Titanium material base material, electrode comprising titanium material base material and preparation methods of titanium material base material and electrode
Through the combination of high-grade titanium substrate and thermal oxidation method, the problem of poor performance of chlorine-eliminated electrode materials is solved, the life and qualification rate of the electrode are improved, and the needs of industrial production are met.
Patent Information
- Application Number
- CN202411315409.2
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-09-20
- Publication Date
- 2024-11-12
AI Technical Summary
The catalytic crystal oxidation properties of existing chlorine-eliminated electrode materials are unstable, have inconsistent morphology, uneven coatings, and are not tightly bound to the substrate, resulting in low electrode performance and low pretreatment efficiency of titanium substrates, which cannot meet the needs of industrial production. .
High-level titanium substrates are prepared by hot continuous rolling, cold rolling and step-by-step annealing treatment, and titanium substrates with grain sizes of 9-9.5, and the surface is covered by sulfuric acid etching and thermal oxidation. Platinum group precious metal catalyst improves the conductivity of the substrate and the solid solution effect of the catalyst.
It improves the conductivity of the titanium substrate and the uniformity of the catalyst, extends the life of the electrode, reduces the potential of the chlorine evolution reaction, improves the product pass rate, shortens the pretreatment time, and meets the needs of large-scale production.
Smart Images

Figure CN118932375A_ABST
Abstract
Description
Technical Field
[0001] The present invention relates to the technical field of electrochemical material preparation, and in particular to a titanium substrate and an electrode containing the same, and methods for preparing the two. Background Art
[0002] Chlorine electrode usually refers to the anode electrode specially used for precipitating chlorine gas during the electrolysis process. When electrolyzing a solution containing chloride ions (such as salt water or seawater), if the potential on the anode (positive electrode) is high enough, the chloride ions will lose electrons on the anode, thereby generating chlorine gas. Chlorine electrode is an important electrode material, which is widely used in the fields of electrolysis industry, chemical production and environmental protection. The performance of chlorine electrode directly affects the electrolysis efficiency and the quality of electrolysis products.
[0003] At present, the mainstream methods to improve the performance of chlorine evolution electrodes mainly focus on improving the composition and manufacturing process of chlorine evolution catalysts. For example, adjusting the proportion of precious metal elements in the catalyst coating, adding non-precious metal catalysts to optimize the catalyst cost and performance, changing the catalyst coating method to roller coating, electrostatic spraying, plasma spraying, changing the catalyst oxidation temperature, time, oxidation atmosphere, etc., although these methods can improve the performance of chlorine evolution electrodes. However, due to the differences in the process and final morphology of catalytic crystals formed by different catalyst elements, although industry researchers have conducted a lot of research on its coating method and oxidation conditions, the chlorine evolution catalytic coating still has defects such as unstable catalytic crystal oxidation performance, inconsistent shape, uneven coating, cracked and porous, and loose bonding with the substrate, and the application of precious metal catalysts significantly increases the cost of chlorine evolution electrodes. In addition, the use of mass-produced titanium substrates to make chlorine evolution electrodes, its pretreatment efficiency, chlorine evolution overpotential and product qualification rate obviously do not meet the needs of industrial production. Summary of the invention
[0004] 1. Technical issues to be resolved
[0005] In view of the above-mentioned shortcomings and deficiencies of the prior art, the present invention provides a titanium substrate and an electrode containing the same and a method for preparing the two, which solves the technical problems that the current titanium substrate has poor uniformity, resistance and other properties resulting in low electrode performance, and in the process of producing electrodes using titanium substrates, the substrate pretreatment time is long resulting in low electrode production efficiency.
[0006] (II) Technical solution
[0007] In order to achieve the above object, the main technical solutions adopted by the present invention include:
[0008] In a first aspect, an embodiment of the present invention provides a titanium substrate having a grain size of 9-9.5, wherein, by mass percentage, the oxygen content is ≤0.03%, the nitrogen content is ≤0.009%, and the hydrogen content is ≤0.008%.
[0009] In a second aspect, an embodiment of the present invention provides an electrode, comprising the titanium substrate described in the first aspect.
[0010] In a third aspect, an embodiment of the present invention provides a method for preparing the electrode according to the second aspect, comprising the following steps:
[0011] Step 1, roughening the surface of the titanium substrate: using a 20-30% by mass sulfuric acid solution at 60-95° C. for etching for 2.5±0.5 h, and then cleaning and drying the titanium substrate to obtain a titanium substrate with a roughened surface;
[0012] Step 2: coating the roughened titanium substrate with a catalyst coating to produce the electrode.
[0013] As a preferred embodiment of the present invention, in the electrode preparation method, in step 2, the process of coating the catalyst coating is to coat the platinum group precious metal elements by thermal oxidation.
[0014] In a fourth aspect, an embodiment of the present invention provides a method for preparing the aforementioned titanium substrate, comprising the following steps:
[0015] S1. Hot rolling: hot rolling and annealing the titanium slab in sequence to obtain primary titanium material;
[0016] S2, cold rolling: cold rolling and cleaning the primary titanium material to obtain the secondary titanium material;
[0017] S3, step annealing: Under an inert atmosphere and negative pressure, the second-grade titanium material is subjected to two-stage step-wise annealing, and then surface treatment is performed to obtain the third-grade titanium material;
[0018] S4, finished product annealing: anneal the grade 3 titanium material, and then obtain the titanium base material by stretching and straightening.
[0019] As a preferred embodiment of the present invention, in the method for preparing the titanium substrate, in S1, the titanium slab is made by melting sponge titanium with a titanium content of ≥99.999% into a titanium ingot, and the hot rolling temperature is 800-900°C in an inert atmosphere, and the thickness of the final primary titanium material after rolling is 4-100mm;
[0020] The annealing process is carried out in an inert atmosphere at 600-750°C for 5-10 minutes, and surface impurities are removed after cooling.
[0021] As a preferred embodiment of the present invention, in the method for preparing the titanium substrate, in S2, the cold rolling process is: after rolling the primary titanium material, annealing treatment is performed: in an inert atmosphere, the temperature is maintained at 620-680° C. for 5-10 minutes, and after cooling, rolling again to roll the primary titanium material to a thickness that meets the finished product thickness;
[0022] In S4, the annealing process is to keep the temperature at 620-680° C. for 5-10 minutes in an inert gas atmosphere.
[0023] As a preferred embodiment of the present invention, in the method for preparing the titanium substrate, in S3, the first step-by-step heating process is: in an inert gas atmosphere, maintaining a negative pressure environment, heating to 400-430°C at a heating rate of 60-80°C / h, and keeping warm for 2-3h.
[0024] The second stage of step-by-step heating process is as follows: based on the first stage of step-by-step heating annealing, in an inert gas atmosphere, maintaining a negative pressure environment, continuing to heat up to 680-720°C at a heating rate of 30-40°C / h, and keeping warm for 6-8h.
[0025] As a preferred embodiment of the present invention, in the method for preparing the titanium substrate, in S3, after the second stage of stepwise heating, the secondary titanium material is cooled to 200°C at a cooling rate of 50-60°C / h, and then rapidly cooled.
[0026] As a preferred embodiment of the present invention, in the method for preparing the titanium substrate, in S3, the vacuum degree of the negative pressure environment in the two-stage step-by-step heating is on the order of 10 -3 Pa.
[0027] (III) Beneficial effects
[0028] The beneficial effects of the present invention are: a titanium substrate and an electrode containing the same and a preparation method of the two of the present invention, wherein the grain size of the titanium substrate is 9-9.5, and the grain size is high; the oxygen content in the titanium substrate is ≤0.03%, the nitrogen content is ≤0.009%, and the hydrogen content is ≤0.008%. Compared with the prior art, the reduction in the O, N, and H contents reduces the substrate resistance, improves the intracrystalline and intercrystalline electron conduction efficiency, and enhances the substrate conductivity.
[0029] When the titanium substrate is used to prepare the electrode, the above crystal structure characteristics of the substrate ensure that the rutile structure does not change when the TiO2 crystals in the titanium substrate are generated, thereby strengthening the solid solution effect of the substrate and the catalyst crystals when the substrate is used to make the electrode, and improving the life of the electrode. In addition, the increase in the grain size of the substrate increases the number of microstructures of the substrate after acid etching, thereby increasing the electrode specific surface area and catalytic crystal nucleation sites, improving the specific surface area, uniformity and firmness of the catalyst coating on the electrode surface, and thus greatly extending the life of the electrode; the conductivity of the substrate and the catalytic ability of the coating are improved at the same time, thereby reducing the potential of the chlorine evolution reaction of the chlorine evolution electrode, and overall improving the electrode potential and life, so that the product qualification rate is significantly improved.
[0030] The crystal surface is more easily exchanged with hydrogen ions and corroded rapidly, and the grains are small and uniform. The overall etching rate of the substrate is faster during the roughening treatment, and the rough surface formed is more consistent. The improvement in the acid etching roughening efficiency shortens the pretreatment time of titanium materials for electrode production, overcomes the limitation of the bottleneck process of titanium material pretreatment on production efficiency, and meets the needs of large-scale production of electrodes.
[0031] During the electrode preparation process, 20-30% sulfuric acid solution is used at 60-95°C to roughen the surface of the titanium substrate, which further improves the uniformity of the catalyst coating during electrode production and increases the specific surface area of the substrate. The pretreatment efficiency of the titanium substrate during electrode production is increased by 1 times (from 5h / batch to 2.5h / batch). Ultimately, the qualified rate of electrode products is increased by 1.42 times (from 40% to 97%), the electrode electrolysis voltage is reduced by 20mV, and the energy consumption is reduced by 12.5kw.h / t.
[0032] In the preparation of the titanium substrate, hot rolling, cold rolling and two-stage step-by-step annealing are adopted, and then the finished product is annealed to ensure uniform grain growth. The grain size of the finally prepared titanium substrate is 9-9.5, and the contents of O, N and H are reduced. At the same time, the performance of the substrate is uniform and stable during mass production, which significantly improves the qualified rate of the corresponding electrode products and is suitable for large-scale production. BRIEF DESCRIPTION OF THE DRAWINGS
[0033] Figure 1 This is a SEM image of the corrosion morphology of the titanium substrate in Example 4;
[0034] Figure 2 This is a SEM image of the catalyst coating on the surface of the titanium substrate in Example 4;
[0035] Figure 3 This is a SEM image of the corrosion morphology of the titanium substrate in Example 5;
[0036] Figure 4 This is a SEM image of the catalyst coating on the surface of the titanium substrate in Example 5;
[0037] Figure 5 This is a SEM image of the corrosion morphology of the titanium substrate in Example 6;
[0038] Figure 6 This is a SEM image of the catalyst coating on the surface of the titanium substrate in Example 6;
[0039] Figure 7 This is a SEM image of the corrosion morphology of the titanium substrate in Comparative Example 1;
[0040] Figure 8 This is a SEM image of the catalyst coating on the surface of the titanium substrate in Comparative Example 1;
[0041] Fig. 9This is a SEM image of the corrosion morphology of the titanium substrate in Comparative Example 2;
[0042] Fig.10 This is a SEM image of the catalyst coating on the surface of the titanium substrate in Comparative Example 2. DETAILED DESCRIPTION
[0043] In order to better explain the present invention and facilitate understanding, the present invention is described in detail below through specific implementation modes in conjunction with the accompanying drawings.
[0044] The embodiments of the present invention provide a titanium substrate, an electrode containing the same, and a preparation method thereof, which are aimed at the technical problems that the poor performance of the titanium substrate leads to low electrode performance, and the long substrate pretreatment time leads to low electrode production efficiency in the process of producing electrodes with the titanium substrate; wherein the grain size of the titanium substrate is 9-9.5, and the grain size is high; the oxygen content in the titanium substrate is ≤0.03%, the nitrogen content is ≤0.009%, and the hydrogen content is ≤0.008%. Compared with the prior art, the reduction of the O, N, and H content reduces the substrate resistance, improves the intracrystalline and intercrystalline electron conduction efficiency, and enhances the conductivity of the substrate. The conductivity of the substrate and the catalytic ability of the coating are improved at the same time, thereby reducing the potential of the chlorine evolution reaction of the chlorine evolution electrode, generally improving the electrode potential and life, and significantly improving the product qualification rate.
[0045] In order to better understand the above technical solution, exemplary embodiments of the present invention will be described in more detail below with reference to the accompanying drawings. Although exemplary embodiments of the present invention are shown in the accompanying drawings, it should be understood that the present invention can be implemented in various forms and should not be limited by the embodiments described herein. On the contrary, these embodiments are provided to enable a clearer and more thorough understanding of the present invention and to fully convey the scope of the present invention to those skilled in the art.
[0046] Example 1
[0047] This embodiment provides a method for preparing a titanium substrate, comprising the following steps:
[0048] (1) Sponge titanium with a purity of ≥99.999% titanium content is melted into titanium ingots and made into titanium slabs. The titanium slabs are hot-rolled at 800°C in an inert atmosphere to form titanium coils. The titanium coils are annealed at 600°C and subjected to surface impurity removal treatment. The impurity removal treatment is mainly carried out by sandblasting, shot blasting and pickling to remove surface oil and oxides to obtain primary titanium materials.
[0049] (2) The primary titanium material is cold rolled using a twenty-roll reciprocating cold rolling mill. After six times of rolling, the titanium material is annealed in an annealing machine, during which argon gas is purged in the annealing machine. The annealing temperature is 650°C and the annealing time is 5 minutes. After cooling, the titanium material is cold rolled again using a twenty-roll reciprocating cold rolling mill. After six times of rolling, the material is rolled to the finished product thickness, and then cleaned and decontaminated to obtain a secondary titanium material.
[0050] (3) The secondary titanium material is transferred to the furnace for heat treatment. The first step-by-step heating process is to evacuate the vacuum to a degree of 10 -3 Pa, and then slowly introduce high-purity argon gas into the furnace to keep the furnace in a negative pressure state, and then heat it to 415℃ at a heating rate of 80℃ / h and keep it warm for 3h without cooling; the second step-by-step heating process is to evacuate the vacuum again to reach 10 -3 Pa, slowly introduce high-purity argon gas to keep the furnace in a negative pressure state, heat it to 700℃ at a heating rate of 30℃ / h and keep it warm for 8h; the cooling process is to turn off the heating system, cool it to 200℃ at a cooling rate of 60℃ / h, and then cool it rapidly. After surface treatment, grade 3 titanium material is obtained.
[0051] (4) Under an inert atmosphere, the grade tertiary titanium material is annealed at 650°C, kept at this temperature for 5 minutes, and then stretched and straightened to obtain a titanium substrate.
[0052] The head and tail of the titanium substrate were sampled and tested, including the grain size, elongation after fracture, O content, N content and H content of the titanium plate, see Table 1 for details.
[0053] Example 2
[0054] This embodiment provides a method for preparing a titanium substrate, which is different from Embodiment 1 in that:
[0055] In step (1), the titanium slab is hot-rolled at 900° C. to form a titanium coil, and the titanium coil is annealed at 750° C.;
[0056] In step (2), the annealing temperature is 620°C and the annealing holding time is 10 min;
[0057] In step (3), during the first step heating process, the temperature is increased to 415°C at a heating rate of 60°C / h and kept at this temperature for 2 hours; during the second step heating process, the temperature is increased to 680°C at a heating rate of 30°C / h and kept at this temperature for 8 hours; during the cooling process, the temperature is cooled to 200°C at a cooling rate of 50°C / h.
[0058] In step (4), the grade 3 titanium material is annealed at 620° C. for 10 min;
[0059] The rest of the steps are the same.
[0060] The head and tail of the titanium substrate were sampled and tested, including the grain size, elongation after fracture, O content, N content and H content of the titanium plate, see Table 1 for details.
[0061] Example 3
[0062] This embodiment provides a method for preparing a titanium substrate, which is different from Embodiment 1 in that:
[0063] In step (2), the annealing temperature is 620° C. and the annealing holding time is 5 min;
[0064] In step (3), during the first step heating process, the temperature is raised to 415°C at a heating rate of 80°C / h and kept at that temperature for 3 hours; during the second step heating process, the temperature is raised to 720°C at a heating rate of 40°C / h and kept at that temperature for 6 hours;
[0065] In step (4), the grade 3 titanium material is annealed at 680° C. and kept at this temperature for 5 minutes;
[0066] The rest of the steps are the same.
[0067] The head and tail of the titanium substrate were sampled and tested, including the grain size, elongation after fracture, O content, N content and H content of the titanium plate, see Table 1 for details.
[0068] Example 4
[0069] This embodiment provides a method for preparing a chlorine evolution electrode, comprising the following steps:
[0070] (1) The titanium substrate prepared in Example 1 was cut into titanium meshes of fixed size, and each batch of 60 sheets was subjected to annealing heat treatment at 450°C to remove stress and keep the titanium mesh flat; each batch of 30 sheets was etched with 28% sulfuric acid at 80°C for 2.8 hours, during which the corrosion morphology of the substrate was uniformly sampled and tested. Figure 1 The surface roughness Ra of the substrate was detected by a portable roughness meter and reached 2-2.3 μm, see Table 2.
[0071] (2) The substrate treated in step (1) is washed with pure water and then dried, and a solution of ruthenium and iridium precious metal elements (catalyst solution, wherein the mass ratio of ruthenium oxide to iridium oxide is 1-5) is coated on the surface of the substrate by electrostatic spraying, and then placed in a high-temperature furnace at 400-550° C. for high-temperature sintering for 10-30 minutes, and repeated 6-10 times to coat the surface of the substrate with a catalyst coating to produce a chlorine evolution electrode, as shown in the attached Figure 2 ; and track the actual electrolysis voltage of the chlorine evolution electrode made from this batch of substrates, see Table 3.
[0072] The specific steps of applying the catalyst coating by thermal oxidation method can be found in the prior art.
[0073] Example 5
[0074] This embodiment provides a method for preparing a chlorine evolution electrode, which differs from Embodiment 4 in that:
[0075] (1) The titanium substrate prepared in Example 2 was cut into fixed sizes and subjected to high-temperature annealing heat treatment in batches of 60 sheets. The material was etched at 60° C. using 30% sulfuric acid at a mass fraction of 30% for 2.5 h. During this period, samples were taken to detect the uniform corrosion morphology of the substrate. See the attached Figure 3 The surface roughness Ra of the substrate was detected by a portable roughness meter and reached 1.8-2.1 μm, see Table 2. The other steps are the same.
[0076] The chlorine evolution electrode is shown in the attached Figure 4 ; and track the actual electrolysis voltage of the chlorine evolution electrode made from this batch of substrates, see Table 3.
[0077] Example 6
[0078] This embodiment provides a method for preparing a chlorine evolution electrode, comprising the following steps:
[0079] (1) The titanium substrate prepared in Example 3 was cut into fixed sizes and subjected to high-temperature annealing heat treatment in batches of 60 sheets. The material was etched at 95° C. using 20% mass fraction sulfuric acid in batches of 30 sheets for 3.0 h. During the etching period, samples were taken to detect the uniform corrosion morphology of the substrate. See the attached Figure 5 The surface roughness Ra of the substrate was detected by a portable roughness meter and reached 2.6-3.1 μm, see Table 2. The other steps are the same.
[0080] The chlorine evolution electrode is shown in the attached Figure 6 ; and track the actual electrolysis voltage of the chlorine evolution electrode made from this batch of substrates, see Table 3.
[0081] Comparative Example 1
[0082] This comparative example provides a method for preparing a chlorine evolution electrode, which differs from Example 1 in that:
[0083] The two-stage step-by-step heating process in step (3) is changed to: evacuate the furnace to a vacuum degree of 10-3 Pa, then slowly introduce high-purity argon gas into the furnace to maintain a negative pressure in the furnace, heat the furnace to 700°C at a heating rate of 80°C / h and keep it warm for 8h; the remaining steps are the same.
[0084] The head and tail of the titanium substrate were sampled and tested, including the grain size, elongation after fracture, O content, N content and H content of the titanium plate, see Table 1 for details.
[0085] The subsequent steps are the same as in Example 4. During this period, samples were taken to detect the uniform corrosion morphology of the substrate. Figure 7 The surface roughness Ra of the substrate was detected by a portable roughness meter and reached 1.7-3.2 μm, see Table 2. Figure 8 , and tracked the actual electrolysis voltage of the chlorine evolution electrode made from this batch of substrates, see Table 3.
[0086] Comparative Example 2
[0087] This comparative example provides a method for preparing a chlorine-evolving electrode, which differs from Example 4 in that: in step (1), 20% hydrochloric acid by mass is used to etch the material at 80°C for 2.8 hours, during which sampling is performed to detect the uniform corrosion morphology of the substrate. Fig. 9 The surface roughness Ra of the substrate was detected by a portable roughness meter and reached 2.0-2.7 μm, see Table 2.
[0088] The rest of the steps are the same. Among them, the titanium substrate head and tail are sampled for testing, including the titanium plate grain size, elongation after fracture, O content, N content, H content, see Table 1 for details; the preparation of chlorine evolution electrode is shown in the attached Fig.10 , and tracked the actual electrolysis voltage of the chlorine evolution electrode made from this batch of substrates, see Table 3.
[0089] Table 1 Physical and chemical test results of different titanium substrates
[0090]
[0091] Table 2 Test results of substrate surface roughness Ra
[0092]
[0093]
[0094] Table 3 Actual electrolysis voltage of chlorine evolution electrodes made from the same batch of titanium substrates
[0095]
[0096]
[0097]
[0098] The above examples and comparative examples are analyzed as follows:
[0099] First, according to Examples 1-3 and Table 1, it can be seen that by adopting hot rolling, cold rolling and two-stage step-by-step annealing, and then adding a step of finished product annealing, the oxygen content in the titanium substrate prepared is ≤0.03%, the nitrogen content is ≤0.009%, and the hydrogen content is ≤0.008%. The reduction of the content of O, N, and H reduces the resistance of the substrate, improves the efficiency of intracrystalline and intercrystalline electron conduction, and enhances the conductivity of the substrate. At the same time, it ensures that the rutile structure does not change when the TiO2 crystal is generated, thereby strengthening the solid solution effect of the substrate and the catalyst crystal, and can improve the life of the electrode prepared therefrom. As shown in Examples 1-3, the elongation after fracture of the titanium substrate prepared in each embodiment of the present invention is above 50%.
[0100] The grain size of the titanium substrate finally prepared in Examples 1-3 is 9-9.5. Compared with Comparative Examples 1 and 2, it can be seen that the titanium substrate prepared in Examples 1-3 has fine and uniform grains, and the formed crystal surface is more easily exchanged with hydrogen ions and rapidly corroded, and the overall corrosion rate of the substrate is faster in the subsequent etching roughening treatment.
[0101] See also Figure 1 , Figure 3 , Figure 5 , Figure 7 , Fig. 9 As shown in Table 2, compared with Comparative Examples 1 and 2, the rough surface formed after the roughening treatment in Examples 4-6 has a higher consistency. In addition, the increase in the grain size of the titanium substrate also increases the number of microstructures of the substrate after corrosion, thereby increasing the specific surface area of the electrode and the catalytic crystal nucleation sites; see Figure 2 , Figure 4 , Figure 6 , Figure 8 and Fig.10 In Examples 4-6, the catalyst is evenly distributed on the surface of the substrate finally coated with the catalyst coating. Figure 3 and Figure 5 The grain size is slightly larger after corrosion, but the consistency of the macroscopic point roughness Ra is higher, corresponding to Figure 4 and Figure 6 , the catalyst coating is also uniform.
[0102] Referring to Table 3, compared with Comparative Examples 1 and 2, the average cell voltage of the chlorine evolution electrodes finally prepared in Examples 4-6 is 2.91V, the qualified rate of the substrate for electrode production is 97-100%, the efficiency of the titanium substrate roughening treatment during electrode production is increased by 1 times (from 5h / batch to 2.5h / batch), the qualified rate of the electrode product is increased by 1.42 times (from 40% to 97%), the electrode electrolysis voltage is reduced by 20mV, and the energy consumption is reduced by 12.5kw.h / t, that is, the conductivity of the substrate and the catalytic ability of the coating are improved at the same time, thereby reducing the chlorine evolution reaction potential of the chlorine evolution electrode.
[0103] Comparative Example 2 uses hydrochloric acid material for etching, the consistency of the surface roughness Ra of the substrate is poor, and the qualified rate of the chlorine evolution electrode finally prepared is low. Fig. 9 The titanium substrate was made by the process of Example 1, so the morphology after hydrochloric acid corrosion is close to Figure 1 However, a closer look reveals that local corrosion is fast during hydrochloric acid corrosion, which leads to uneven roughness measurement and poor uniformity in catalyst coating production.
[0104] Finally, it should be noted that the above embodiments are only used to illustrate the technical solutions of the present invention, rather than to limit it. Although the present invention has been described in detail with reference to the aforementioned embodiments, those skilled in the art should understand that they can still modify the technical solutions described in the aforementioned embodiments, or replace some or all of the technical features therein with equivalents. However, these modifications or replacements do not cause the essence of the corresponding technical solutions to deviate from the scope of the technical solutions of the embodiments of the present invention.
Claims
1. A titanium substrate, characterized in that: The grain size is 9-9.5, wherein, by mass percentage, the oxygen content is ≤0.03%, the nitrogen content is ≤0.009%, and the hydrogen content is ≤0.008%.
2. An electrode, characterized in that: It comprises the titanium substrate as claimed in claim 1.
3. A method for preparing an electrode as claimed in claim 2, characterized in that: The following steps are involved: Step 1, roughening the surface of the titanium substrate: using a 20-30% by mass sulfuric acid solution at 60-95° C. for etching for 2.5±0.5 h, and then cleaning and drying the titanium substrate to obtain a titanium substrate with a roughened surface; Step 2: coating the roughened titanium substrate with a catalyst coating to produce the electrode.
4. The electrode preparation method according to claim 3, characterized in that: In step 2, the process of coating the catalyst coating is to coat the platinum group precious metal elements by thermal oxidation method.
5. A method for preparing a titanium substrate as claimed in any one of claims 1 to 4, characterized in that: The following steps are involved: S1. Hot rolling: hot rolling and annealing the titanium slab in sequence to obtain primary titanium material; S2, cold rolling: cold rolling and cleaning the primary titanium material to obtain the secondary titanium material; S3, step annealing: in an inert atmosphere and negative pressure, the second-grade titanium material is subjected to two-stage step-wise annealing, and then surface treated to obtain the third-grade titanium material; S4, finished product annealing: anneal the grade 3 titanium material, and then obtain the titanium base material by stretching and straightening.
6. The method for preparing a titanium substrate according to claim 5, characterized in that: In S1, the titanium slab is made of titanium ingots melted from titanium sponge with a purity of ≥99.999% titanium content, and the hot rolling temperature is 800-900°C in an inert atmosphere, and the thickness of the final primary titanium material is 4-100mm; The annealing process is carried out in an inert atmosphere at 600-750°C for 5-10 minutes, and surface impurities are removed after cooling.
7. The method for preparing a titanium substrate according to claim 5, characterized in that: In S2, the cold rolling process is as follows: after rolling the primary titanium material, annealing treatment is performed: in an inert atmosphere, the temperature is maintained at 620-680°C for 5-10 minutes, and after cooling, rolling is performed again to roll the primary titanium material to a thickness that meets the requirements of the finished product; In S4, the annealing process is to keep the temperature at 620-680° C. for 5-10 minutes in an inert gas atmosphere.
8. The method for preparing a titanium substrate according to claim 5, characterized in that: In S3, the first stage of the step-by-step temperature increase process is: in an inert gas atmosphere, maintaining a negative pressure environment, heating to 400-430°C at a heating rate of 60-80°C / h, and keeping warm for 2-3h. The second stage of step-by-step heating process is as follows: based on the first stage of step-by-step heating annealing, in an inert gas atmosphere, maintaining a negative pressure environment, continuing to heat up to 680-720°C at a heating rate of 30-40°C / h, and keeping warm for 6-8h.
9. The method for preparing a titanium substrate according to claim 8, characterized in that: In S3, after the second stage of stepwise heating, the secondary titanium material is cooled to 200°C at a cooling rate of 50-60°C / h, and then rapidly cooled.
10. The method for preparing a titanium substrate according to claim 8, characterized in that: In S3, the vacuum degree of the negative pressure environment in the two-stage step-by-step heating is on the order of 10 -3 Pa.