Manufacturing process of high-surge high-voltage diode product

By optimizing the chip thickness and structure, combining welding and corrosion treatment, the problems of high-surge rectifier diode chip manufacturing difficulty and poor surge are solved, high surge capability and stability are achieved, and thermal resistance and power consumption are reduced.

CN118943014AInactive Publication Date: 2024-11-12GALAXY SEMICON HLDG LTD
View PDF 5 Cites 0 Cited by

Patent Information

Application Number
CN202411042514.3
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-07-31
Publication Date
2024-11-12
Estimated Expiration
Not applicable · inactive patent

AI Technical Summary

Technical Problem

In micro-packages, it is difficult to manufacture high-surge rectifier diode chips, resulting in poor surge phenomena, and the chip's surge capability has not been reduced, but requires improvement. It is difficult for the existing technology to effectively solve this problem.

Method used

By optimizing the chip thickness and structure, phosphorus pre-diffusion, phosphorus re-diffusion, back and double-side thinning, surface metallization and welding treatment are adopted to reduce the chip thermal resistance, improve the heat conduction speed and structural compactness, combined with thick countertop leads and thin The welding process of welding sheets controls welding temperature and pickling corrosion conditions to ensure high surge capacity.

Benefits of technology

The high surge capability of the chip is achieved, the surge effect is improved, the thermal resistance and power consumption is reduced, the voltage consistency and stability is improved, the chip storage time is extended, and the mechanical damage and corrosion amount is reduced.

✦ Generated by Eureka AI based on patent content.
Patent Text Reader

Abstract

The invention relates to the technical field of semiconductor separation device production, and particularly discloses a manufacturing process of a high-surge high-voltage diode product. The invention discloses a manufacturing process of a high-surge high-voltage diode product. The manufacturing process comprises the following steps of S1, wafer selection: selecting a single crystal wafer with the resistance of 20-27 omega * cm and the thickness of 265-280 microns; s2, wafer treatment: carrying out phosphorus pre-diffusion, phosphorus re-diffusion, back thinning, boron diffusion, double-sided thinning, surface metallization and scribing treatment on the single crystal wafer to obtain a wafer to be treated; and S3, packaging: carrying out welding, acid pickling, gluing, curing and mold pressing on the wafer to be processed to obtain a diode semi-finished product. The diode prepared by the invention can be used in electrical components, and has the advantages of high surge capacity, complete structure, low power consumption and the like.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present application relates to the technical field of semiconductor separation device production, and more specifically, it relates to a high-surge high-voltage diode product manufacturing process. Background Art

[0002] With the development of miniaturization of electrical components, the miniaturization and SMD of chip packaging has become a market standard demand, but the requirements for chip capabilities in product applications have only increased. In miniaturized packaging, the chip size and power consumption are required to be reduced, but the chip surge capability has not only not decreased but has been required to be improved. However, the manufacturing of high surge rectifier diode chips is difficult, resulting in surge defects in some products, so it is necessary to improve the manufacturing method of diode chips. Summary of the invention

[0003] In order to improve the problem of poor surge of diode products, the present application provides a high-surge high-voltage diode product manufacturing process, which adopts the following technical solutions:

[0004] The present application provides a high-surge high-voltage diode product manufacturing process, comprising the following steps:

[0005] S1. Wafer selection: select a single wafer with a resistance of 20-27Ω*cm and a thickness of 265-280μm;

[0006] S2. Wafer processing: performing phosphorus pre-diffusion, phosphorus re-diffusion, backside thinning, boron diffusion, double-side thinning, surface metallization, and dicing on the single crystal to obtain a wafer to be processed;

[0007] S3, packaging: the wafer to be processed is welded, pickled, glued, cured, and molded to obtain a semi-finished diode.

[0008] By adopting the above technical solution, the thickness of the chip is optimized in this application, and the base width is compressed while reducing the thermal resistance of the chip to form an effective transistor, thereby providing good amplification performance. The main source of heat in the chip during surge is the impedance of the PN junction and the N-region P-region generated under high current. Therefore, when reducing the thickness of the chip, in addition to reducing the generation of heat, the heat conduction speed is also accelerated. By using grinding and thinning processes such as back grinding and double-sided grinding, the thickness of the chip can be further reduced, the thermal resistance of the chip can be further reduced, the heat conduction speed of the chip can be improved, and the structure can be made more compact. It can also make the welding pores of the wafer smaller, and obtain better forward voltage drop and voltage consistency.

[0009] Optionally, in step S2, the sheet resistance R□ after the phosphorus pre-diffusion is 0.25-0.36Ω*cm.

[0010] By adopting the above technical solution, the resistivity in the pre-diffusion is optimized, the pre-diffusion effect is made uniform, and the surge effect of the chip is improved.

[0011] Optionally, in step S2, the back side thinning amount is 15-20 μm, and the back side thinning includes sandblasting thinning and grinding thinning, the sandblasting thinning amount is 10-15 μm, and the grinding thinning amount is 5 μm.

[0012] Optionally, in step S2, the double-sided thinning amount is 20-30 μm, and the double-sided thinning includes sandblasting thinning and grinding thinning, the sandblasting thinning amount is 15-20 μm, and the grinding thinning amount is 5-10 μm.

[0013] By adopting the above technical solution, the total thickness of the chip is fully reduced by double-sided thinning, and the total thickness of the wafer is appropriate, which can make the structure of the chip product more compact and reduce the amount of materials. The total thickness of the chip is appropriate, which can reduce the forward resistance of the product, the power consumption under high current, and the occurrence of weak stress resistance.

[0014] Optionally, in step S2, the surface metallization method is as follows: place the double-sided ground diffusion sheet in a corrosive solution for corrosion, clean, clean with a phosphoric acid solution, chemically nickel plated, clean and dry, burn infiltration, pickle, secondary nickel plating, clean and dry, burn infiltration, pickle, gold plating, and drying; wherein the thickness of a single nickel plating is 0.15-0.3μm, and the thickness of the gold plating is ≤0.1μm.

[0015] By adopting the above technical solution, double-layer nickel plating and surface metallization treatment are performed on the surface of the wafer, the thickness of the nickel plating layer is thinned, which can reduce the stress when it comes into contact with silicon during high-temperature sintering. By electroplating a thinner gold layer on the surface, the overall structure of the wafer changes less. Due to the inertness of gold itself, the storage time of the wafer at room temperature and humidity can be effectively increased, the weldability of the wafer is improved, and the stability of the chip product is improved.

[0016] Optionally, in step S3, during the welding process, a thick table with a wire diameter of ≥0.78 mm and a thin welding sheet with a thickness of 0.03-0.05 mm and a silver content of ≥3% are selected.

[0017] By adopting the above technical solution, the heat dissipation effect is increased through the combination of thick table leads and thin solder sheets, which can greatly improve the surge level. The high conductivity of silver in the solder sheet is used to improve the thermal conductivity of the chip, and the selection of thin solder sheets ensures the ductility and conductivity of the solder.

[0018] Optionally, in step S3, during the welding process, the temperature of the welding furnace is 313-335°C, and the time that the temperature of the welding furnace is above 300°C is controlled within 7.5-12 minutes.

[0019] By adopting the above technical solution, the welding temperature is optimized in the present application. By performing welding processing at a lower temperature, the welding pores of the wafer can be made smaller, which is beneficial to improving the forward voltage drop and voltage consistency, and effectively improving the problem of excessively large pores in tunnel furnace welding.

[0020] Optionally, in step S3, the pickling temperature is 15-21°C, the water support (liquid seal) temperature is 15-21°C, and the difference between the pickling temperature and the ambient temperature is ≤3°C.

[0021] By adopting the above technical solution, the difference between the ambient temperature and the corrosive acid temperature is strictly controlled. The difference between the corrosive acid temperature and the ambient temperature is less than 3 degrees Celsius, which avoids diamond corrosion phenomenon, makes the chip corrosion surface smoother and more stable, reduces the corrosion amount, and increases the current area to achieve micro-corrosion effect.

[0022] Optionally, in step S3, the maximum reduction of the product after pickling treatment is ≤0.26 mm.

[0023] By adopting the above technical solution, the corrosion amount of pickling corrosion is controlled, so that the chip surface achieves a micro-corrosion effect, which is beneficial for the chip to obtain a higher current area.

[0024] Optionally, the surge capability of the diode product is ≥36A / mm 2 .

[0025] By adopting the above technical solution, the diode prepared by the manufacturing process of this application can obtain higher surge capability and effectively improve the surge effect of the chip.

[0026] In summary, this application has the following beneficial effects:

[0027] 1. Since the chip material single crystal wafer used in this application is single crystal silicon SI, and silicon is a poor conductor of heat, the heat of the chip during surge mainly comes from the impedance of the PN junction and the N and P regions under large currents. Therefore, this application reduces the thickness of the chip, not only reduces the generation of heat, but also speeds up the heat conduction speed, effectively reduces the thermal resistance of the chip product, and obtains better consistency of the chip, maintaining the reliability level of the product.

[0028] 2. In this application, the chip is ground to make the chip welding pores smaller and obtain excellent forward voltage drop and voltage consistency.

[0029] 3. In this application, the nickel plating layer is thinned and gold-plated, which prolongs the storage time of the chip at room temperature and humidity, and is conducive to maintaining good solderability of the chip.

[0030] 4. In this application, thick table leads and silver-containing thin solder sheets are preferably used to process the chip, which improves the heat dissipation effect of the chip and can greatly increase the surge level of the chip. Under high surges, the forward voltage drop is reduced, the power consumption is reduced, and less heat needs to be dissipated.

[0031] 5. When processing the chip in this application, high-speed cutting and slow stepping are used, which can effectively reduce the mechanical damage to the chip caused by cutting and maintain the integrity of the chip.

[0032] 6. In this application, the ambient temperature, corrosion temperature and corrosion time of pickling corrosion are reduced to make the chip surface PN smoother and improve production efficiency. DETAILED DESCRIPTION

[0033] The present application is further described in detail below with reference to the embodiments.

[0034] Example

[0035] Example 1

[0036] The present application provides a high-surge high-voltage diode product manufacturing process, comprising the following steps:

[0037] S1. Wafer selection: Select a single crystal wafer with a resistance of 20Ω*cm and a thickness of 265μm

[111] radial as the wafer to be processed;

[0038] S2. Wafer processing:

[0039] S21, pre-diffusion: paper source process is used for phosphorus pre-diffusion. During phosphorus pre-diffusion, the resistance is 0.25Ω*cm;

[0040] S22, phosphorus re-diffusion: phosphorus re-diffusion is carried out using paper source process, and the sheet resistance R□ is 0.25Ω*cm;

[0041] S23, back grinding: grinding the back side of the wafer after phosphorus pre-diffusion, specifically, the back side grinding includes sandblasting thinning and grinding thinning, the sandblasting thinning is 10 μm, the grinding thinning is 5 μm, and the total back side grinding thickness is 15 μm;

[0042] S24, boron diffusion: boron diffusion is performed on the wafer after back grinding. During the boron diffusion, the sheet resistance R□ is controlled to be 0.1Ω*cm and the junction depth is 90μm;

[0043] S25, double-sided grinding: using double-sided sandblasting to thin the boron-diffused wafer, the double-sided grinding includes sandblasting and grinding, the sandblasting thinning is 15 μm, the grinding thinning is 5 μm, the total thinning is 20 μm, and a thinned wafer is obtained; using a grinding machine, using an 8000# grinding wheel, at a speed of 3000 r / min, the thinned wafer is double-sided ground to a thickness of 230 μm;

[0044] S26, gold plating treatment: the double-sided polished wafer is placed in a corrosive solution (hydrofluoric acid: buffer mass ratio is 1:20), the etching treatment is repeated three times, and the wafer is washed, and then the wafer is placed in a 5% by mass Hammer powder solution, ultrasonicated for 30 seconds, washed with hot water, and then washed with acid (H3PO4:H2O2:H2O mass ratio is 1:1:5), washed with water, nickel plated, the thickness of the nickel layer is controlled to be 0.15μm, washed, dried, burned, rinsed with acid to remove surface oxidation, nickel plated twice, the thickness of the nickel layer is controlled to be 0.15μm, washed, dried, burned, rinsed with acid to remove surface oxidation, gold plated, the thickness of the gold layer is 0.01μm, washed, dried, and dried at 70℃ for 30min;

[0045] S27, scribing: scribing the gold-plated wafer to obtain an intermediate wafer;

[0046] S3, packaging:

[0047] S31, welding: welding the intermediate wafer, specifically, using 0.78mm thick table lead wire, using 3% silver-containing 0.03mm thick thin solder, controlling the welding furnace temperature at 313-335°C, and maintaining the welding furnace temperature ≥300°C for a total of 7.5 minutes;

[0048] S32, pickling treatment: pickling and etching the soldered chip at 21°C;

[0049] S33, intermediate processing: gluing, curing, molding and aging the chip after pickling to obtain a diode product.

[0050] Example 2

[0051] The present application provides a high-surge high-voltage diode product manufacturing process, comprising the following steps:

[0052] S1. Wafer selection: Select a single crystal wafer with a resistivity of 24Ω*cm and a thickness of 275μm

[111] radial as the wafer to be processed;

[0053] S2. Wafer processing:

[0054] S21, pre-diffusion: phosphorus pre-diffusion is performed using a paper source process. During phosphorus pre-diffusion, the sheet resistance R□ is 0.30Ω*cm;

[0055] S22, phosphorus re-diffusion: phosphorus re-diffusion is carried out using paper source process, and the sheet resistance R□ is 0.30Ω*cm;

[0056] S23, back grinding: grinding the back side of the wafer after phosphorus pre-diffusion, specifically, the back side grinding includes sandblasting thinning and grinding thinning, the sandblasting thinning is 13 μm, the grinding thinning is 5 μm, and the total back side grinding thickness is 18 μm;

[0057] S24, boron diffusion: Boron diffusion is performed on the wafer after back grinding. During the boron diffusion, the sheet resistance R□ is controlled to be 0.11Ω*cm and the junction depth is 100μm;

[0058] S25, double-sided grinding: double-sided sandblasting is used to thin the boron-diffused wafer, and double-sided grinding includes sandblasting thinning and grinding thinning, sandblasting thinning is 20μm, grinding thinning is 5μm, and the total thinning amount is 25μm, to obtain a thinned wafer; using a grinding machine, using an 8000# grinding wheel, double-sided grinding of the thinned wafer at a speed of 3000r / min, so that the thickness of the wafer is 240μm;

[0059] S26, gold plating treatment: the double-sided polished wafer is placed in a corrosive solution (hydrofluoric acid: buffer mass ratio is 1:20), the etching treatment is repeated three times, and the wafer is washed, and then the wafer is placed in a 5% by mass Hammer powder solution, ultrasonicated for 30 seconds, washed with hot water, and then washed with acid solution (H3PO4:H2O2:H2O mass ratio is 1:1:5), washed with water, nickel plated, the thickness of the nickel layer is controlled to be 0.2μm, washed, dried, burned, rinsed with acid solution to remove surface oxidation, nickel plated twice, the thickness of the nickel layer is controlled to be 0.2μm, washed, dried, burned, rinsed with acid solution to remove surface oxidation, gold plated, the thickness of the gold layer is 0.01μm, washed, dried, and dried at 70℃ for 30min;

[0060] S27, scribing: scribing the gold-plated wafer to obtain an intermediate wafer;

[0061] S3, packaging:

[0062] S31. Welding: welding the intermediate wafer. Specifically, using a 0.78 mm thick table lead wire and a 0.04 mm thick thin solder containing 3% silver, the welding furnace temperature is controlled at 313-335°C, and the welding furnace temperature is maintained at ≥300°C for a total of 10 minutes.

[0063] S32, pickling treatment: pickling and etching the soldered chip at 21°C;

[0064] S33, intermediate processing: gluing, curing, molding and aging the chip after pickling to obtain a diode product.

[0065] Example 3

[0066] The present application provides a high-surge high-voltage diode product manufacturing process, comprising the following steps:

[0067] S1. Wafer selection: Select a single crystal wafer with a resistivity of 27Ω*cm and a thickness of 280μm

[111] radial direction as the wafer to be processed;

[0068] S2. Wafer processing:

[0069] S21, pre-diffusion: phosphorus pre-diffusion is carried out by paper source process. During phosphorus pre-diffusion, the sheet resistance R□ is 0.36Ω*cm;

[0070] S22, phosphorus re-diffusion: phosphorus re-diffusion is carried out using paper source process, and the sheet resistance R□ is 0.36Ω*cm;

[0071] S23, back grinding: grinding the back side of the wafer after phosphorus pre-diffusion, specifically, the back side grinding includes sandblasting thinning and grinding thinning, the sandblasting thinning is 15 μm, the grinding thinning is 5 μm, and the total back side grinding thickness is 20 μm;

[0072] S24, boron diffusion: Boron diffusion is performed on the wafer after back grinding. During the boron diffusion, the sheet resistance R□ is controlled to be 0.12Ω*cm and the junction depth is 110μm;

[0073] S25, double-sided grinding: double-sided sandblasting is used to thin the boron-diffused wafer, and double-sided grinding includes sandblasting thinning and grinding thinning, sandblasting thinning is 20μm, grinding thinning is 10μm, and the total thinning amount is 30μm, to obtain a thinned wafer; using an 8000# grinding wheel, double-sided grinding is performed on the thinned wafer at a rotation speed of 3000r / min, so that the thickness of the wafer is 250μm;

[0074] S26, gold plating treatment: the double-sided polished wafer is placed in a corrosive solution (hydrofluoric acid: buffer mass ratio is 1:20), the etching treatment is performed for 30 seconds, repeated three times, and then the wafer is placed in a 5% by mass Hammer powder solution, ultrasonicated for 30 seconds, washed with hot water, and then cleaned with an acid solution (H3PO4:H2O2:H2O mass ratio is 1:1:5), washed with water, nickel plated, the thickness of the nickel layer is controlled to be 0.3 μm, washed, dried, burned, rinsed with acid to remove surface oxidation, nickel plated twice, the thickness of the nickel layer is controlled to be 0.3 μm, washed, dried, burned, rinsed with acid to remove surface oxidation, gold plated, the thickness of the gold layer is 0.01 μm, washed, dried, and dried at 70°C for 30 minutes;

[0075] S27, dicing: dicing the gold-plated wafer to obtain an intermediate wafer; S3, packaging:

[0076] S31. Welding: welding the intermediate wafer. Specifically, using a 0.78 mm thick table lead wire and a 0.05 mm thick thin solder containing 3% silver, the welding furnace temperature is controlled at 313-335°C, and the welding furnace temperature is maintained at ≥300°C for a total of 12 minutes.

[0077] S32, pickling treatment: pickling and etching the soldered chip at 21°C;

[0078] S33, intermediate processing: gluing, curing, molding and aging the chip after pickling to obtain a diode product.

[0079] Comparative Example

[0080] Comparative Example 1

[0081] The present application provides a high-surge high-voltage diode product manufacturing process, comprising the following steps:

[0082] S1. Wafer selection: Select a single crystal wafer with a resistivity of 20Ω*cm and a thickness of 265μm

[111] radial as the wafer to be processed;

[0083] S2. Wafer processing:

[0084] S21, pre-diffusion: During phosphorus pre-diffusion, the sheet resistance R□ is 0.25Ω*cm;

[0085] S22, back grinding: grinding the back side of the wafer after phosphorus pre-diffusion, specifically, the grinding thickness is 15 μm;

[0086] S23, boron diffusion: boron diffusion is performed on the wafer after back grinding. During the boron diffusion, the sheet resistance R□ is controlled to be 0.1Ω*cm and the junction depth is 90μm;

[0087] S24, double-sided grinding: double-sided grinding of the boron-diffused wafer to make the wafer thickness 230 μm;

[0088] S25, gold plating treatment: the double-sided polished wafer is placed in an etching solution (hydrofluoric acid: buffer mass ratio is 1:20), the etching treatment is performed for 30 seconds, repeated three times, and then the wafer is placed in a 5% by mass Hammer powder solution, ultrasonicated for 30 seconds, washed with hot water, and then cleaned with an acid solution (H3PO4:H2O2:H2O mass ratio is 1:1:5), washed with water, nickel plated, the thickness of the nickel layer is controlled to be 0.15 μm, cleaned, dried, burned, rinsed with acid to remove surface oxidation, nickel plated twice, the thickness of the nickel layer is controlled to be 0.15 μm, cleaned, and dried;

[0089] S26, scribing: scribing the gold-plated wafer to obtain an intermediate wafer;

[0090] S3, packaging:

[0091] S31, welding: welding the intermediate wafer, specifically, using 0.78mm thick table lead wire, using 3% silver-containing 0.03mm thick thin solder, controlling the welding furnace temperature at 313-335°C, and maintaining the welding furnace temperature ≥300°C for a total of 7.5 minutes;

[0092] S32, pickling treatment: pickling and etching the chip after welding;

[0093] S33, intermediate processing: gluing, curing, molding and aging the chip after pickling to obtain a diode product.

[0094] Performance testing

[0095] (1) Surge capability test: Use the PIF8000 test system to perform surge capability test on diode products.

[0096] After testing, the surge capacity of the diode products in Examples 1 to 3 is ≥36A / mm 2 Specifically, the surge capacity of the diode product in Example 1 is 36A / mm 2 The surge capacity of the diode product in Example 2 is 38A / mm 2 The surge capacity of the diode product in Example 3 is 39A / mm 2 The surge capacity of the diode product in Comparative Example 1 is 30A / mm 2 .

[0097] This specific embodiment is merely an explanation of the present application and is not a limitation of the present application. After reading this specification, those skilled in the art may make modifications to the present embodiment without any creative contribution as needed, but such modifications are protected by the patent law as long as they are within the scope of the claims of the present application.

Claims

1. A high surge high voltage diode product manufacturing process, characterized in that: The following steps are involved: S1. Wafer selection: select a single wafer with a resistance of 20-27Ω*cm and a thickness of 265-280μm; S2. Wafer processing: performing phosphorus pre-diffusion, phosphorus re-diffusion, backside thinning, boron diffusion, double-side thinning, surface metallization, and dicing on the single crystal to obtain a wafer to be processed; S3, packaging: the wafer to be processed is welded, pickled, glued, cured, and molded to obtain a semi-finished diode.

2. The high surge high voltage diode product manufacturing process according to claim 1, characterized in that: In step S2, the square resistance R□ after the phosphorus pre-diffusion is 0.25-0.36Ω*cm.

3. The high surge high voltage diode product manufacturing process according to claim 1, characterized in that: In step S2, the back side thinning amount is 15-20 μm, and the back side thinning includes sandblasting thinning and grinding thinning. The sandblasting thinning amount is 10-15 μm, and the grinding thinning amount is 5 μm.

4. The high surge high voltage diode product manufacturing process according to claim 1, characterized in that: In step S2, the double-sided thinning amount is 20-30 μm, and the double-sided thinning includes sandblasting thinning and grinding thinning. The sandblasting thinning amount is 15-20 μm, and the grinding thinning amount is 5-10 μm.

5. The high surge high voltage diode product manufacturing process according to claim 1, characterized in that: In step S2, the surface metallization method is as follows: place the double-sided polished diffusion sheet in a corrosive solution for corrosion, clean, clean with a phosphoric acid solution, chemically nickel plated, clean and dry, burn infiltration, pickle, secondary nickel plating, clean and dry, burn infiltration, pickle, gold plating, and drying; wherein the thickness of a single nickel plating is 0.15-0.3μm, and the thickness of the gold plating is ≤0.015μm.

6. The high surge high voltage diode product manufacturing process according to claim 5, characterized in that: In step S3, during the welding process, a thick table with a wire diameter of ≥0.78 mm and a thin welding sheet with a thickness of 0.03-0.05 mm and a silver content of ≥3% are selected.

7. The high surge high voltage diode product manufacturing process according to claim 6, characterized in that: In step S3, during the welding process, the temperature of the welding furnace is 313-335°C, and the time when the temperature of the welding furnace is above 300°C is controlled within 7.5-12 minutes.

8. The high surge high voltage diode product manufacturing process according to claim 1, characterized in that: In step S3, the pickling temperature is 15-21°C, the water support (liquid seal) temperature is 15-21°C, and the difference between the pickling temperature and the ambient temperature is ≤3°C.

9. The high surge high voltage diode product manufacturing process according to claim 8, characterized in that: In step S3, the maximum reduction of the product after pickling treatment is ≤0.26 mm.

10. The high surge high voltage diode product manufacturing process according to claim 1, characterized in that: The surge capability of the diode product is ≥36A / mm 2 .

Citation Information

Patent Citations

  • High-voltage diode for frequency-variable microwave oven and production process thereof

    CN102064107A

  • Fast recovery diode (FRD) chip and production process thereof

    CN102087976A

  • Production technology for transient voltage suppressor chip with channeling effect

    CN103956324A

  • Transient diode and packaging process thereof

    CN111403366A

  • Diode and manufacture thereof

    JP2000323488A