Anti-freezing and anti-cracking composite modified asphalt and preparation method thereof

By using polyurethane-grafted graphene oxide and epoxy soybean oil acrylate in modified asphalt, combined with specific proportions and preparation methods, the problem of insufficient crack resistance of modified asphalt under low temperature conditions is solved, significantly improving the Low-temperature crack resistance and durability reduce cracking risk.

CN118931214APending Publication Date: 2024-11-12WUHAN SILITE HIGHWAY MATERIALS CO LTD
View PDF 0 Cites 5 Cited by

Patent Information

Application Number
CN202411158125.7
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-08-22
Publication Date
2024-11-12

AI Technical Summary

Technical Problem

Existing modified asphalt is prone to cracking under extremely low temperature conditions, resulting in accelerated aging of road surfaces and reduced load-bearing capacity, and insufficient crack resistance, affecting road safety and maintenance costs.

Method used

Polyurethane grafted graphene oxide and epoxy soybean oil acrylate are used to combine specific raw material ratios and preparation methods to improve the flexibility and crack resistance of asphalt and reduce the risk of cracking.

Benefits of technology

It significantly improves the low-temperature crack resistance of modified asphalt, extends the service life of the road surface, reduces the risk of cracking, and optimizes production efficiency and raw material compatibility.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure BDA0005005655890000071
    Figure BDA0005005655890000071
  • Figure BDA0005005655890000081
    Figure BDA0005005655890000081
Patent Text Reader

Abstract

The invention relates to the technical field of asphalt. The invention discloses anti-freezing and anti-cracking composite modified asphalt and a preparation method thereof. The modified asphalt is prepared from the following raw materials: matrix asphalt, SBS (Styrene Butadiene Styrene), rubber powder, an antioxidant, a plasticizer, polyurethane grafted graphene oxide and epoxidized soybean oil acrylate. The preparation method comprises the following steps: S1, heating matrix asphalt to 160-180 DEG C, adding SBS, and shearing to obtain a premix; s2, adding rubber powder into the premix, stirring, sequentially adding an antioxidant, a plasticizer, polyurethane grafted graphene oxide and epoxidized soybean oil acrylate, and stirring to obtain the anti-freezing and anti-cracking composite modified asphalt. The prepared modified asphalt is excellent in low-temperature crack resistance, the cracking risk of a pavement can be reduced, and the durability of the asphalt pavement is improved.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present application relates to the technical field of asphalt, and in particular to an antifreeze and anti-cracking composite modified asphalt and a preparation method thereof. Background Art

[0002] With the rapid development of the transportation industry, road infrastructure is facing higher and higher performance requirements. Especially in the cold northern regions, road maintenance and durability under low temperature conditions have become an urgent problem to be solved. Traditional asphalt materials are prone to brittle cracking under low temperature conditions, resulting in road surface damage, which seriously affects the service life and service quality of the road. Therefore, the development of modified asphalt is very important.

[0003] Modified asphalt is an asphalt binder made by adding admixtures (modifiers) such as rubber, resin, high molecular polymer, ground rubber powder or other fillers to the base asphalt, or by taking measures such as mild oxidation of the asphalt to improve the performance of asphalt or asphalt mixture.

[0004] Existing modified asphalt has improved the performance of asphalt pavement to a certain extent, but there are still some problems in its application in cold northern regions. Under extreme low temperature conditions, the pavement is still prone to cracking due to low temperature brittleness problems. These cracks will not only accelerate the aging process of the pavement, but also cause rainwater to penetrate into the roadbed, causing the base layer to soften, thereby further aggravating pavement damage and reducing the pavement's bearing capacity. In addition, the crack resistance of existing modified asphalt under low temperature conditions still needs to be improved. Under the repeated action of traffic loads, the pavement may have secondary serious pavement problems such as potholes and cracks. These problems not only affect driving safety, but also increase the cost and frequency of road maintenance.

[0005] Therefore, there is an urgent need to develop a modified asphalt with excellent low-temperature crack resistance, which can reduce the cracking risk of road pavements paved with modified asphalt under the cold environmental conditions of northern winter and improve the durability of asphalt pavements. Summary of the invention

[0006] In order to solve at least one of the above technical problems, a modified asphalt with excellent low-temperature crack resistance is developed. The present application provides an antifreeze and anti-cracking composite modified asphalt and a preparation method thereof.

[0007] On the one hand, the present application provides an antifreeze and anti-cracking composite modified asphalt, whose raw material composition includes, by weight: 80-100 parts of base asphalt, 5-10 parts of SBS, 10-15 parts of rubber powder, 0.1-1 parts of antioxidant, 1-3 parts of plasticizer, 0.5-1.5 parts of polyurethane grafted graphene oxide, and 0.5-1.5 parts of epoxy soybean oil acrylate.

[0008] By adopting the above technical scheme, the present application adopts specific raw materials and proportions to prepare modified asphalt with excellent low-temperature crack resistance, which can reduce the cracking risk of road pavement paved with modified asphalt under the cold environmental conditions of northern winter and improve the durability of asphalt pavement.

[0009] This application adds polyurethane grafted graphene oxide, which has good weather resistance and chemical corrosion resistance, can enhance the durability of asphalt, extend the service life of the road surface, and improve the flexibility and crack resistance of asphalt. This application adds epoxy soybean oil acrylate, which can improve the flexibility of asphalt at low temperatures, thereby reducing the risk of cracking caused by temperature changes.

[0010] The polyurethane grafted graphene oxide and epoxy soybean oil acrylate in the present application work together to improve the flexibility of asphalt and reduce the brittle temperature, thereby improving the low-temperature performance and crack resistance of the modified asphalt.

[0011] Optionally, the raw material composition includes, by weight: 85-95 parts of base asphalt, 6-9 parts of SBS, 12-13 parts of rubber powder, 0.3-0.7 parts of antioxidant, 1.5-2.5 parts of plasticizer, 0.8-1.2 parts of polyurethane grafted graphene oxide, and 0.8-1.2 parts of epoxy soybean oil acrylate.

[0012] Optionally, the raw material composition includes, by weight: 90 parts of base asphalt, 7.5 parts of SBS, 12.5 parts of rubber powder, 0.5 parts of antioxidant, 2 parts of plasticizer, 1 part of polyurethane grafted graphene oxide, and 1 part of epoxy soybean oil acrylate.

[0013] Optionally, the needle penetration of the base asphalt is 80 to 120 1 / 10 mm.

[0014] By adopting the above technical solution, the needle penetration of the base asphalt of the present application can ensure that the modified asphalt has good low-temperature ductility and crack resistance.

[0015] Optionally, the average particle size of the rubber powder is 0.1 to 0.5 mm.

[0016] By adopting the above technical solution, the average particle size of the rubber powder of the present application can make it better dispersed in asphalt, and can effectively improve the low temperature performance and crack resistance of the modified asphalt.

[0017] Optionally, the antioxidant is selected from at least one of 2,6-di-tert-butyl-4-methylphenol, dilauryl thiodipropionate and N,N'-diphenyl-1,4-phenylenediamine.

[0018] By adopting the above technical solution, the antioxidant of the present application can prevent the performance of asphalt from deteriorating due to oxidation during long-term use, slow down the aging process of asphalt, and improve its durability and long-term stability.

[0019] Optionally, the plasticizer is selected from at least one of dioctyl phthalate, triphenyl phosphate and dioctyl adipate.

[0020] By adopting the above technical solution, the plasticizer of the present application can improve the flexibility of asphalt, making it less prone to brittle cracking at low temperatures, thereby improving its low-temperature performance and crack resistance.

[0021] Optionally, the preparation method of the polyurethane grafted graphene oxide is: Step 1: dispersing graphene oxide in water to obtain a graphene oxide aqueous solution; Step 2: mixing isocyanate and polyether polyol to prepare a polyurethane precursor; Step 3: adding the graphene oxide aqueous solution to the polyurethane precursor, adding 0.1-0.5wt% of dibutyltin dilaurate, reacting for 4-6h, centrifuging, washing, and drying to obtain polyurethane grafted graphene oxide; Wherein, the weight ratio of graphene oxide, isocyanate and polyether polyol is 1:1-3:8-12.

[0022] Optionally, the weight ratio of the polyurethane grafted graphene oxide to the epoxy soybean oil acrylate is 1:0.8-1.2.

[0023] By adopting the above technical scheme, the polyurethane grafted graphene oxide and epoxy soybean oil acrylate of the present application work together to further improve the flexibility of the modified asphalt and reduce the brittle temperature, thereby improving its low temperature performance and crack resistance.

[0024] In a second aspect, the present application provides a method for preparing the above-mentioned antifreeze and anti-cracking composite modified asphalt, comprising the following steps: S1. Heat the base asphalt to 160° C. to 180° C., add the SBS, and shear at a speed of 1000 to 2000 rpm for 10 to 20 minutes to obtain a premix; S2. Add the rubber powder to the premix, stir at a speed of 300-500 rpm for 30-60 min, add the antioxidant, plasticizer, polyurethane grafted graphene oxide, and epoxy soybean oil acrylate in sequence, stir for 30-60 min, and obtain the antifreeze and anti-cracking composite modified asphalt.

[0025] By adopting the above technical solution, the preparation method adopted in this application has a simple process and high production efficiency. The raw materials have good compatibility and dispersibility, further optimizing the low temperature performance and crack resistance of the modified asphalt, and improving its applicability in cold regions.

[0026] In summary, the present invention includes at least one of the following beneficial technical effects: 1. The modified asphalt prepared by the application adopts specific raw materials and proportions and has excellent low-temperature crack resistance, which can reduce the cracking risk of roads paved with modified asphalt under the cold environmental conditions of northern winter and improve the durability of asphalt pavement.

[0027] 2. The polyurethane grafted graphene oxide and epoxy soybean oil acrylate of the present application work together to improve the flexibility of asphalt and improve the low temperature performance and crack resistance of the modified asphalt.

[0028] 3. The preparation method adopted in this application has a simple process and high production efficiency. The raw materials have good compatibility and dispersibility, which further optimizes the low temperature performance and crack resistance of the modified asphalt. DETAILED DESCRIPTION

[0029] The present application is further described in detail below with reference to the embodiments.

[0030] The present application designs an antifreeze and anti-cracking composite modified asphalt, and its raw material composition includes, by weight: 80-100 parts of base asphalt, 5-10 parts of SBS, 10-15 parts of rubber powder, 0.1-1 parts of antioxidant, 1-3 parts of plasticizer, 0.5-1.5 parts of polyurethane grafted graphene oxide, and 0.5-1.5 parts of epoxy soybean oil acrylate.

[0031] The antifreeze and anti-cracking composite modified asphalt of the present application is prepared by the following method, comprising the following steps: S1. Heat the base asphalt to 160° C. to 180° C., add the SBS, and shear at a speed of 1000 to 2000 rpm for 10 to 20 minutes to obtain a premix; S2. Add the rubber powder to the premix, stir at a speed of 300-500 rpm for 30-60 min, add the antioxidant, plasticizer, polyurethane grafted graphene oxide, and epoxy soybean oil acrylate in sequence, stir for 30-60 min, and obtain the antifreeze and anti-cracking composite modified asphalt.

[0032] The applicant has designed the technical solution of the present application to address the problem that the existing modified asphalt has insufficient anti-cracking performance under low temperature conditions.

[0033] The raw materials used in this application are as follows: SBS:CAS:9003-55-8.

[0034] 2,6-Di-tert-butyl-4-methylphenol: CAS: 128-37-0.

[0035] Dilauryl thiodipropionate: CAS: 123-28-4.

[0036] Dioctyl phthalate: CAS: 117-84-0.

[0037] Dioctyl adipate: CAS: 123-79-5.

[0038] Isocyanate: CAS: 75-13-8.

[0039] Polyether polyol: CAS: 9003-11-6.

[0040] Dibutyltin dilaurate: CAS: 77-58-7.

[0041] Epoxidized soybean oil acrylate: Huainan Kedi Chemical Technology Co., Ltd. Specific embodiments

[0042] The preparation method of polyurethane grafted graphene oxide used in Examples 1 to 5 is: Step 1: dispersing graphene oxide in water to obtain a graphene oxide aqueous solution; Step 2: mixing isocyanate and polyether polyol to prepare a polyurethane precursor; Step 3: adding the graphene oxide aqueous solution to the polyurethane precursor, adding 0.3wt% of dibutyltin dilaurate, reacting for 5h, centrifuging, washing, and drying to obtain polyurethane-grafted graphene oxide; Among them, the weight ratio of graphene oxide, isocyanate and polyether polyol is 1:2:10.

[0043] Examples 1 to 5 Example 1 This embodiment provides an antifreeze and anti-cracking composite modified asphalt, and its raw material composition includes, by weight: 80 parts of base asphalt, 10 parts of SBS, 15 parts of rubber powder, 0.1 parts of antioxidant, 3 parts of plasticizer, 0.5 parts of polyurethane grafted graphene oxide, and 0.5 parts of epoxy soybean oil acrylate; The penetration of the base asphalt is 100 1 / 10 mm; the average particle size of the rubber powder is 0.3 mm; the antioxidant is 2,6-di-tert-butyl-4-methylphenol; the plasticizer is dioctyl phthalate; The preparation method comprises the following steps: S1. Heat the base asphalt to 160°C, add SBS, and shear at a speed of 2000 rpm for 10 minutes to prepare a premix; S2. Add rubber powder to the premix, stir at a speed of 500 rpm for 30 minutes, add antioxidant, plasticizer, polyurethane grafted graphene oxide, and epoxy soybean oil acrylate in sequence, stir for 30 minutes, and prepare antifreeze and anti-cracking composite modified asphalt.

[0044] Example 2 This embodiment provides an antifreeze and anti-cracking composite modified asphalt, and its raw material composition includes, by weight: 95 parts of base asphalt, 6 parts of SBS, 12 parts of rubber powder, 0.7 parts of antioxidant, 1.5 parts of plasticizer, 0.8 parts of polyurethane grafted graphene oxide, and 0.8 parts of epoxy soybean oil acrylate; The penetration of the base asphalt is 100 1 / 10 mm; the average particle size of the rubber powder is 0.3 mm; the antioxidant is 2,6-di-tert-butyl-4-methylphenol; the plasticizer is dioctyl phthalate; The preparation method comprises the following steps: S1. Heat the base asphalt to 165°C, add SBS, and shear at a speed of 1800 rpm for 12 minutes to prepare a premix; S2. Add rubber powder to the premix, stir at a speed of 450 rpm for 35 minutes, add antioxidant, plasticizer, polyurethane grafted graphene oxide, and epoxy soybean oil acrylate in sequence, stir for 35 minutes, and prepare antifreeze and anti-cracking composite modified asphalt.

[0045] Example 3 This embodiment provides an antifreeze and anti-cracking composite modified asphalt, and its raw material composition includes, by weight: 90 parts of base asphalt, 7.5 parts of SBS, 12.5 parts of rubber powder, 0.5 parts of antioxidant, 2 parts of plasticizer, 1 part of polyurethane grafted graphene oxide, and 1 part of epoxy soybean oil acrylate; The penetration of the base asphalt is 100 1 / 10 mm; the average particle size of the rubber powder is 0.3 mm; the antioxidant is 2,6-di-tert-butyl-4-methylphenol; the plasticizer is dioctyl phthalate; The preparation method comprises the following steps: S1. Heat the base asphalt to 170°C, add SBS, and shear at a speed of 1500 rpm for 15 minutes to prepare a premix; S2. Add rubber powder to the premix, stir at 400 rpm for 45 min, add antioxidant, plasticizer, polyurethane grafted graphene oxide, and epoxy soybean oil acrylate in sequence, stir for 45 min, and prepare antifreeze and anti-cracking composite modified asphalt.

[0046] Example 4 This embodiment provides an antifreeze and anti-cracking composite modified asphalt, and its raw material composition includes, by weight: 85 parts of base asphalt, 9 parts of SBS, 13 parts of rubber powder, 0.3 parts of antioxidant, 2.5 parts of plasticizer, 1.2 parts of polyurethane grafted graphene oxide, and 1.2 parts of epoxy soybean oil acrylate; The penetration of the base asphalt is 100 1 / 10 mm; the average particle size of the rubber powder is 0.3 mm; the antioxidant is 2,6-di-tert-butyl-4-methylphenol; the plasticizer is dioctyl phthalate; The preparation method comprises the following steps: S1. Heat the base asphalt to 175°C, add SBS, and shear at a speed of 1200 rpm for 18 minutes to prepare a premix; S2. Add rubber powder to the premix, stir at a speed of 350 rpm for 55 minutes, add antioxidant, plasticizer, polyurethane grafted graphene oxide, and epoxy soybean oil acrylate in sequence, stir for 55 minutes, and prepare antifreeze and anti-cracking composite modified asphalt.

[0047] Example 5 This embodiment provides an antifreeze and anti-cracking composite modified asphalt, and its raw material composition includes, by weight: 100 parts of base asphalt, 5 parts of SBS, 10 parts of rubber powder, 1 part of antioxidant, 1 part of plasticizer, 1.5 parts of polyurethane grafted graphene oxide, and 1.5 parts of epoxy soybean oil acrylate; The penetration of the base asphalt is 100 1 / 10 mm; the average particle size of the rubber powder is 0.3 mm; the antioxidant is 2,6-di-tert-butyl-4-methylphenol; the plasticizer is dioctyl phthalate; The preparation method comprises the following steps: S1. Heat the base asphalt to 180°C, add SBS, and shear at a speed of 1000 rpm for 20 minutes to prepare a premix; S2. Add rubber powder to the premix, stir at a speed of 300 rpm for 60 minutes, add antioxidant, plasticizer, polyurethane grafted graphene oxide, and epoxy soybean oil acrylate in sequence, stir for 60 minutes, and prepare antifreeze and anti-cracking composite modified asphalt.

[0048] Comparative Examples 1 to 4 Comparative Example 1 The difference between Comparative Example 1 and Example 3 is that polyurethane-grafted graphene oxide and epoxy soybean oil acrylate are not added in Comparative Example 1.

[0049] Comparative Example 2 The difference between Comparative Example 2 and Example 3 is that no polyurethane-grafted graphene oxide is added in Comparative Example 2.

[0050] Comparative Example 3 The difference between Comparative Example 3 and Example 3 is that no epoxy soybean oil acrylate is added in Comparative Example 3.

[0051] Comparative Example 4 The difference between Comparative Example 4 and Example 3 is that the preparation method of Comparative Example 4 is: S1. Heat the base asphalt to 170°C, add SBS, and shear at a speed of 1500 rpm for 15 minutes to prepare a premix; S2. Add rubber powder, antioxidant, plasticizer, polyurethane grafted graphene oxide and epoxy soybean oil acrylate into the premix, stir at a speed of 400 rpm for 45 minutes to obtain antifreeze and anti-cracking composite modified asphalt.

[0052] Experimental testing Test items and test methods Low temperature crack resistance: According to T0604-2011 in JTG E20-2011 "Test Procedures for Asphalt and Asphalt Mixtures for Highway Engineering", the penetration of antifreeze and anti-cracking composite modified asphalt is measured; T0606-2011 is used to measure the softening point; T0605-2011 is used to measure the ductility; T0613-1993 is used to measure the brittle point; Durability: The prepared antifreeze and anti-cracking composite modified asphalt was placed in an aging box at 175°C for 5 hours, and the elongation retention rate was tested; elongation retention rate = (elongation after aging test / elongation before aging test) × 100%.

[0053] The antifreeze and anti-cracking composite modified asphalts prepared in Examples 1 to 5 and Comparative Examples 1 to 4 were tested for penetration, softening point, ductility, brittle point and ductility retention rate. The test results are shown in Table 1.

[0054] Table 1 From the test results in Table 1, it can be seen that the frost-resistant and crack-resistant composite modified asphalt prepared in Examples 1 to 5 has high ductility, low brittle point, excellent low-temperature crack resistance, high ductility retention rate and good durability after aging test.

[0055] Comparative Example 1 did not add polyurethane grafted graphene oxide and epoxy soybean oil acrylate, Comparative Example 2 did not add polyurethane grafted graphene oxide, and Comparative Example 3 did not add epoxy soybean oil acrylate. The low-temperature crack resistance of the antifreeze and anti-cracking composite modified asphalt prepared in Comparative Examples 1 to 3 was significantly reduced, and the durability deteriorated.

[0056] In step S2 of comparative example 4, the raw materials are mixed and stirred together without being added sequentially, so the low-temperature crack resistance and durability of the antifreeze and anti-cracking composite modified asphalt obtained are both reduced.

[0057] Embodiments 6 to 11 Example 6 The difference between Example 6 and Example 3 is that in Example 6, the average particle size of the rubber powder is 0.1 mm.

[0058] Example 7 The difference between Example 7 and Example 3 is that in Example 7, the average particle size of the rubber powder is 0.5 mm.

[0059] Example 8 The difference between Example 8 and Example 3 is that in Example 8, the antioxidant is dilauryl thiodipropionate.

[0060] Example 9 The difference between Example 9 and Example 3 is that in Example 9, the plasticizer is dioctyl adipate.

[0061] Example 10 The difference between Example 10 and Example 3 is that in Example 10, the total weight of polyurethane grafted graphene oxide and epoxy soybean oil acrylate remains unchanged, and the weight ratio of polyurethane grafted graphene oxide to epoxy soybean oil acrylate is 1:0.8.

[0062] Embodiment 11 The difference between Example 11 and Example 3 is that in Example 11, the total weight of polyurethane grafted graphene oxide and epoxy soybean oil acrylate remains unchanged, and the weight ratio of polyurethane grafted graphene oxide to epoxy soybean oil acrylate is 1:1.2.

[0063] The antifreeze and anti-cracking composite modified asphalts prepared in Examples 6 to 11 were tested for penetration, softening point, ductility, brittle point and ductility retention. The test results are shown in Table 2.

[0064] Table 2 From the test results in Table 2, it can be seen that the difference between Example 6 and Example 7 and Example 3 is that the average particle size of the rubber powder is different. Among them, the antifreeze and anti-cracking composite modified asphalt prepared in Example 3 has the best low-temperature crack resistance and durability.

[0065] The low-temperature crack resistance and durability of the frost-resistant and crack-resistant composite modified asphalt prepared in Examples 8 to 9 are similar to those in Example 3.

[0066] The difference between Example 10 and Example 11 and Example 3 is that the weight ratios of polyurethane grafted graphene oxide and epoxy soybean oil acrylate are different. Among them, the antifreeze and anti-cracking composite modified asphalt prepared in Example 3 has the best low-temperature crack resistance and durability.

[0067] The above are all preferred embodiments of the present application, and the protection scope of the present application is not limited thereto. Therefore, any equivalent changes made according to the structure, shape, and principle of the present application should be included in the protection scope of the present application.

Claims

1. A frost-resistant and crack-resistant composite modified asphalt, characterized in that: The raw material composition includes, by weight: 80-100 parts of base asphalt, 5-10 parts of SBS, 10-15 parts of rubber powder, 0.1-1 parts of antioxidant, 1-3 parts of plasticizer, 0.5-1.5 parts of polyurethane grafted graphene oxide, and 0.5-1.5 parts of epoxy soybean oil acrylate.

2. The antifreeze and anti-cracking composite modified asphalt according to claim 1, characterized in that: The raw material composition includes, by weight: 85-95 parts of base asphalt, 6-9 parts of SBS, 12-13 parts of rubber powder, 0.3-0.7 parts of antioxidant, 1.5-2.5 parts of plasticizer, 0.8-1.2 parts of polyurethane grafted graphene oxide, and 0.8-1.2 parts of epoxy soybean oil acrylate.

3. The antifreeze and anti-cracking composite modified asphalt according to claim 1, characterized in that: The raw material composition includes, by weight: 90 parts of base asphalt, 7.5 parts of SBS, 12.5 parts of rubber powder, 0.5 parts of antioxidant, 2 parts of plasticizer, 1 part of polyurethane grafted graphene oxide, and 1 part of epoxy soybean oil acrylate.

4. The antifreeze and anti-cracking composite modified asphalt according to claim 1, characterized in that: The needle penetration of the base asphalt is 80~120 1 / 10mm.

5. The antifreeze and anti-cracking composite modified asphalt according to claim 1, characterized in that: The average particle size of the rubber powder is 0.1-0.5 mm.

6. The antifreeze and anti-cracking composite modified asphalt according to claim 1, characterized in that: The antioxidant is selected from at least one of 2,6-di-tert-butyl-4-methylphenol, dilauryl thiodipropionate and N,N'-diphenyl-1,4-phenylenediamine.

7. The antifreeze and anti-cracking composite modified asphalt according to claim 1, characterized in that: The plasticizer is selected from at least one of dioctyl phthalate, triphenyl phosphate and dioctyl adipate.

8. The antifreeze and anti-cracking composite modified asphalt according to claim 1, characterized in that: The preparation method of the polyurethane grafted graphene oxide is: Step 1: dispersing graphene oxide in water to obtain a graphene oxide aqueous solution; Step 2: mixing isocyanate and polyether polyol to prepare a polyurethane precursor; Step 3: adding the graphene oxide aqueous solution to the polyurethane precursor, adding 0.1-0.5wt% of dibutyltin dilaurate, reacting for 4-6h, centrifuging, washing, and drying to obtain polyurethane-grafted graphene oxide; Wherein, the weight ratio of graphene oxide, isocyanate and polyether polyol is 1:1~3:8~12.

9. The antifreeze and anti-cracking composite modified asphalt according to claim 1, characterized in that: The weight ratio of the polyurethane grafted graphene oxide to the epoxy soybean oil acrylate is 1:0.8-1.

2.

10. A method for preparing the antifreeze and anti-cracking composite modified asphalt according to any one of claims 1 to 9, characterized in that: The following steps are involved: S1. Heat the base asphalt to 160°C-180°C, add the SBS, and shear at a speed of 1000-2000 rpm for 10-20 min to obtain a premix; S2. Add the rubber powder to the premix, stir at a speed of 300-500 rpm for 30-60 min, add the antioxidant, plasticizer, polyurethane grafted graphene oxide, and epoxy soybean oil acrylate in sequence, stir for 30-60 min, and obtain the antifreeze and anti-cracking composite modified asphalt.

Citation Information

Cited By

  • Polyphosphoric acid-polymer composite modified asphalt and preparation method thereof

    CN120173426A

  • Polyphosphoric acid-polymer complex modified asphalt and method for preparing the same

    CN120173426B

  • Anti-crack plastomer modified asphalt and preparation method thereof

    CN120310287A

  • Tough synergistic composite modified asphalt for hydraulic panel leveling layer and preparation method of tough synergistic composite modified asphalt

    CN120623799A

  • Tough synergy type composite modified asphalt for hydraulic panel leveling layer and preparation method thereof