Preparation and application of aqueous zinc ion battery electrolyte with wide temperature range, high stability and high entropy

By using multi-component high-entropy electrolyte in aqueous zinc ion batteries, the problems of dendrites on the zinc negative electrode and hydrogen evolution reaction are solved, the cycle performance and safety of the battery are improved, and stable under low temperature conditions are maintained, which is broadened Battery application range.

CN118943519APending Publication Date: 2024-11-12JIANGSU UNIV

Patent Information

Application Number
CN202410988556.X
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-07-23
Publication Date
2024-11-12

AI Technical Summary

Technical Problem

Water-based zinc ion batteries have poor cycle reversibility, low Coulomb efficiency and short cycle life due to the formation of zinc negative side dendrites, hydrogen evolution reaction and high corrosion, which limits their large-scale application.

Method used

Using multi-component high-entropy electrolytes, including zinc sulfate, zinc trifluoromethanesulfonate and zinc chloride, combined with ethylene glycol, deionized water and dimethyl sulfoxide as solvents, the solvation structure of the electrolyte is changed. and increase complexity, inhibit dendrite generation and hydrogen evolution reaction, improve uniform deposition of zinc ions and cell stability.

Benefits of technology

It significantly improves the circulation performance, Coulomb efficiency and safety of zinc ion batteries, extends the cycle life of the battery, broadens the operating conditions of the battery, realizes high-power energy storage, and maintains stability under low temperature conditions.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118943519A_ABST
    Figure CN118943519A_ABST
Patent Text Reader

Abstract

The invention discloses preparation and application of a wide-temperature-range, high-stability and high-entropy aqueous zinc ion battery electrolyte. The electrolyte contains a plurality of soluble zinc salts and a plurality of solvents; the various soluble zinc salts are zinc sulfate, zinc trifluoromethanesulfonate and zinc chloride; the various solvents are ethylene glycol, deionized water and dimethyl sulfoxide. According to the preparation and application of the wide-temperature-range high-stability high-entropy aqueous zinc ion battery electrolyte, the electrolyte can promote uniform deposition of zinc ions, avoid generation of zinc dendrites and improve coulombic efficiency and cycle performance of a zinc negative electrode; hydrogen evolution corrosion and dissolution of the zinc negative electrode can be effectively inhibited, the problem of battery expansion is avoided, the safety of the battery is improved, and the cycle life of the battery is prolonged; the capacity fading rate of the zinc ion battery can be improved and the capacity of the battery can be improved by improving the reaction kinetics of the battery; and the zinc ion battery has relatively good stability and low-temperature performance, and the application condition of the zinc ion battery is widened.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention relates to the technical field of aqueous zinc ion batteries, and in particular to the preparation and application of an aqueous zinc ion battery electrolyte with high stability and high entropy over a wide temperature range. Background Art

[0002] Since the advent of lithium-ion batteries (LIBs), they have been widely used in energy storage, portable electronic devices, and electric vehicles due to their high energy density and long cycle life. However, the scarcity of lithium resources, high prices, lack of environmental protection, and the toxic, volatile, and flammable organic electrolytes used have greatly hindered their further development.

[0003] At present, aqueous zinc-ion batteries (ZIBs) have been widely used due to their abundant resources, low cost, high safety, environmental friendliness, high theoretical energy (820 mAh g -1 , 5855mAh cm -2 ) and lower redox potential (-0.762V vs. SHE), etc., which have attracted wide attention in energy storage devices. In addition, compared with lithium-ion batteries, aqueous zinc-ion batteries use aqueous electrolytes, which have the advantages of better safety, simpler operation, low viscosity and higher ionic conductivity. These advantages make aqueous zinc-ion batteries have broader application prospects in the field of energy storage.

[0004] However, there are some challenges in the practical application of aqueous zinc-ion batteries. Due to the formation of side dendrites, hydrogen evolution reaction, high corrosion and passivation of the zinc metal negative electrode, the cycle reversibility of the zinc negative electrode is poor, the coulombic efficiency is low and the cycle life is short, which eventually leads to battery failure. These challenges have become the main obstacles to the large-scale application of aqueous zinc-ion batteries, so it is necessary to find suitable methods to improve the above problems.

[0005] In terms of zinc anode protection, electrolyte modification is a simple and easy method that can effectively inhibit dendrite growth. By adding other soluble zinc salts and organic component solvents to the aqueous electrolyte, the electrochemical performance of the battery can be significantly improved, and the safety and cycle life of the aqueous zinc-ion battery can be increased.

[0006] The participation of multiple components adjusts the solvation structure in the electrolyte, improves the interface performance of the electrode / electrolyte, promotes the uniform deposition of zinc ions, and inhibits the formation of moss-like dendrites. At the same time, it reduces the presence of active water, inhibits the hydrogen evolution reaction, avoids the generation of side reactions and corrosion of the zinc negative electrode, and can also improve the energy density of aqueous zinc-ion batteries and improve the capacity decay of batteries.

[0007] In addition, due to the participation of multiple components, the electrolyte has multiple solvation structures, which increases the complexity of the electrolyte, increases the entropy value of the electrolyte system, and effectively reduces the freezing point of the electrolyte, so that the electrolyte can operate at low temperatures of -20°C, broadens the battery operation conditions, and further improves the stability of aqueous zinc-ion batteries. Therefore, the aqueous high-entropy electrolyte formed by mixing multiple components can effectively solve the dendrite formation and corrosion problems of aqueous zinc-ion batteries and broaden the battery operation conditions, which will have broad application prospects. Summary of the invention

[0008] To solve the above problems, the present invention provides a preparation and application of a high-entropy aqueous zinc ion battery electrolyte with high stability in a wide temperature range. The prepared high-entropy electrolyte containing multiple components has good stability, can effectively protect the zinc negative electrode, increase the battery capacity, enhance the low-temperature performance, and can achieve high-power energy storage, thereby improving the cycle performance, coulombic efficiency, safety and electrochemical performance of the aqueous zinc ion battery.

[0009] To achieve the above object, the present invention provides a method for preparing a high-entropy aqueous zinc ion battery electrolyte with high stability over a wide temperature range, comprising the following steps:

[0010] S1. Dissolve zinc sulfate in ethylene glycol, and stir and dissolve at room temperature to prepare electrolyte A;

[0011] S2, dissolving zinc trifluoromethanesulfonate in deionized water, stirring and dissolving at room temperature to prepare electrolyte B;

[0012] S3, dissolving zinc chloride in dimethyl sulfoxide, stirring and dissolving at room temperature to prepare electrolyte C;

[0013] S4. A wide temperature range, high stability, and high entropy aqueous zinc ion battery electrolyte is prepared according to the volume ratio of electrolyte A: electrolyte B: electrolyte C of 2:2:1.

[0014] Preferably, in step S1, the concentration of electrolyte A is 2 mol / L.

[0015] Preferably, in step S2, the concentration of electrolyte B is 3 mol / L.

[0016] Preferably, in step S3, the concentration of the electrolyte C is 2 mol / L.

[0017] In the high entropy electrolyte containing multiple components disclosed in the present invention, zinc sulfate, zinc trifluoromethanesulfonate and zinc chloride are all soluble zinc salts. - It is a hydrophobic anion that can effectively prevent water from reaching the zinc negative electrode, avoiding hydrogen evolution reaction and negative electrode corrosion; Cl -The ions have strong electronegativity and penetrability, and can effectively destroy the zinc oxide passivation layer generated on the surface of zinc metal, thereby improving the reaction activity of the zinc negative electrode.

[0018] The three solvents used are ethylene glycol, deionized water and dimethyl sulfoxide, which are mainly composed of organic components. The presence of deionized water in the solvent can improve the ionic conductivity of the electrolyte, reduce the viscosity of the electrolyte, and increase the transmission rate of zinc ions in the electrolyte, thereby improving the electrochemical performance of the zinc ion battery.

[0019] After the three electrolytes are mixed, due to the complex components and the presence of multiple functional groups, the solvation structure in the electrolyte can be changed, the types of solvation in the electrolyte system can be increased, and the complexity of the system can be increased. The functional groups in the organic components can be adsorbed on the surface of the zinc negative electrode of the zinc ion battery, giving it properties such as high chemical adsorption effect and interface stability, thereby inducing uniform deposition of zinc ions, inhibiting the "tip effect", and reducing the formation of zinc dendrites.

[0020] At the same time, since ethylene glycol and dimethyl sulfoxide are anticoagulant solvents, they can lower the freezing point of the electrolyte, allowing the electrolyte to operate at a low temperature of -20°C, broadening the conditions for battery operation and further improving the stability of the aqueous zinc-ion battery.

[0021] The preparation and application of a wide temperature range, high stability and high entropy aqueous zinc ion battery electrolyte of the present invention have the following beneficial effects:

[0022] (1) The multi-component electrolyte can accelerate the reversibility of the zinc negative electrode electroplating / stripping process, promote uniform zinc deposition, inhibit the formation of moss-like dendrites, and improve the cycle performance, coulombic efficiency and reversible capacity of the zinc ion battery, thereby obtaining better electrochemical performance;

[0023] (2) The participation of multiple components changes the solvation structure of the electrolyte, resulting in a decrease in the amount of active water in the electrolyte, which can weaken the hydrogen evolution reaction and corrosion on the zinc negative electrode side, thereby improving the safety and cycle life of the battery;

[0024] (3) The electrolyte has a variety of solvation structures, which increases the complexity of the electrolyte, increases the entropy value of the electrolyte system, effectively reduces the freezing point of the electrolyte, improves the low-temperature performance of the battery, and broadens the operating conditions of the battery;

[0025] (4) The participation of multiple components can also improve the capacity, energy density and rate performance of the battery and improve the capacity attenuation problem of zinc ion batteries;

[0026] (5) The full battery assembled with the high-entropy electrolyte containing multiple components has a higher specific capacity and capacity retention rate, which further shows that the electrolyte can effectively improve the electrochemical performance of aqueous zinc-ion batteries, which is of great significance for the development of rechargeable aqueous zinc-ion batteries with excellent performance and high safety;

[0027] (6) The present invention synthesizes three electrolytes separately first and then mixes them into a final electrolyte in a certain proportion. The synthesis process is simple, the raw materials are easily available, the reaction conditions are easy to control and easy to implement, and the obtained electrolyte is relatively stable, not easy to volatilize and burn, and has good compatibility with zinc ion batteries. This mixed electrolyte is helpful for the development of rechargeable aqueous zinc ion batteries with excellent performance, high safety and green environmental protection.

[0028] The technical solution of the present invention is further described in detail below through the accompanying drawings and embodiments. BRIEF DESCRIPTION OF THE DRAWINGS

[0029] Figure 1 The aqueous zinc ion Zn / / Cu asymmetric battery prepared by the blank zinc sulfate electrolyte of the comparative example of the present invention and the multi-component electrolyte of the embodiment was subjected to a temperature of 25°C and a current density of 1 mA / cm 2 and 1mAh / cm 2 Coulomb efficiency under conditions;

[0030] Figure 2 The aqueous zinc ion Zn / / Zn symmetric battery prepared by the blank zinc sulfate electrolyte of the comparative example of the present invention and the multi-component electrolyte of the embodiment was subjected to a temperature of 25°C and a current density of 1 mA / cm 2 and 1mAh / cm 2 Time voltage curve under the conditions;

[0031] Figure 3 The aqueous zinc ion Zn / / Cu asymmetric battery prepared by the blank zinc sulfate electrolyte of the comparative example of the present invention and the multi-component electrolyte of the embodiment is subjected to a current density of 1 mA / cm 2 and 1mAh / cm 2 Scanning electron microscopy image of zinc negative electrode after 50 cycles under the same conditions;

[0032] Figure 4 It is a long cycle performance diagram of an aqueous zinc ion Zn / / PANI full battery prepared by a blank zinc sulfate electrolyte of the comparative example of the present invention and a multi-component electrolyte of the embodiment at a temperature of 25° C. and a charge and discharge current density of 1 A / g;

[0033] Figure 5 The aqueous zinc ion Zn / / Cu asymmetric battery prepared by the blank zinc sulfate electrolyte of the comparative example of the present invention and the multi-component electrolyte of the embodiment was subjected to a temperature of -20°C and a current density of 1 mA / cm2 and 1mAh / cm 2 Coulomb efficiency under these conditions. DETAILED DESCRIPTION

[0034] In order to make the purpose, technical scheme and advantages disclosed in the embodiments of the present invention clearer, the embodiments of the present invention are further described in detail in conjunction with the accompanying drawings and embodiments. It should be understood that the specific embodiments described herein are only used to explain the embodiments of the present invention and are not intended to limit the embodiments of the present invention. Based on the embodiments in this application, all other embodiments obtained by ordinary technicians in this field without making creative work are within the scope of protection of this application. Examples of the embodiments are shown in the accompanying drawings, where the same or similar reference numerals throughout represent the same or similar elements or elements with the same or similar functions.

[0035] It should be noted that the terms "including" and "having" and any variations thereof are intended to cover non-exclusive inclusions. For example, a process, method, system, product or server that includes a series of steps or units is not necessarily limited to those steps or units explicitly listed, but may include other steps or units that are not explicitly listed or inherent to these processes, methods, products or devices.

[0036] Like reference numerals and letters denote similar items in the following drawings, and thus, once an item is defined in one drawing, further definition and explanation thereof is not required in subsequent drawings.

[0037] Example

[0038] An aqueous zinc ion battery with a wide temperature range, high stability and high entropy aqueous zinc ion battery electrolyte, the preparation process comprising:

[0039] S1. Preparation of multi-component electrolyte

[0040] S1-1, dissolve 1.150g zinc sulfate in 2mL ethylene glycol, stir and dissolve at room temperature to prepare electrolyte A with a concentration of 2mol / L;

[0041] S1-2, dissolve 2.181g zinc trifluoromethanesulfonate in 2mL deionized water, and stir and dissolve at room temperature to prepare electrolyte B with a concentration of 3mol / L;

[0042] S1-3, dissolve 0.273g zinc chloride in 1mL dimethyl sulfoxide, stir and dissolve at room temperature to prepare electrolyte C with a concentration of 2mol / L;

[0043] S1-4. Mix the three electrolytes ABC in a ratio of 2:2:1 to form 5 mL of a multi-component electrolyte for standby use.

[0044] S2. Assembly of aqueous zinc ion batteries: First, place the zinc foil on the negative electrode shell side, then place the diaphragm in turn, add 0.1 mL of electrolyte to wet the diaphragm, then place the copper foil (Zn / / Cu asymmetric battery), zinc foil (Zn / / Zn symmetric battery) and positive electrode sheet (Zn / / PANI full battery) in turn, then place the gasket, spring and positive electrode shell in turn, and finally put it into the static press for static pressure sealing and set aside.

[0045] Comparative Example

[0046] A conventional aqueous zinc ion battery

[0047] Preparation of 2.3 mol / L pure zinc sulfate electrolyte: Dissolve 33.072 g zinc sulfate heptahydrate in 50 mL deionized water, stir and dissolve at room temperature to prepare a comparative electrolyte for standby use.

[0048] Composition of aqueous zinc ion battery:

[0049] (1) An aqueous zinc ion asymmetric battery is assembled using zinc foil as the negative electrode, copper foil as the positive electrode, and glass fiber as the separator;

[0050] (2) Using zinc foil as positive and negative electrodes and glass fiber as separator to assemble aqueous zinc ion symmetric battery;

[0051] (3) Using zinc foil as the negative electrode, glass fiber as the separator, and polyaniline (PANI) as the active material loaded on titanium foil as the positive electrode, an aqueous zinc ion full battery was assembled;

[0052] The electrolyte used was the prepared pure zinc sulfate electrolyte, with a usage of 0.1 mL.

[0053] The specific steps are as follows:

[0054] S1. Preparation of polyaniline positive electrode material: 0.365 mL of aniline monomer was added to 15 mL of HCl (1 M) solution in an ice bath. After stirring for 1 h, 5 mL of HCl (1 M) containing 0.228 g of ammonium persulfate was added dropwise to the above solution. After a few minutes, the colorless solution turned dark green. After the reaction was stirred for 1 h, the green precipitate was collected and washed several times with deionized water and ethanol, and then dried in vacuo at 60 ° C for 12 h. Finally, the obtained polyaniline powder was collected.

[0055] S2. Preparation of polyaniline positive electrode: polyaniline: acetylene black: PTFE = 7:2:1 by mass ratio are mixed and stirred to form a slurry, coated on the surface of titanium foil, placed in a vacuum drying oven at 130°C for 12 hours, and the electrode is taken out after drying and set aside.

[0056] S3. Preparation of negative electrode sheet: Cut the uncontaminated zinc foil into negative electrode sheets with a diameter of 12 mm, clean them with anhydrous ethanol ultrasonically, put them into an oven for drying, take out the electrode sheets after drying and set them aside for use.

[0057] S4. Preparation of glass fiber diaphragm: Cut the uncontaminated glass fiber diaphragm into discs with a diameter of 16 mm.

[0058] S5. Assembly of aqueous zinc ion batteries: First, place the zinc foil on the negative electrode shell side, then place the diaphragm in turn, add 0.1 mL of electrolyte to wet the diaphragm, then place the copper foil (Zn / / Cu asymmetric battery), zinc foil (Zn / / Zn symmetric battery) and positive electrode sheet (Zn / / PANI full battery) in turn, then place the gasket, spring and positive electrode shell in turn, and finally put it into the static press for static pressure sealing and set aside.

[0059] The aqueous zinc ion batteries assembled using the examples and comparative examples were subjected to electrochemical tests under certain conditions.

[0060] (1) The coulombic efficiency test results of Zn / / Cu asymmetric battery at 25°C are as follows Figure 1 shown.

[0061] Zn / / Cu battery using pure zinc sulfate electrolyte at 1mA / cm 2 , 1mAh / cm 2 The coulombic efficiency showed obvious fluctuations after 70 cycles under the test conditions, indicating that in pure zinc sulfate electrolyte, the coulombic efficiency was low and unstable due to the formation of dendrites, significant hydrogen evolution reaction and severe corrosion of the zinc negative electrode, which led to battery failure.

[0062] Zn / / Cu battery using multi-component electrolyte at 1 mA / cm 2 , 1mAh / cm 2 Under the test conditions, it can cycle 1420 times, and the average coulombic efficiency reaches more than 99%. Compared with pure zinc sulfate electrolyte, multi-component electrolyte can effectively inhibit dendrite growth, limit hydrogen evolution reaction and avoid corrosion of zinc negative electrode, improve the reversibility of battery plating / stripping, and improve coulombic efficiency and cycle performance.

[0063] (2) The time-voltage curve test results of Zn / / Zn symmetrical battery at 25°C are as follows Figure 2 shown.

[0064] Zn / / Zn battery using pure zinc sulfate electrolyte at 1 mA / cm 2 , 1mAh / cm 2 Under the test conditions, the cycle life is only 100h, after which a short circuit occurs and the polarization voltage is 40mV, indicating that in the pure zinc sulfate electrolyte, there is obvious dendrite formation, which pierces the diaphragm and causes the battery to short circuit.

[0065] Zn / / Zn battery using multi-component electrolyte at 1 mA / cm 2 , 1mAh / cm 2 Under the test conditions, it can cycle stably for 1220 hours with a polarization voltage of 42mV, showing a more stable voltage and longer cycle life. Thanks to the dendrite-free zinc deposition, the limitation of hydrogen evolution reaction and the weakening of zinc negative electrode corrosion, the cycle life of the battery is significantly increased.

[0066] (3) Zn / / Cu asymmetric battery at 25°C, current density 1 mA / cm 2 and 1mAh / cm 2 The scanning electron microscope image of the zinc negative electrode after 50 cycles under the conditions is shown in the figure.

[0067] The zinc negative electrode using pure zinc sulfate electrolyte is Figure 3 As shown in (a), a large number of dendrites are generated on the surface, which has suffered severe corrosion, with many broken zinc deposits and an uneven surface.

[0068] Zinc anode using multi-component electrolytes such as Figure 3 As shown in (b), it presents a flat, dense, uniform and dendrite-free surface without corrosion, showing a uniform and ordered zinc deposition morphology, which can effectively improve the electrochemical performance of zinc-ion batteries.

[0069] (4) The long cycle performance test results of Zn / / PANI full battery at 25°C with a charge and discharge current density of 1A / g are as follows: Figure 4 shown.

[0070] The battery using pure zinc sulfate electrolyte has a short cycle life and fails after 300 cycles, with a capacity retention rate of only 72%.

[0071] The coulombic efficiency of the multi-component mixed electrolyte is above 99%, and it can be stably cycled for more than 2,000 cycles with a capacity retention rate of 83%. The mixed electrolyte effectively improves the cycle performance and life of the entire battery, increases the capacity attenuation rate, and achieves a higher performance zinc-ion battery.

[0072] (5) The coulombic efficiency test results of Zn / / Cu asymmetric battery at -20℃ are as follows Figure 5 shown.

[0073] Zn / / Cu battery using pure zinc sulfate electrolyte at 1mA / cm 2 , 1mAh / cm 2 It cannot operate under the test conditions and the battery is invalid.

[0074] Zn / / Cu battery using multi-component electrolyte at 1 mA / cm2 , 1mAh / cm 2 Under the test conditions, it can stably cycle 700 times, with a coulombic efficiency of 99.9%. It also has good zinc ion plating / stripping reversibility under low temperature conditions, and can effectively inhibit dendrite growth, hydrogen evolution reaction and negative electrode corrosion, broadening the operating conditions of zinc ion batteries and further improving the reversibility and electrochemical performance of zinc ion batteries.

[0075] The invention discloses preparation and application of a wide temperature range high-stability high-entropy aqueous zinc ion battery electrolyte. The electrolyte can promote uniform deposition of zinc ions to avoid generation of zinc dendrites, improve coulombic efficiency and cycle performance of a zinc negative electrode, and improve electrochemical performance of the zinc ion battery; can effectively inhibit hydrogen evolution reaction, corrosion and dissolution of the zinc negative electrode, avoid battery expansion problems, and improve battery safety and cycle life; can improve the capacity attenuation rate of the zinc ion battery and increase the battery capacity by improving the reaction kinetics of the battery; the electrolyte has good stability and a low freezing point, so that the battery can operate under low temperature conditions of -20°C, has good low temperature performance, and broadens the operating conditions of the zinc ion battery; the electrolyte has a simple preparation process and strong operability, and has good application prospects in the field of aqueous zinc ion batteries.

[0076] Finally, it should be noted that the above embodiments are only used to illustrate the technical solution of the present invention rather than to limit it. Although the present invention has been described in detail with reference to the preferred embodiments, those skilled in the art should understand that they can still modify or replace the technical solution of the present invention with equivalents, and these modifications or equivalent replacements cannot cause the modified technical solution to deviate from the spirit and scope of the technical solution of the present invention.

Claims

1. A method for preparing a wide temperature range, high stability, high entropy aqueous zinc ion battery electrolyte, characterized in that: The steps include: S1. Dissolve zinc sulfate in ethylene glycol, and stir and dissolve at room temperature to prepare electrolyte A; S2, dissolving zinc trifluoromethanesulfonate in deionized water, stirring and dissolving at room temperature to prepare electrolyte B; S3, dissolving zinc chloride in dimethyl sulfoxide, stirring and dissolving at room temperature to prepare electrolyte C; S4. A wide temperature range, high stability, and high entropy aqueous zinc ion battery electrolyte is prepared according to the volume ratio of electrolyte A: electrolyte B: electrolyte C of 2:2:

1.

2. The method for preparing a wide temperature range, high stability and high entropy aqueous zinc ion battery electrolyte according to claim 1, characterized in that: In step S1, the concentration of electrolyte A is 2 mol / L.

3. The method for preparing a wide temperature range, high stability and high entropy aqueous zinc ion battery electrolyte according to claim 1, characterized in that: In step S2, the concentration of electrolyte B is 3 mol / L.

4. The method for preparing a wide temperature range, high stability and high entropy aqueous zinc ion battery electrolyte according to claim 1, characterized in that: In step S3, the concentration of the electrolyte C is 2 mol / L.

5. A wide temperature range, high stability, high entropy aqueous zinc ion battery electrolyte prepared by the method for preparing a wide temperature range, high stability, high entropy aqueous zinc ion battery electrolyte as described in any one of claims 1 to 4.

6. Use of the wide temperature range, high stability, high entropy aqueous zinc ion battery electrolyte as claimed in claim 5 in the preparation of aqueous zinc ion batteries.

Citation Information

Patent Citations

  • Aqueous zinc ion battery electrolyte capable of protecting vanadium-containing compound positive electrode and application of aqueous zinc ion battery electrolyte

    CN113097576A

  • Electrolyte for aqueous zinc-based battery as well as preparation and application of electrolyte

    CN116565346A

  • Additive for aqueous zinc ion battery electrolyte and application

    CN117996232A

Cited By

  • Electrolysis process based on high-entropy electrolyte and application of electrolysis process

    CN120844150A

  • Preparation method of electrolyte suitable for manganese-zinc secondary battery

    CN121260955A