a large number of mechanical operations are used, the floats, nets, and machinery are squeezed, collided, and torn against each other. Due to the poor rebound performance of PVC and EPS foam floats, the breakage rate of nets and floats is increased. In addition, PVC and EPS foam floats are difficult to degrade plastic products. If they are discarded at will, they will pollute the environment. Summary of the invention
[0004] In view of the technical problems that the above traditional fishing floats are easy to break and have poor rebound performance, the present invention provides a foam float and a manufacturing method thereof. The foam float uses recyclable EVA as the main raw material, is environmentally friendly, and has good pressure resistance. After being compressed, it has good rebound elasticity and is not easy to break, thereby effectively avoiding damage to the float.
[0005] To this end, the technical solution of the present invention is a foamed float, including a float body and a wear-resistant ring. The interior of the float body is provided with a central axis hole, and one or both ends of the central axis hole are provided with a wear-resistant ring made of hard material. The raw materials for making the float body include EVA particles, synthetic rubber, PE particles and calcium bicarbonate.
[0006] Furthermore, a luminous layer is provided on the outer side of the floating sphere, and fluorescent material is added to the raw materials of the luminous layer.
[0007] Furthermore, the synthetic rubber is one or more of styrene-butadiene rubber, butadiene rubber, isoprene rubber, butyl rubber, chloroprene rubber, ethylene-propylene rubber and nitrile rubber.
[0008] A method for manufacturing a foaming float, the foaming float comprising the following raw materials in weight ratio: 75-80 parts of EVA particles, 5-10 parts of synthetic rubber materials, 5-10 parts of PE particles, 1 part of a cross-linking agent, 1 part of a foaming agent, 1 part of calcium bicarbonate, and 0.5-1 part of color particles, and the specific steps are as follows:
[0009] 1. Ingredients
[0010] According to the raw material ratio of the foaming float, prepare the main material EVA particles and the auxiliary material mixture respectively;
[0011] 2. Rubber refining
[0012] Turn on the internal mixer, add the main ingredient EVA particles, and after the EVA particles are completely melted, pour in the auxiliary material mixture and continue to internally mix, and pour out the mixed rubber;
[0013] Open the mixing mill, put the rubber material on the rubber roller to slice, turn the material over 3-5 times, and then discharge, cut and cool the material;
[0014] Use a grinder to grind the cooled slices for later use;
[0015] 3. Injection molding semi-finished products
[0016] The crushed rubber is injected into semi-finished products using an injection molding machine;
[0017] 4. Make the initial finished product
[0018] After the vulcanizer is equipped with the foaming mold, it is heated to 175-180 degrees using a mold temperature controller. After the temperature reaches a constant temperature, the foaming mold is opened and the semi-finished injection product is loaded. After the mold is closed and heated for the set heating time, the foaming mold automatically pops open and the initial finished product is taken out;
[0019] 5. Finalization of the initial product
[0020] The taken out primary finished product is inserted into the shaping tube and placed on the shaping frame, and the finished foamed float is obtained after the primary product is naturally cooled and plasticized.
[0021] Furthermore, the processing time of the main ingredient EVA particles in the internal mixer is 10-15 minutes, and the temperature is 105-110 degrees.
[0022] Furthermore, the auxiliary material mixture is further kneaded for 5-10 minutes.
[0023] Further, the cooling time is 10-15 minutes.
[0024] Furthermore, the temperature of the injection molding machine is controlled between 95-115 degrees.
[0025] Furthermore, the set heating time is 10-30 minutes.
[0026] Furthermore, the natural cooling and plasticizing time of the primary product is 8-10 hours.
[0027] The beneficial effect of the present invention is that EVA material is used as the main material of the foam float for the first time, replacing the hard plastic float, PVC, and EPS materials of the traditional fishing float. At the same time, in order to meet the requirements of the foam float for elasticity, hardness, and wear resistance, the elasticity is increased by adding synthetic rubber material, the hardness is increased by adding PE particles, and the wear resistance is increased by adding calcium bicarbonate. The foam float uses recyclable EVA as the main raw material, has good environmental protection, and has good pressure resistance. After being compressed, it has good resilience and is not easy to break, which effectively avoids damage to the float. BRIEF DESCRIPTION OF THE DRAWINGS
[0028] Figure 1 It is a schematic diagram of the overall structure of the present invention;
[0029] Figure 2 yes Figure 1 The main view;
[0030] Figure 3 yes Figure 1 sectional view of .
[0031] Explanation of symbols in the figure:
[0032] 1. Floating ball; 101. Center axis hole; 2. Wear-resistant ring; 3. Luminous layer. DETAILED DESCRIPTION
[0033] The following will be combined with the drawings in the embodiments of the present invention to clearly and completely describe the technical solutions in the embodiments of the present invention. Obviously, the described embodiments are only part of the embodiments of the present invention, not all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.
[0034] like Figure 1-Figure 3 As shown, the present invention provides a foaming float, which includes a float body 1 and a wear-resistant ring 2. The raw materials for making the float body 1 include EVA particles (ethylene-vinyl acetate copolymer), synthetic rubber, PE particles (polyethylene), calcium bicarbonate, a cross-linking agent, a foaming agent, color particles and other materials. The raw materials for making the float body 1 can also add other auxiliary materials according to different uses, such as fluorescent materials, etc. The fluorescent material is made of metal (zinc, chromium) sulfide or rare earth oxide and a trace amount of activator through calcination. The synthetic rubber includes one or more of styrene-butadiene rubber, butadiene rubber, isoprene rubber, butyl rubber, chloroprene rubber, ethylene-propylene rubber and nitrile rubber.
[0035] A central axis hole 101 is provided inside the float body 1, and the central axis hole 101 is used for connecting the string of the foam float. According to the characteristics of the foam float product that requires stringing, wear-resistant rings 2 made of hard material are added at both ends of the central axis hole 101 of the float body 1, and according to the mechanical principles in actual applications, the wear-resistant rings 2 are designed with different positions and different curvatures, thereby increasing the service life of the product.
[0036] A luminous layer 3 is provided on the outer side of the float body 1. The luminous layer 3 is made of fluorescent materials. The foam float can be more easily found and identified when used at night.
[0037] The invention discloses a method for manufacturing a foaming float. The foaming float comprises the following raw materials in weight ratio: 75-80 parts of EVA particles, 5-10 parts of synthetic rubber materials, 5-10 parts of PE particles, 1 part of a cross-linking agent, 1 part of a foaming agent, 1 part of calcium bicarbonate, and 0.5-1 part of color particles. The foaming float adopts recyclable EVA as a main raw material, has good environmental protection, and has good pressure resistance. After being compressed, it has good resilience and is not easy to be damaged, thus avoiding damage to the float.
[0038] The present invention uses EVA material as the main material of the foam float for the first time, replacing the hard plastic float, PVC, and EPS materials of the traditional fishing float. At the same time, in order to meet the requirements of the foam float for elasticity, hardness, and wear resistance, the present invention increases the elasticity by adding synthetic rubber material, increases the hardness by adding PE particles, and increases the wear resistance by adding calcium bicarbonate. After two years of research and development and experiments, the above-mentioned added components and their optimal ratios and processing techniques are finally determined.
[0039] The specific steps are as follows:
[0040] 1. Ingredients
[0041] According to the above raw material ratio of the foaming float, prepare the main material EVA particles and the auxiliary material mixture respectively. The auxiliary material mixture is to mix and stir all the auxiliary materials evenly, and put them into a container for later use.
[0042] 2. Rubber refining
[0043] Turn on the internal mixer, wait for the internal mixer to operate normally, pour the main material EVA particles into the internal mixer box, and after running for 10-15 minutes, the temperature is 105-110 degrees. Open the observation port, after the raw material EVA particles are completely melted, pour in the auxiliary material mixture, continue to mix for 5-10 minutes, open the warehouse, and pour out the refined rubber.
[0044] Turn on the mixing mill, put the rubber material on the rubber roller, open the sheet, and turn the material over 3-5 times. After 10-15 minutes of manual sheeting, cutting and cooling, the sheet will be of appropriate hardness and softness.
[0045] Use a crusher to crush the cooled sheets, pack them into bags and set them aside.
[0046] 3. Injection molding semi-finished products
[0047] The crushed rubber is injected into semi-finished products using an injection molding machine. By replacing different types of molds, injection-molded semi-finished products of different shapes and sizes can be produced. The temperature of the injection molding machine is controlled between 95-115 degrees.
[0048] 4. Make the initial finished product
[0049] After the vulcanizer is equipped with the foaming mold, it is heated to 175-180 degrees using a mold temperature controller. After the temperature reaches a constant temperature, the foaming mold is opened and the semi-finished injection product is loaded. After the mold is closed and heated for the set heating time, the foaming mold automatically pops open and the product can be taken out. The set heating time is 10-30 minutes.
[0050] 5. Finalization of the initial product
[0051] Insert the taken out primary finished product into the shaping tube and place it on the shaping rack. After the primary product is naturally cooled and plasticized for 8-10 hours, the finished foamed float ball is obtained. The finished product is taken out, inspected and packaged for storage.
[0052] The EVA foamed float ball product of the present invention is a solid core product, which will not be damaged and water infiltrated, and adopts a closed-cell foaming process, and will not absorb water. According to the needs and directly adjust the color during production, 0.5-1 part of color particles are added, eliminating the pollution problem caused by surface spraying after the product comes out.
[0053] In addition, when a ship is moored at a dock, in order to avoid collision, some old black tires are hung and tied around the hull or at the dock. Although this option is practical, it greatly reduces the aesthetic feeling and reduces the comfort of play. The EVA foamed buoy of the present invention can also replace the old black tires and be used as a fender product for the hull or the dock. It is not only beautiful, but also has strong elasticity, high hardness and good wear resistance.
[0054] However, the above description is only a specific embodiment of the present invention and should not be used to limit the scope of implementation of the present invention. Therefore, the replacement of equivalent components, or equivalent changes and modifications made according to the scope of protection of the present invention should still fall within the scope covered by the claims of the present invention.
Claims
1. A foaming float, characterized in that: It includes a float body and a wear-resistant ring. The float body is provided with a central axis hole inside. One end or both ends of the central axis hole are provided with a wear-resistant ring made of hard material. The raw materials for making the float body include EVA particles, synthetic rubber, PE particles and calcium bicarbonate.
2. A foaming float according to claim 1, characterized in that: A luminous layer is arranged on the outer side of the floating sphere, and the material for making the luminous layer includes fluorescent material.
3. A foaming float according to claim 1, characterized in that: The synthetic rubber is one or more of styrene-butadiene rubber, butadiene rubber, isoprene rubber, butyl rubber, chloroprene rubber, ethylene-propylene rubber and nitrile rubber.
4. A method for manufacturing a foaming float, characterized in that: The foaming float comprises the following raw materials in weight ratio: 75-80 parts of EVA particles, 5-10 parts of synthetic rubber materials, 5-10 parts of PE particles, 1 part of cross-linking agent, 1 part of foaming agent, 1 part of calcium bicarbonate, and 0.5-1 part of color particles. The specific steps are as follows: S1. Ingredients According to the raw material ratio of the foaming float, prepare the main material EVA particles and the auxiliary material mixture respectively; S2. Rubber mixing Turn on the internal mixer, add the main ingredient EVA particles, and after the EVA particles are completely melted, pour in the auxiliary material mixture and continue to internally mix, and pour out the mixed rubber; Open the mixing mill, put the rubber material on the rubber roller to slice, turn the material over 3-5 times, and then discharge, cut and cool the material; Use a grinder to grind the cooled slices for later use; S3. Injection molding semi-finished products The crushed rubber is injected into semi-finished products using an injection molding machine; S4. Make the initial finished product After the vulcanizer is equipped with the foaming mold, it is heated to 175-180 degrees using a mold temperature controller. After the temperature reaches a constant temperature, the foaming mold is opened and the semi-finished injection product is loaded. After the mold is closed and heated for the set heating time, the foaming mold automatically pops open and the initial finished product is taken out; S5. Initial product shaping The taken out primary finished product is inserted into the shaping tube and placed on the shaping frame, and the finished foamed float is obtained after the primary product is naturally cooled and plasticized.
5. The method for manufacturing a foaming float according to claim 4, characterized in that: The processing time of the main ingredient EVA particles in the internal mixer is 10-15 minutes, and the temperature is 105-110 degrees.
6. The method for manufacturing a foaming float according to claim 5, characterized in that: The auxiliary material mixture is further kneaded for 5-10 minutes.
7. The method for manufacturing a foaming float according to claim 4, characterized in that: The cooling time is 10-15 minutes.
8. The method for manufacturing a foaming float according to claim 4, characterized in that: The temperature of the injection molding machine is controlled between 95-115 degrees.
9. The method for manufacturing a foaming float according to claim 4, characterized in that: The set heating time is 10-30 minutes.
10. The method for manufacturing a foaming float according to claim 4, characterized in that: The time for the primary product to be naturally cooled and plasticized is 8-10 hours.