A carburized bearing steel and a preparation method thereof
Through dual vacuum process and multi-stage vacuum heat treatment, the problem of carbide growth and grain size control of M50NiL bearing steel under high temperature conditions is solved, the fracture toughness and fatigue life of bearing steel are improved, and high surface hardness and crack resistance are achieved. effect.
Patent Information
- Application Number
- CN202211017631.5
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2022-08-23
- Publication Date
- 2024-11-12
- Estimated Expiration
- 2042-08-23
AI Technical Summary
M50NiL bearing steel is difficult to control the growth of carbides under high temperature conditions, especially to avoid the formation of mesh carbides during carburizing. The thermal processing and heat treatment process are long, and the grain size is difficult to control, resulting in fracture toughness and fatigue life. insufficient.
The bearing steel is prepared by double vacuum process, forging and high-temperature vacuum carburizing heat treatment, combined with multi-stage vacuum heat treatment, including vacuum austenitization, oil quenching, tempering and deep cooling treatment, control the grain size and carburizing layer thickness, and improve the The fracture toughness and crack propagation of the material.
Through appropriate high-temperature carburizing process and multi-stage vacuum heat treatment, the surface hardness and crack resistance of the material are improved, the fatigue life is extended, and the high-temperature use requirements of aviation bearings are met.
Smart Images

Figure CN115449613B_ABST
Abstract
Description
Technical Field
[0001] The invention belongs to the field of heat treatment, and in particular relates to carburized bearing steel and a preparation method thereof. Background Art
[0002] At present, the commonly used bearing steels at home and abroad are GCr15, M50, M50NiL and CSS-42L. Among them, GCr15 has a low working temperature, often below 150°C. M50 has poor fracture toughness and is prone to fatigue cracks. M50NiL and CSS-42L have high working temperatures and can maintain stable hardness and good toughness at 350°C, so they are widely used in the manufacture of aircraft engine bearings.
[0003] M50NiL was successfully developed in the 1980s. Its fatigue life is about twice that of M50 steel. Due to its excellent fracture toughness and hardness, it gradually replaces M50 steel for the production of bearings of key engine components. At present, the research hotspots of this material at home and abroad are mainly divided into two categories. One is the study of its failure mechanism, and the other is the study of its surface treatment process, including surface carburizing treatment and the influence of various complex heat treatment operations on its performance. After carburizing and multi-stage heat treatment, M50NiL can not only ensure the hardness and fatigue strength at high temperature, but also avoid the generation of cracks. However, how to control the growth of its carbides, especially to avoid the formation of network carbides during carburizing, is crucial to its application. At the same time, the hot processing and heat treatment process of M50NiL is long, the temperature is high, and the grain size is difficult to control. Summary of the invention
[0004] In view of the above problems, the present invention provides the following solutions:
[0005] In one aspect, the present invention provides a method for preparing carburized bearing steel, comprising:
[0006] The bearing steel ingot is prepared according to the double vacuum process and forged to obtain fine-grained carburized bearing steel;
[0007] Carburizing fine-grained bearing steel by high-temperature vacuum carburizing heat treatment to obtain carburized bearing steel with a carburized layer thickness;
[0008] Carburized bearing steel having a carburized layer thickness is subjected to multi-stage vacuum heat treatment to obtain carburized bearing steel.
[0009] Further, the forging process includes:
[0010] Before forging, the bearing steel ingot is heated to 1150℃-1180℃ in a heating furnace and kept warm for 3h-3.5h;
[0011] A three-upsetting and three-drawing process is performed, wherein each upsetting deformation is greater than 60%, the drawing deformation is greater than 70%, the initial forging temperature is ≥1100°C, and the final forging temperature is ≥980°C.
[0012] Furthermore, the high temperature vacuum carburizing heat treatment comprises:
[0013] Carburize the fine-grained carburized bearing steel in a high-temperature vacuum environment for 8 hours;
[0014] After carburizing, keep at 850℃-900℃ for 2h and then oil quench.
[0015] Furthermore, the high temperature vacuum environment is 1100°C-1150°C, the number of pulses is 10, the diffusion ratio is 1:20, and the acetylene pressure is 2500Pa.
[0016] Furthermore, the multi-stage vacuum heat treatment includes:
[0017] The primary heat treatment system is vacuum austenitization followed by oil quenching, followed by vacuum tempering and cryogenic treatment, wherein the vacuum tempering temperature is 500°C-550°C and the time is 1.5h-2h;
[0018] The secondary heat treatment system is vacuum oil quenching, followed by vacuum tempering and deep cryogenic treatment, wherein the vacuum tempering temperature is 550°C-580°C and the time is 1h-1.5h;
[0019] The three-stage heat treatment system is vacuum oil quenching, followed by vacuum tempering treatment, the vacuum tempering temperature is 580℃-600℃, and the time is 1.5h-2h;
[0020] The fourth-level heat treatment system is vacuum oil quenching, followed by vacuum tempering, wherein the vacuum tempering temperature is 500°C-550°C, and the time is 1h-1.5h;
[0021] The five-stage heat treatment system is vacuum oil quenching followed by vacuum tempering, wherein the vacuum tempering temperature is 500° C.-550° C. and the time is 1 h-1.5 h.
[0022] Furthermore, the cryogenic treatment temperature is minus 80°C to 100°C, and the time is 2h to 2.5h.
[0023] Furthermore, the primary heat treatment temperature is 1150°C-1180°C, and the time is 1h-1.5h.
[0024] Furthermore, the secondary heat treatment temperature is 1100°C-1150°C, and the time is 2h-2.5h.
[0025] Furthermore, the temperature of the third-stage heat treatment is 950°C-1000°C, and the time is 0.5h-0.6h.
[0026] Furthermore, the temperature of the fourth stage heat treatment is 850°C-900°C, and the time is 2h-2.5h.
[0027] Furthermore, the five-stage heat treatment temperature is 750°C-800°C and the time is 3h-3.5h.
[0028] On the other hand, a carburized bearing steel is characterized in that the carburized bearing steel is recorded in percentage by weight as follows: C: 0.12-0.15, Mo: 4.00-4.50, Cr: 4.00-4.25, V: 1.13-1.33, Ni: 3.20-3.60, Mn: 0.15-0.35, Si: 0.10-0.25, and the remainder is iron and impurity elements.
[0029] Furthermore, the carburized bearing steel Ac1=745°C, Ac3=930°C.
[0030] The present invention improves the grain size and the fracture toughness of the material by providing a suitable high-temperature carburizing process, multi-stage vacuum heat treatment and other means, thereby obtaining an aviation bearing steel with high surface hardness, crack propagation resistance and high fatigue life.
[0031] Other features and advantages of the present invention will be described in the following description, and partly become apparent from the description, or understood by practicing the present invention. The purpose and other advantages of the present invention can be realized and obtained by the structures pointed out in the description, claims and drawings. BRIEF DESCRIPTION OF THE DRAWINGS
[0032] In order to more clearly illustrate the embodiments of the present invention or the technical solutions in the prior art, the following briefly introduces the drawings required for use in the embodiments or the description of the prior art. Obviously, the drawings described below are some embodiments of the present invention. For ordinary technicians in this field, other drawings can be obtained based on these drawings without paying creative work.
[0033] Figure 1 A preparation flow chart of carburized bearing steel according to an embodiment of the present invention is shown. DETAILED DESCRIPTION
[0034] In order to make the purpose, technical solution and advantages of the embodiments of the present invention clearer, the technical solution in the embodiments of the present invention will be clearly and completely described below in conjunction with the drawings in the embodiments of the present invention. Obviously, the described embodiments are part of the embodiments of the present invention, not all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.
[0035] like Figure 1 As shown, the preparation method of carburized bearing steel includes preparing the carburized bearing steel according to a conventional double vacuum process, forging to obtain fine-grained carburized bearing steel; subjecting the fine-grained carburized bearing steel to high-temperature vacuum carburizing heat treatment to obtain carburized bearing steel with a carburized layer thickness; subjecting the carburized bearing steel with a carburized layer thickness to multi-stage vacuum heat treatment to obtain carburized bearing steel.
[0036] The carburized bearing steel is prepared according to the conventional double vacuum process and forged. In order to strictly control the grain size, the multi-pass forging temperature and deformation can be appropriately adjusted. Before forging, the steel ingot is placed in a heating furnace, heated to 1150°C-1180°C, and kept warm for 3h-3.5h. Then, a three-upsetting and three-drawing process is performed, with each upsetting deformation of more than 60%, and the drawing deformation of more than 70%, the initial forging temperature ≥1100°C, and the final forging temperature ≥980°C. After the forging is slowly cooled, annealing is performed.
[0037] Among them, the high temperature vacuum carburizing heat treatment has a temperature of 1100-1150℃, a time of 8h, a pulse number of 10, a diffusion ratio of 1:20, and an acetylene pressure of 2500Pa. After carburizing, it is kept at 850-900℃ for 2h and then oil quenched. The effective carburized layer thickness can reach more than 3mm, and the surface hardness of the carburized layer is more than 75HRC. In addition, the carburized layer thickness can be adjusted by adjusting the carburizing time.
[0038] Among them, multi-stage vacuum heat treatment generally carries out four or five stages of heat treatment to control the grain size. The first stage heat treatment system is vacuum austenitizing followed by oil quenching, the temperature is 1150℃-1180℃, the time is 1h-1.5h, and then vacuum tempering is carried out, the temperature is 500℃-550℃, the time is 1.5h-2h, and the deep cryogenic treatment temperature is minus 80℃-100℃, the time is 2h-2.5h. After complete austenitization, the elements are fully diffused for a long time to achieve uniformity of the edge and core structure, improve the toughness of the core, and also make the transition of the edge carburized layer smooth, so as not to cause a sudden change in hardness, thereby improving fatigue life; the second stage heat treatment system is vacuum oil quenching, the temperature is 1100℃-1150℃, the time is 2h-2.5h, and then vacuum tempering is carried out, the temperature is 550℃-580℃, the time is 1h-1.5h, and the deep cryogenic treatment temperature is minus 80℃-100℃, the time is 2h-2.5h. 80℃-100℃, time is 2h-2.5h; the third-level heat treatment system is vacuum oil quenching, temperature is 950℃-1000℃, time is 0.5h-0.6h, and then vacuum tempering is 580℃-600℃, time is 1.5h-2h; the fourth-level heat treatment system is vacuum oil quenching, temperature is 850-900℃, time is 2h-2.5h, and then vacuum tempering is 500℃-550℃, time is 1h-1.5h. It is more preferred to carry out the fifth-level heat treatment system of vacuum oil quenching, temperature is 750℃-800℃, time is 3h-3.5h, and then vacuum tempering, and the tempering temperature and time are the same as the fourth-level heat treatment system. Through multi-stage heat treatment, the grain size can be controlled at about level 8, and the fracture toughness of the core is 65MPa.m 1 / 2 , meeting the usage requirements.
[0039] It should be noted that the carburized bearing steel prepared by the above preparation method is recorded as follows by weight percentage: C: 0.12-0.15, Mo: 4.00-4.50, Cr: 4.00-4.25, V: 1.13-1.33, Ni: 3.20-3.60, Mn: 0.15-0.35, Si: 0.10-0.25, and the remainder is iron and impurity elements. The carburized bearing steel Ac1 = 745 ° C and Ac3 = 930 ° C were measured by a phase change instrument.
[0040] Among them, Ac1 is the temperature at which austenite begins to form when the steel is heated, and Ac3 is the temperature at which all ferrite is transformed into austenite when the hypoeutectoid steel is heated.
[0041] Embodiment 1:
[0042] The carburized bearing steel is prepared according to the conventional double vacuum process and forged. In order to strictly control the grain size, the multi-pass forging temperature and deformation are appropriately adjusted. Before forging, the steel ingot is placed in a heating furnace, heated to 1175°C, and kept warm for about 3 hours. A three-upsetting and three-drawing process is performed, with each upsetting deformation of 65% and the drawing deformation of 75%. The initial forging temperature is 1123°C and the final forging temperature is 995°C. After the forging is slowly cooled, annealing is performed.
[0043] Carry out high temperature vacuum carburizing heat treatment. The temperature is 1145℃, the time is 8h, the number of pulses is 10, the expansion ratio is 1:20, and the acetylene pressure is 2500Pa. After carburizing, keep it at 875℃ for 2h and then oil quench. The effective carburized layer thickness can reach 3.2mm, and the surface hardness of the carburized layer is 78HRC.
[0044] Multi-stage vacuum heat treatment is carried out, and four or five-stage heat treatment is carried out to control the grain size. The first-stage heat treatment system is vacuum austenitization followed by oil quenching at a temperature of 1175°C for 1.2 hours, followed by vacuum tempering at a temperature of 530°C for 1.6 hours, and deep cryogenic treatment at a temperature of -85°C for 2 hours. After complete austenitization, the elements are fully diffused for a long time to achieve uniformity of the edge and core structures, improve the toughness of the core, and make the transition of the edge carburized layer smooth, so as not to cause a sudden change in hardness, thereby improving fatigue life; the secondary heat treatment system is vacuum oil quenching, the temperature is 1145℃, the time is 2.2h, and then vacuum tempering is performed at a temperature of 555℃, the time is about 1h, and the deep cold treatment temperature is minus 85℃, the time is about 2h; the third-level heat treatment system is vacuum oil quenching, the temperature is 980℃, the time is 0.5h, and then vacuum tempering is performed at 590℃, the time is 1.7h; the fourth-level heat treatment system is vacuum oil quenching, the temperature is 860℃, the time is about 2h, and then vacuum tempering is performed at 545℃. It is more preferred to perform a fifth-level heat treatment system of vacuum oil quenching, the temperature is 780℃, the time is 3.2h, and then vacuum tempering is performed, and the tempering temperature and time are the same as the fourth-level heat treatment system. Through multi-stage heat treatment, the grain size can be controlled to 8.5 level, and the core fracture toughness is 68MPa.m 1 / 2 , meeting the usage requirements.
[0045] The composition of the high temperature carburized bearing steel is recorded as C: 0.13, Mo: 4.23, Cr: 4.19, V: 1.19, Ni: 3.45, Mn: 0.23, Si: 0.22, and the balance is iron and inevitable impurity elements. The temperature of the aviation bearing steel Ac1 = 745 ° C and Ac3 = 930 ° C was measured by a phase change instrument.
[0046] Embodiment 2:
[0047] The carburized bearing steel is prepared according to the conventional double vacuum process and forged. In order to strictly control the grain size, the multi-pass forging temperature and deformation are appropriately adjusted. Before forging, the steel ingot is placed in a heating furnace, heated to 1175°C, and kept warm for 3 hours. A three-upsetting and three-drawing process is performed, with each upsetting deformation of 66% and the drawing deformation of 72%. The initial forging temperature is 1120°C and the final forging temperature is 982°C. After the forging is slowly cooled, annealing is performed.
[0048] Carry out high temperature vacuum carburizing heat treatment. The temperature is 1145℃, the time is 8.5h, the number of pulses is 12, the expansion ratio is 1:20, and the acetylene pressure is 2500Pa. After carburizing, keep it at 880℃ for 2h and then oil quench. The effective carburizing layer thickness can reach 3.5mm, and the surface hardness of the carburizing layer is above 75HRC. In addition, the carburizing layer thickness can be adjusted by adjusting the carburizing time.
[0049] Multi-stage vacuum heat treatment is carried out, and four or five-stage heat treatment is carried out to control the grain size. The first-stage heat treatment system is vacuum austenitization followed by oil quenching at a temperature of 1175°C for 1.3 hours, followed by vacuum tempering at a temperature of 540°C for 1.8 hours, and deep cryogenic treatment at a temperature of -95°C for about 2 hours. After complete austenitization, the elements are fully diffused for a long time to achieve uniformity of the edge and core structure, improve the toughness of the core, and make the transition of the edge carburized layer smooth, so as not to cause a sudden change in hardness, thereby improving fatigue life; the secondary heat treatment system is vacuum oil quenching, the temperature is 1145℃, the time is 2.2h, and then vacuum tempering is performed at a temperature of 560℃, the time is about 1h, and the deep cold treatment temperature is minus 90℃, the time is about 2h; the third-level heat treatment system is vacuum oil quenching, the temperature is 975℃, the time is 0.5h, and then vacuum tempering is performed at 585℃, the time is 1.7h; the fourth-level heat treatment system is vacuum oil quenching, the temperature is 875℃, the time is about 2h, and then vacuum tempering is performed at 545℃. It is more preferred to perform a fifth-level heat treatment system of vacuum oil quenching, the temperature is 760℃, the time is 3.4h, and then vacuum tempering, and the tempering temperature and time are the same as the fourth-level heat treatment system. Through multi-stage heat treatment, the grain size can be controlled to about 9 levels, and the core fracture toughness is 69MPa.m 1 / 2 , meeting the usage requirements.
[0050] The composition of the high temperature carburized bearing steel is recorded as C: 0.15, Mo: 4.35, Cr: 4.15, V: 1.19, Ni: 3.35, Mn: 0.23, Si: 0.21, and the balance is iron and inevitable impurity elements. The temperature of the aviation bearing steel Ac1 = 745 ° C and Ac3 = 930 ° C was measured by a phase change instrument.
[0051] Embodiment 3:
[0052] The carburized bearing steel is prepared according to the conventional double vacuum process and forged. In order to strictly control the grain size, the multi-pass forging temperature and deformation are appropriately adjusted. Before forging, the steel ingot is placed in a heating furnace, heated to 1165°C, and kept warm for 3 hours. A three-upsetting and three-drawing process is performed, with each upsetting deformation of 70% and the drawing deformation of 75%. The initial forging temperature is 1125°C and the final forging temperature is 990°C. After the forging is slowly cooled, annealing is performed.
[0053] Carry out high temperature vacuum carburizing heat treatment. The temperature is 1145℃, the time is 9.5h, the number of pulses is 15, the expansion ratio is 1:22, and the acetylene pressure is 2500Pa. After carburizing, keep it at 880℃ for 2h and then oil quench. The effective carburized layer thickness can reach 3.8mm, and the surface hardness of the carburized layer is 79HRC.
[0054] Multi-stage vacuum heat treatment is carried out, and four or five-stage heat treatment is carried out to control the grain size. The first-stage heat treatment system is vacuum austenitization followed by oil quenching at a temperature of 1175°C for 1.4 hours, followed by vacuum tempering at a temperature of 550°C for 1.8 hours, and deep cryogenic treatment at a temperature of -90°C for about 2 hours. After complete austenitization, the elements are fully diffused for a long time to achieve uniformity of the edge and core structures, improve the toughness of the core, and make the transition of the edge carburized layer smooth, so as not to cause a sudden change in hardness, thereby improving fatigue life; the secondary heat treatment system is vacuum oil quenching, the temperature is 1145℃, the time is 2.4h, and then vacuum tempering is performed at a temperature of 580℃, the time is about 1h, and the deep cold treatment temperature is minus 90℃, the time is about 2h; the third-level heat treatment system is vacuum oil quenching, the temperature is 975℃, the time is 0.5h, and then vacuum tempering is performed at 590℃, the time is 1.8h; the fourth-level heat treatment system is vacuum oil quenching, the temperature is 860℃, the time is about 2h, and then vacuum tempering is performed at 570℃. It is more preferred to perform a fifth-level heat treatment system of vacuum oil quenching, the temperature is 780℃, the time is 3.6h, and then vacuum tempering is performed, and the tempering temperature and time are the same as the fourth-level heat treatment system. Through multi-stage heat treatment, the grain size can be controlled to level 9, and the core fracture toughness is 70MPa.m 1 / 2 , meeting the usage requirements.
[0055] The composition of the high temperature carburized bearing steel is recorded as C: 0.14, Mo: 4.23, Cr: 4.15, V: 1.21, Ni: 3.25, Mn: 0.18, Si: 0.15, and the balance is iron and inevitable impurity elements. The temperature of the aviation bearing steel Ac1 = 745 ° C and Ac3 = 930 ° C was measured by a phase change instrument.
[0056] The aviation bearing steel produced by the present invention has a surface hardness of more than 70HRC, a carburized layer thickness of more than 3mm, a grain size of 8, and a core fracture toughness of 65MPa.m 1 / 2Not only does it have high surface hardness, it also effectively prevents cracks from spreading and extends its service life.
[0057] It should be noted that the terms "first", "second" etc. in the present application are used to distinguish similar objects, and are not necessarily used to describe a specific order or sequential order. It should be understood that the data used in this way can be interchanged in appropriate circumstances, so that the embodiments of the present application described here. In the present application, the orientation or positional relationship indicated by the terms "upper", "lower", "left", "right", "front", "back", "top", "bottom", "inside", "outside", "middle", "vertical", "horizontal", "lateral", "longitudinal" etc. are based on the orientation or positional relationship shown in the accompanying drawings.
[0058] Although the present invention has been described in detail with reference to the aforementioned embodiments, those skilled in the art should understand that they can still modify the technical solutions described in the aforementioned embodiments, or make equivalent substitutions for some of the technical features therein; and these modifications or substitutions do not make the essence of the corresponding technical solutions deviate from the spirit and scope of the technical solutions of the embodiments of the present invention.
Claims
1. A method for preparing carburized bearing steel, comprising: The bearing steel ingot is prepared according to the double vacuum process and forged to obtain fine-grained carburized bearing steel; Carburizing fine-grained bearing steel by high-temperature vacuum carburizing heat treatment to obtain carburized bearing steel with a carburized layer thickness; Carburized bearing steel having a carburized layer thickness is subjected to multi-stage vacuum heat treatment to obtain carburized bearing steel; The forging process includes: before forging, the bearing steel ingot is heated to 1150℃-1180℃ in a heating furnace and kept warm for 3h-3.5h; three-upsetting and three-drawing processes are performed, wherein the upsetting deformation is greater than 60% each time, the drawing deformation is greater than 70%, the initial forging temperature is ≥1100℃, and the final forging temperature is ≥980℃; High temperature vacuum carburizing heat treatment includes: Carburizing the fine-grained carburized bearing steel in a high-temperature vacuum environment for 8 hours; after carburizing, the steel is kept at 850°C-900°C for 2 hours and then oil quenched; the temperature of the high-temperature vacuum environment is 1100°C-1150°C, the number of pulses is 10, the expansion ratio is 1:20, and the acetylene pressure is 2500Pa; Multi-stage vacuum heat treatment includes: The primary heat treatment system is vacuum austenitization followed by oil quenching, followed by vacuum tempering and cryogenic treatment, wherein the temperature of the primary heat treatment is 1150°C-1180°C; the vacuum tempering temperature is 500°C-550°C, and the time is 1.5h-2h; the cryogenic treatment temperature is minus 80°C-minus 100°C; The secondary heat treatment system is vacuum oil quenching, followed by vacuum tempering and cryogenic treatment, wherein the temperature of the secondary heat treatment is 1100°C-1150°C; the vacuum tempering temperature is 550°C-580°C, and the time is 1h-1.5h; the temperature of the cryogenic treatment is minus 80°C-minus 100°C; The three-stage heat treatment system is vacuum oil quenching, followed by vacuum tempering treatment, the temperature of the three-stage heat treatment is 950°C-1000°C; the vacuum tempering temperature is 580°C-600°C, and the time is 1.5h-2h; The four-stage heat treatment system is vacuum oil quenching, followed by vacuum tempering treatment, wherein the temperature of the four-stage heat treatment is 850°C-900°C; the vacuum tempering temperature is 500°C-550°C, and the time is 1h-1.5h; The five-stage heat treatment system is vacuum oil quenching followed by vacuum tempering treatment, wherein the temperature of the five-stage heat treatment is 750°C-800°C, the vacuum tempering temperature is 500°C-550°C, and the time is 1h-1.5h.
2. A method for preparing carburized bearing steel according to claim 1, wherein: The time of the deep freezing treatment is 2h-2.5h.
3. The method for preparing carburized bearing steel according to claim 1, wherein: The time of the primary heat treatment is 1h-1.5h.
4. The method for preparing carburized bearing steel according to claim 1, wherein: The time of the secondary heat treatment is 2h-2.5h.
5. The method for preparing carburized bearing steel according to claim 1, wherein: The time of the three-stage heat treatment is 0.5h-0.6h.
6. The method for preparing carburized bearing steel according to claim 1, wherein: The time of the four-stage heat treatment is 2h-2.5h.
7. The method for preparing carburized bearing steel according to claim 1, wherein: The time of the five-stage heat treatment is 3h-3.5h.
8. A carburized bearing steel, prepared by the preparation method according to any one of claims 1 to 7, characterized in that: The carburized bearing steel comprises, by weight percentage: C: 0.12-0.15, Mo: 4.00-4.50, Cr: 4.00-4.25, V: 1.13-1.33, Ni: 3.20-3.60, Mn: 0.15-0.35, Si: 0.10-0.25, and the remainder is iron and impurity elements. 9 . The carburized bearing steel according to claim 8 , wherein the carburized bearing steel Ac1=745° C., Ac3=930° C.