Preparation method of broadband optical limiter based on gallium nitride nanowires

By growing on conductive carbon paper and peeling off gallium nitride nanowires using pyrolytic tape, an efficient gallium nitride nanowire photolimiting device was prepared, which solved the problem of high transmittance of ultraviolet light limiting materials in the prior art. , achieving high-efficiency optical limiting performance and low-cost production in the deep ultraviolet to near-infrared range.

CN118938564APending Publication Date: 2024-11-12DONGGUAN UNIV OF TECH
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202410988420.9
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-07-23
Publication Date
2024-11-12

AI Technical Summary

Technical Problem

The existing ultraviolet limiting materials have high transmittance under ultraviolet lasers, and cannot effectively limit the light from the ultraviolet to the wide band of near-infrared light, resulting in limited applications in the fields of inspection and detection, spectral analysis, and laser weapons.

Method used

Using a broadband optical-limiting device preparation method based on gallium nitride nanowires, high concentration gallium nitride nanowires are prepared by using catalysts on conductive carbon paper, and using pyrolytic tape peeling and spin coating technology. Line dispersion or anhydrous optical limiting device, covering and glueing the edges to achieve interlayer design.

Benefits of technology

It achieves high-efficiency optical limiting performance in the wavelength range of deep ultraviolet 266nm to near infrared 1064nm, especially in the ultraviolet band, which reduces material costs and the presence of impurities and impurities, and improves the purity and stability of the sample. Sex, suitable for a variety of occasions.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118938564A_ABST
    Figure CN118938564A_ABST
Patent Text Reader

Abstract

The invention discloses a preparation method of a broadband optical limiter based on gallium nitride nanowires, which utilizes conductive carbon paper to grow the gallium nitride nanowires, and arranges a catalyst on the conductive carbon paper, so that the use of the catalyst can be saved, and the preparation cost is further reduced. According to the preparation method, large-area transfer of the heat-release adhesive tape is combined with growth on the conductive carbon paper, the preparation method is simple, the usage amount of a catalyst is small, the cost is low, batch preparation can be achieved, the gallium nitride nanowire growing on the carbon paper is stripped through the heat-release adhesive tape, the pure gallium nitride nanowire is obtained, application of the gallium nitride nanowire is expanded, and the preparation method is suitable for industrial production. The invention proves that the gallium nitride nanowire can be used for preparing an ultraviolet-visible-near infrared band broadband optical limiter, and compared with a common ultrasonic stripping method, the heat release adhesive tape stripping method has the advantages that impurities such as carbon paper and a catalyst are reduced, the purity of a prepared sample is high, the integrity of the nanowire can be protected, and the service life of the nanowire is prolonged. And the damage and fracture degree of the nanowire is reduced.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention relates to the technical field of preparing optical limiting devices, and more specifically, to a method for preparing a broadband optical limiting device based on gallium nitride nanowires. Background Art

[0002] People have conducted in-depth research on the nonlinear optical effects of inorganic semiconductors, conjugated organic polymers, inorganic metal cluster compounds, carbon nanomaterials and two-dimensional materials. The results show that their optical limiting wavelengths are in the visible light to near outer red band. Ultraviolet lasers have the characteristics of large photon energy and high resolution. They are increasingly widely used in fine processing, inspection and testing, medicine, atmospheric detection, scientific research, etc. However, the development of ultraviolet band optical limiting technology faces very few materials. Common ultraviolet limiting materials include silicon dioxide, diamond, gallium nitride crystals, etc., which have the disadvantage of high light intensity transmittance. For example, the normalized transmittance of gallium nitride crystals under 390nm ultraviolet lasers is 99.88% (Applied Physics Letters, 2000, 76, 439), and the normalized transmittance of diamond under 310nm ultraviolet lasers is 42.9% (Optics letters, 1991, 16, 499). At the same time, the application of multi-wavelength lasers with a wide spectrum from ultraviolet to near-infrared is increasing in inspection and testing, spectral analysis, and laser weapons. Optical limiting devices with a wide spectral range from ultraviolet to visible light are in urgent need of preparation and research. Summary of the invention

[0003] The purpose of the present invention is to overcome the above-mentioned defects in the prior art and provide a method for preparing a broadband optical limiting device based on gallium nitride nanowires.

[0004] To achieve the above object, the present invention provides a method for preparing a broadband optical limiting device based on gallium nitride nanowires, comprising the following steps:

[0005] Step 1: Perform ultrasonic cleaning on the conductive carbon paper for multiple times, and dry the conductive carbon paper after cleaning;

[0006] Step 2: arranging a catalyst for preparing gallium nitride nanowires on a dried conductive carbon paper;

[0007] Step 3: Using gallium oxide as a gallium source and ammonia as a nitrogen source, a chemical vapor deposition method is used in a high-temperature tube furnace to grow gallium nitride nanowires on a conductive carbon paper with a catalyst arranged on the surface;

[0008] Step 4: Take out the conductive carbon paper from the high-temperature tube furnace, adhere the thermal release tape to the surface of the conductive carbon paper with the gallium nitride nanowires grown, and evenly peel off the thermal release tape with the gallium nitride nanowires from the conductive carbon paper completely;

[0009] Step 5: The side of the thermal release tape with the GaN nanowires is tightly attached to the quartz plate, and then the quartz plate and the thermal release tape are heated as a whole, so that the thermal release tape foams and loses its stickiness, and the GaN nanowires are separated from the thermal release tape and fall on the quartz plate;

[0010] Step 6: Place the quartz sheet with the GaN nanowires attached in a beaker filled with deionized water, rinse it several times, and take out the quartz sheet to obtain a GaN nanowire dispersion;

[0011] Step 7: Heat the beaker to evaporate part of the water to obtain a high concentration of gallium nitride nanowire dispersion;

[0012] Step 8: The obtained high-concentration gallium nitride nanowire dispersion is sealed in a light-transmitting container to produce a gallium nitride nanowire optical limiting device;

[0013] Alternatively, the obtained high-concentration gallium nitride nanowire dispersion is spin-coated on a light-transmitting substrate, and the water is evaporated to obtain a water-free gallium nitride nanowire optical limiting device;

[0014] Alternatively, the obtained high-concentration gallium nitride nanowire dispersion is spin-coated on a light-transmitting substrate, and after the water is evaporated, the edges are covered and glued to prepare a gallium nitride nanowire sandwich optical limiting device.

[0015] Preferably, when growing gallium nitride nanowires on conductive carbon paper by chemical vapor deposition in step three, first place a ceramic boat containing gallium oxide powder in the middle position of a high-temperature tubular furnace quartz tube, place a conductive carbon paper with a catalyst arranged on the surface in the downstream position of the airflow in the high-temperature tubular furnace quartz tube, and then seal the high-temperature tubular furnace quartz tube, evacuate the high-temperature tubular furnace quartz tube, and then fill argon into the high-temperature tubular furnace quartz tube after evacuation until it reaches normal pressure, heat the high-temperature tubular furnace, and continuously introduce 150 sccm of nitrogen for protection during the heating process. After the temperature of the high-temperature tubular furnace is raised to 1200 degrees, stop the input of nitrogen, and instead introduce 100 sccm of ammonia, and keep the system at 1200 degrees for 45 minutes to allow gallium oxide and ammonia to react and grow on the conductive carbon paper. After the insulation is completed, stop the introduction of ammonia, and instead introduce 150 sccm of nitrogen, and let the system cool to room temperature under continuous protection of nitrogen.

[0016] Preferably, before performing step 1, the conductive carbon paper is cut into a shape of appropriate size.

[0017] Preferably, when ultrasonically cleaning the conductive carbon paper in step 1, acetone, ethanol, deionized water, and dilute hydrochloric acid are used to ultrasonically clean the conductive carbon paper in sequence, and then the conductive carbon paper is rinsed and ultrasonically cleaned again with deionized water to remove residual chemicals.

[0018] Preferably, the catalyst in step 2 is set to be metallic copper, metallic gold or nickel nitrate solution.

[0019] Preferably, in step 2, the catalyst is arranged on the conductive carbon paper by deposition, coating or infiltration.

[0020] Preferably, the high temperature tube furnace is configured as a single temperature zone horizontal high temperature tube furnace.

[0021] Preferably, when heating the quartz sheet and the thermal release tape in step five, the heating table is first heated to 120 degrees, and then the thermal release tape and the quartz sheet are placed on the heating table as a whole and heated for 5 minutes.

[0022] Preferably, the light-transmitting substrate is configured as a transparent quartz substrate or a sapphire substrate, and the light-transmitting container is configured as a transparent quartz container.

[0023] Compared with the prior art, the present invention has the following beneficial effects:

[0024] 1. The preparation process of the present invention is simple and convenient. The preparation raw materials are gallium oxide and ammonia, which are low in cost and require very little catalyst. The preparation process is simple and convenient for mass production. The catalyst is arranged on the conductive carbon paper for growth, which can save the use of the catalyst and further reduce the preparation cost. The present invention combines large-area transfer of the thermal release tape with growth on the conductive carbon paper. The preparation method is simple, the amount of catalyst used is small, the cost is low, and batch preparation is possible. The gallium nitride nanowires grown on the carbon paper are stripped by the thermal release tape to obtain pure gallium nitride nanowires, remove the carbon paper and the catalyst, and expand the application of the gallium nitride nanowires. The present invention proves that it can be used to prepare gallium nitride optical limiting devices. Compared with the commonly used ultrasonic stripping method, the thermal release tape stripping method of the present invention reduces impurities such as carbon paper and catalyst, prepares samples with high purity, and can protect the integrity of the nanowires, reducing the degree of damage and breakage of the nanowires.

[0025] 2. The gallium nitride nanowires of the present invention are prepared at high temperature, have good physical and chemical stability, are resistant to high temperatures, have good thermal conductivity, and have a high damage threshold. The optical limiting device based on this material can be used in the form of a dispersion or adsorbed on a substrate in an anhydrous form and is suitable for a variety of occasions. The nanowires prepared by this preparation method have good crystallinity, a large aspect ratio, and good diameter uniformity, so the prepared optical limiting device has stable and excellent performance.

[0026] 3. The working spectrum range of the optical limiting device prepared by this preparation method is from deep ultraviolet 266nm to near infrared 1064nm wavelength, especially in the ultraviolet band, it has good optical limiting performance, and is a nano ultraviolet light limiting device with excellent performance.

[0027] 4. The optical limiting device based on gallium nitride nanowires prepared by this preparation method has a large modulation depth and a low transmittance. The modulation depths at wavelengths of 266nm, 355nm, 532nm and 1064nm are 73.6%, 74.9%, 63.1% and 64.3%, respectively, and the corresponding minimum transmittances are 26.4%, 25.1%, 36.9% and 35.7%.

[0028] 5. The optical limiting device of the present invention covers and glues the edges, realizing the sandwich design of the optical limiting device, ensuring that the position of the gallium nitride nanowires is accurate and will not shift, the structure is stable, and the application occasions are wide. BRIEF DESCRIPTION OF THE DRAWINGS

[0029] In order to more clearly illustrate the embodiments of the present invention or the technical solutions in the prior art, the drawings required for use in the embodiments or the description of the prior art will be briefly introduced below. Obviously, the drawings described below are some embodiments of the present invention. For ordinary technicians in this field, other drawings can be obtained based on these drawings without paying creative work.

[0030] Figure 1 It is a flow chart of a method for preparing a broadband optical limiting device based on gallium nitride nanowires provided by an embodiment of the present invention;

[0031] Figure 2 is a HR-SEM image of gallium nitride nanowires grown on conductive carbon paper provided by an embodiment of the present invention;

[0032] Figure 3 is a HR-SEM image of a single gallium nitride nanowire provided by an embodiment of the present invention;

[0033] Figure 4 is the quantitative elemental analysis data of the gallium nitride nanowire composite sample provided by the embodiment of the present invention;

[0034] Figure 5 This is a low-magnification TEM image of the gallium nitride nanowires provided by an embodiment of the present invention;

[0035] Figure 6 is a high-resolution TEM image of gallium nitride nanowires provided by an embodiment of the present invention;

[0036] Figure 7 is an electron diffraction pattern of gallium nitride nanowires provided by an embodiment of the present invention;

[0037] Figure 8 is a transmission spectrum diagram of the optical limiting device provided in an embodiment of the present invention;

[0038] Fig. 9The optical limiting device provided in the embodiment of the present invention has an excitation peak power density of 10.21 GW / cm at a laser wavelength of 266 nm. 2 The Z-scan test result of the opening when (the dotted line is the experimental measurement data, and the solid line is the nonlinear absorption theory fitting curve);

[0039] Fig.10 The optical limiting device provided in the embodiment of the present invention has an excitation peak power density of 11.02 GW / cm at a laser wavelength of 355 nm. 2 The Z-scan test result of the opening when (the dotted line is the experimental measurement data, and the solid line is the nonlinear absorption theory fitting curve);

[0040] Fig.11 The optical limiting device provided in the embodiment of the present invention has an excitation peak power density of 45.07 GW / cm at a laser wavelength of 532 nm. 2 The Z-scan test result of the opening when (the dotted line is the experimental measurement data, and the solid line is the nonlinear absorption theory fitting curve);

[0041] Fig.12 The optical limiting device provided in the embodiment of the present invention has an excitation peak power density of 98.26 GW / cm at a laser wavelength of 1064 nm. 2 The Z-scan test result of the opening when (the dotted line is the experimental measurement data, and the solid line is the nonlinear absorption theory fitting curve);

[0042] Fig.13 It is a graph showing the relationship between the normalized transmittance of the optical limiting device provided by an embodiment of the present invention and the peak power density at 266nm, 355nm, 532nm and 1064nm (the dotted line is the experimental measurement data, and the solid line is the nonlinear absorption theory fitting curve). DETAILED DESCRIPTION

[0043] In order to make the purpose, technical solution and advantages of the embodiments of the present invention clearer, the technical solution in the embodiments of the present invention will be clearly and completely described below in conjunction with the drawings in the embodiments of the present invention. Obviously, the described embodiments are part of the embodiments of the present invention, not all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.

[0044] Please refer to Figure 1 The embodiment of the present invention provides a method for preparing a broadband optical limiting device based on gallium nitride nanowires, comprising the following steps:

[0045] Step 1: Cut the conductive carbon paper into a shape of suitable size, perform ultrasonic cleaning on the conductive carbon paper for multiple times, and dry the conductive carbon paper after cleaning;

[0046] When ultrasonically cleaning the conductive carbon paper, acetone, ethanol, deionized water, and dilute hydrochloric acid may be used in sequence for ultrasonic cleaning, and then the conductive carbon paper may be rinsed and ultrasonically cleaned again with deionized water to remove residual chemicals.

[0047] Step 2: depositing catalyst metal gold for preparing gallium nitride nanowires on the dried conductive carbon paper;

[0048] Of course, in this embodiment, the catalyst is preferably metal gold, while in other embodiments, the catalyst may also be metal copper, nickel nitrate solution or other catalysts used for catalysis in the production of gallium nitride nanowires. When the catalyst is arranged on the conductive carbon paper, the catalyst may be arranged on the conductive carbon paper by coating, infiltration or other methods, which is not limited to this embodiment.

[0049] Step 3: Using gallium oxide as a gallium source and ammonia as a nitrogen source, a chemical vapor deposition method is used in a high-temperature tube furnace to grow gallium nitride nanowires on a conductive carbon paper with gold deposited on the surface. First, a ceramic boat containing gallium oxide powder is placed in the middle of a quartz tube of a high-temperature tube furnace, and a conductive carbon paper with a catalyst arranged on the surface is placed in the downstream position of the air flow in the quartz tube of the high-temperature tube furnace. Then, the quartz tube of the high-temperature tube furnace is sealed and evacuated. After evacuation, argon gas is filled into the quartz tube of the high-temperature tube furnace until it reaches normal pressure.

[0050] The high temperature tube furnace was heated up, and 150 sccm of nitrogen was continuously introduced for protection during the heating process;

[0051] After the temperature of the high-temperature tube furnace is raised to 1200 degrees, the input of nitrogen is stopped and 100 sccm of ammonia is introduced instead. The system is kept at 1200 degrees for 45 minutes to allow gallium oxide and ammonia to react and grow on the conductive carbon paper.

[0052] After the insulation is completed, stop the introduction of ammonia and introduce 150 sccm of nitrogen instead, and allow the system to cool to room temperature under the continuous protection of nitrogen;

[0053] In this embodiment, a mechanical pump may be used to evacuate the quartz tube into a vacuum, and the high-temperature tube furnace is set to be a single-temperature-zone horizontal high-temperature tube furnace available on the market.

[0054] Step 4: Take out the conductive carbon paper, adhere the thermal release tape to the surface of the conductive carbon paper with the gallium nitride nanowires grown, and evenly peel off the thermal release tape with the gallium nitride nanowires from the conductive carbon paper completely;

[0055] Step 5: The side of the thermal release tape with the GaN nanowires is tightly attached to the quartz plate, and then the quartz plate and the thermal release tape are heated as a whole, so that the thermal release tape foams and loses its stickiness, and the GaN nanowires are separated from the thermal release tape and fall on the quartz plate;

[0056] Preferably, in this embodiment, the quartz sheet and the thermal release tape are heated by a heating table, and the operation is: firstly, the heating table is heated to 120 degrees, and then the thermal release tape and the quartz sheet are placed on the heating table as a whole and heated for 5 minutes.

[0057] Step 6: Place the quartz sheet with the GaN nanowires attached in a beaker filled with deionized water, rinse it several times, and take out the quartz sheet to obtain a GaN nanowire dispersion;

[0058] Step 7: Heat the beaker to evaporate part of the water to obtain a high concentration of gallium nitride nanowire dispersion;

[0059] Step 8: The obtained high-concentration GaN nanowire dispersion is sealed in a light-transmitting container to produce a GaN nanowire optical limiting device, wherein the light-transmitting container can be a transparent quartz container.

[0060] In another embodiment, after obtaining a high-concentration gallium nitride nanowire dispersion, the user may also spin-coat the obtained gallium nitride nanowire dispersion on a light-transmitting substrate (e.g., a transparent quartz substrate or a sapphire substrate) and evaporate the water to obtain a water-free gallium nitride nanowire optical limiting device. In order to fix the gallium nitride nanowire layer, after evaporating the water, a light-transmitting material (e.g., a transparent quartz sheet, sapphire, etc.) may be used to cover the gallium nitride nanowire layer, and then the edge of the gallium nitride nanowire layer may be fixed by silica gel, hot melt adhesive or glass adhesive.

[0061] In summary, the present invention has the following advantages:

[0062] 1. The preparation process of the present invention is simple and convenient. The preparation raw materials are gallium oxide and ammonia, which are low in cost and require very little catalyst. The preparation process is simple and convenient for mass production. The catalyst is arranged on the conductive carbon paper for growth, which can save the use of the catalyst and further reduce the preparation cost. The present invention combines large-area transfer of the thermal release tape with growth on the conductive carbon paper. The preparation method is simple, the amount of catalyst used is small, the cost is low, and batch preparation is possible. The gallium nitride nanowires grown on the carbon paper are stripped by the thermal release tape to obtain pure gallium nitride nanowires, remove the carbon paper and the catalyst, and expand the application of the gallium nitride nanowires. The present invention proves that it can be used to prepare gallium nitride optical limiting devices. Compared with the commonly used ultrasonic stripping method, the thermal release tape stripping method of the present invention reduces impurities such as carbon paper and catalyst, prepares samples with high purity, and can protect the integrity of the nanowires, reducing the degree of damage and breakage of the nanowires.

[0063] 2. The gallium nitride nanowires of the present invention are prepared at high temperatures, have good physical and chemical stability, are resistant to high temperatures, have good thermal conductivity, and have a high damage threshold. The optical limiting device based on this material can be used as a dispersion or adsorbed on a substrate in an anhydrous form, and is suitable for a variety of occasions. The nanowires prepared by the preparation method have good crystallinity, a large aspect ratio, and good diameter uniformity, so the prepared optical limiting device has stable and excellent performance.

[0064] 3. The working spectrum range of the optical limiting device prepared by this preparation method is from deep ultraviolet 266nm to near infrared 1064nm wavelength, especially in the ultraviolet band, it has good optical limiting performance, and is a nano ultraviolet light limiting device with excellent performance.

[0065] 4. The optical limiting device based on gallium nitride nanowires prepared by this preparation method has high linear transmittance, and the transmittance at wavelengths of 266nm, 355nm, 532nm, and 1064nm is 50.2%, 53.5%, 59.9% and 65.6%, respectively. Figure 8 As shown, the optical limiting device has a large modulation depth. Figures 9 to 13 It can be seen that the modulation depths of this embodiment at 266nm, 355nm, 532nm and 1064nm wavelengths are 73.6%, 74.9%, 63.1% and 64.3% respectively, and the corresponding minimum transmittances are 26.4%, 25.1%, 36.9% and 35.7%. The nonlinear absorption theory fitting curve ( Figures 9 to 13 The solid line shows that the anti-saturation effect at 266 nm, 355 nm, and 532 nm is caused by two-photon absorption, and the two-photon absorption coefficients are 0.22 cm / GW, 0.28 cm / GW, and 0.08 cm / GW, respectively. The anti-saturation effect at 1064 nm is caused by three-photon absorption, and the three-photon absorption coefficient is 2.82×10 -4 cm 3 / GW 2 .

[0066] 5. The optical limiting device of the present invention covers and glues the edges, realizing the sandwich design of the optical limiting device, ensuring that the position of the gallium nitride nanowires is accurate and will not shift, the structure is stable, and the application occasions are wide.

[0067] The above embodiments are preferred implementation modes of the present invention, but the implementation modes of the present invention are not limited to the above embodiments. Any other changes, modifications, substitutions, combinations, and simplifications that do not deviate from the spirit and principles of the present invention should be equivalent replacement methods and are included in the protection scope of the present invention.

Claims

1. A method for preparing a broadband optical limiting device based on gallium nitride nanowires, characterized in that: The following steps are involved: Step 1: Perform ultrasonic cleaning on the conductive carbon paper for multiple times, and dry the conductive carbon paper after cleaning; Step 2: arranging a catalyst for preparing gallium nitride nanowires on a dried conductive carbon paper; Step 3: Using gallium oxide as a gallium source and ammonia as a nitrogen source, a chemical vapor deposition method is used in a high-temperature tube furnace to grow gallium nitride nanowires on a conductive carbon paper with a catalyst arranged on the surface; Step 4: Take out the conductive carbon paper from the high-temperature tube furnace, adhere the thermal release tape to the surface of the conductive carbon paper with the gallium nitride nanowires grown, and evenly peel off the thermal release tape with the gallium nitride nanowires from the conductive carbon paper completely; Step 5: The side of the thermal release tape with the GaN nanowires is tightly attached to the quartz plate, and then the quartz plate and the thermal release tape are heated as a whole, so that the thermal release tape foams and loses its stickiness, and the GaN nanowires are separated from the thermal release tape and fall on the quartz plate; Step 6: Place the quartz sheet with the GaN nanowires attached in a beaker filled with deionized water, rinse it several times, and take out the quartz sheet to obtain a GaN nanowire dispersion; Step 7: Heat the beaker to evaporate part of the water to obtain a high concentration of gallium nitride nanowire dispersion; Step 8: The obtained high-concentration gallium nitride nanowire dispersion is sealed in a light-transmitting container to produce a gallium nitride nanowire optical limiting device; Alternatively, the obtained high-concentration gallium nitride nanowire dispersion is spin-coated on a light-transmitting substrate, and the water is evaporated to obtain a water-free gallium nitride nanowire optical limiting device; Alternatively, the obtained high-concentration gallium nitride nanowire dispersion is spin-coated on a light-transmitting substrate, and after the water is evaporated, the edges are covered and glued to prepare a gallium nitride nanowire sandwich optical limiting device.

2. The method for preparing a broadband optical limiting device based on gallium nitride nanowires according to claim 1, characterized in that: When the gallium nitride nanowires are grown on the conductive carbon paper by chemical vapor deposition in step 3, the ceramic boat containing gallium oxide powder is first placed in the middle position of the high-temperature tubular furnace quartz tube, and the conductive carbon paper with a catalyst arranged on the surface is placed in the downstream position of the airflow in the high-temperature tubular furnace quartz tube, and then the high-temperature tubular furnace quartz tube is sealed, and the high-temperature tubular furnace quartz tube is evacuated into a vacuum. After evacuation, argon gas is filled into the high-temperature tubular furnace quartz tube until it reaches normal pressure, and the high-temperature tubular furnace is heated. During the heating process, 150 sccm of nitrogen is continuously introduced for protection. After the temperature of the high-temperature tubular furnace is raised to 1200 degrees, the input of nitrogen is stopped, and 100 sccm of ammonia is introduced instead, and the system is kept at 1200 degrees for 45 minutes to allow gallium oxide and ammonia to react and grow on the conductive carbon paper. After the insulation is completed, the introduction of ammonia is stopped, and 150 sccm of nitrogen is introduced instead, and the system is cooled to room temperature under the continuous protection of nitrogen.

3. The method for preparing a broadband optical limiting device based on gallium nitride nanowires according to claim 1, characterized in that: Before proceeding to step 1, cut the conductive carbon paper into a shape of appropriate size.

4. The method for preparing a broadband optical limiting device based on gallium nitride nanowires according to claim 1, characterized in that: When ultrasonically cleaning the conductive carbon paper in step 1, acetone, ethanol, deionized water, and dilute hydrochloric acid are used to ultrasonically clean the conductive carbon paper in sequence, and then the conductive carbon paper is rinsed and ultrasonically cleaned again with deionized water to remove residual chemicals.

5. The method for preparing a broadband optical limiting device based on gallium nitride nanowires according to claim 1, characterized in that: The catalyst in step 2 is set to be metal copper, metal gold or nickel nitrate solution.

6. The method for preparing a broadband optical limiting device based on gallium nitride nanowires according to claim 1, characterized in that: In step 2, the catalyst is arranged on the conductive carbon paper by deposition, coating or infiltration.

7. The method for preparing a broadband optical limiting device based on gallium nitride nanowires according to claim 1, characterized in that: The high temperature tube furnace is configured as a single temperature zone horizontal high temperature tube furnace.

8. The method for preparing a broadband optical limiting device based on gallium nitride nanowires according to claim 1, characterized in that: When heating the quartz sheet and the thermal release tape in step 5, first raise the temperature of the heating table to 120 degrees, and then place the thermal release tape and the quartz sheet as a whole on the heating table and heat for 5 minutes.

9. The method for preparing a broadband optical limiting device based on gallium nitride nanowires according to claim 1, characterized in that: The light-transmitting substrate is configured as a transparent quartz substrate or a sapphire substrate, and the light-transmitting container is configured as a transparent quartz container.