Antibacterial degradable calcium phosphate bone cement and preparation method thereof
By combining strontium copper-doped β-tricalcium phosphate powder with tetracalcium phosphate and anhydrous calcium hydrogen phosphate powder, an antibacterial degradable calcium phosphate bone cement was prepared, which solved the mismatch of the existing bone cement degradation rate with human bones and The lack of antibacterial ability has achieved bone tissue regeneration and angiogenesis, and has significant clinical application prospects.
Patent Information
- Application Number
- CN202411079414.8
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-08-07
- Publication Date
- 2024-11-15
- Estimated Expiration
- 2044-08-07
AI Technical Summary
The degradation rate of existing calcium phosphate bone cement does not match human bones and lacks antibacterial ability. It has problems with antibiotic toxicity and bacterial resistance, which affects the mechanical properties of bone cement.
Using strontium copper-doped β-tricalcium phosphate powder combined with tetracalcium phosphate and anhydrous calcium hydrogen phosphate powder, an antibacterial degradable calcium phosphate bone cement, strontium ion To promote bone formation, copper ions have antibacterial effects and control the degradation rate by regulating the strontium doping/copper content and calcium strontium copper/phosphorus ratio.
It achieves the degradation rate matching human bones, and has antibacterial, biocompatible and high mechanical properties, which can promote bone tissue regeneration and angiogenesis, avoid the toxicity problem of traditional antibiotic-doped bone cement, and has significant clinical application prospects.
Smart Images

Figure CN118949126A_ABST
Abstract
Description
Technical Field
[0001] The invention belongs to the technical field of production and preparation of biomedical materials, and specifically relates to an antibacterial and degradable calcium phosphate bone cement and a preparation method thereof. Background Art
[0002] Osteoporosis is one of the most common bone diseases, characterized by bone loss and destruction of bone microstructure, leading to increased bone brittleness and increased risk of fractures. There is a huge demand for bone repair materials clinically. Calcium Phosphate Cement (CPC) is one of the most promising injectable bone repair materials. CPC solid phase is a mixture of one or more calcium phosphate powders, while CPC liquid phase is usually water or aqueous solution. CPC solid phase and liquid phase are blended into a paste in a certain proportion. The paste can be arbitrarily shaped and has certain mechanical properties, and a curing reaction can occur when implanted in the body. It can be used for the repair of bone defects, but there are obvious disadvantages in actual use, mainly including degradation rate that does not match human bones and lack of antibacterial ability. Therefore, it is very important to develop calcium phosphate cement with antibacterial properties and regulated degradation rate.
[0003] A Chinese patent (application number: 202310966230.2, publication number: CN116870250A) discloses an antibacterial bone cement composed of three parts: powder, antibiotics and liquid, and a preparation method thereof. Antibiotics are physically doped into non-leaching furan-based bone cement to develop a dual-functional antibacterial bone cement that combines non-releasable and releasable antibacterial properties. However, bone cement with added antibiotics has problems with antibiotic toxicity and bacterial resistance, and will affect the mechanical properties of bone cement. Summary of the invention
[0004] In order to solve the problems existing in the prior art, the purpose of the present invention is to provide an antibacterial and degradable calcium phosphate bone cement and a preparation method thereof. The degradation rate of the bone cement of the present invention matches well with that of human bones, and it also has the characteristics of antibacterial, good biocompatibility and good mechanical properties. This bone cement product will have good application prospects in the field of orthopedics.
[0005] To achieve the above purpose, the technical solution adopted by the present invention is as follows:
[0006] An antibacterial and degradable calcium phosphate bone cement, the raw materials of which include a solid phase powder component and a solidifying liquid, wherein the solid-liquid ratio of the solid phase powder component to the solidifying liquid is 0.7 g: (330 μL to 360 μL);
[0007] The solid phase powder component includes tetracalcium phosphate powder, anhydrous calcium hydrogen phosphate powder and strontium copper doped β-tricalcium phosphate powder, wherein the molar ratio of the tetracalcium phosphate powder to the anhydrous calcium hydrogen phosphate powder is 1:1, and the mass ratio of the sum of the mass of the tetracalcium phosphate powder and the anhydrous calcium hydrogen phosphate powder to the mass of the strontium copper doped β-tricalcium phosphate powder is (7-9):(1-3).
[0008] Preferably, the particle size of the tetracalcium phosphate powder ranges from 0.1 μm to 100 μm.
[0009] Preferably, the particle size of the anhydrous calcium hydrogen phosphate powder ranges from 0.2 μm to 10 μm.
[0010] Preferably, the particle size of the strontium copper doped β-tricalcium phosphate powder is in the range of 0.2 μm to 10 μm.
[0011] Preferably, the solidifying liquid is a phosphoric acid aqueous solution with a concentration of 0.5 to 1 mol / L.
[0012] More preferably, the concentration of the phosphoric acid aqueous solution is 0.75 mol / L.
[0013] Preferably, in the strontium-copper doped β-tricalcium phosphate powder, the molar amount of strontium (ie, n(Sr)) accounts for 2% to 8% of the total molar amount of calcium, strontium and copper (ie, n(Ca+Sr+Cu)).
[0014] Preferably, the molar amount of copper (ie, n(Cu)) accounts for 2% to 8% of the total molar amount of calcium, strontium and copper (ie, n(Ca+Sr+Cu)).
[0015] Preferably, the total molar amount of strontium and copper (ie, n(Sr+Cu)) accounts for no more than 10% of the total molar amount of calcium, strontium and copper (ie, n(Ca+Sr+Cu)).
[0016] The method for preparing the antibacterial degradable calcium phosphate bone cement of the present invention comprises:
[0017] The solid phase powder component and the solidifying liquid are blended to form a bone cement slurry;
[0018] The bone cement slurry is solidified to form the antibacterial and degradable calcium phosphate bone cement.
[0019] Preferably, when the bone cement slurry is solidified:
[0020] Pre-curing the bone cement slurry in an environment of 36-37° C. and a relative humidity of 75% to 100% for 30 minutes to 2 hours to obtain a pre-cured molded body;
[0021] The pre-cured molded body is then finally cured in the use environment of the antibacterial and degradable calcium phosphate bone cement.
[0022] The present invention has the following beneficial effects:
[0023] The antibacterial and degradable calcium phosphate bone cement of the present invention is a strontium-copper ion-doped biphasic calcium phosphate bioactive bone cement. The present invention adopts strontium-copper doped β-tricalcium phosphate powder, in which the strontium contained can stimulate bone formation and reduce bone absorption. For osteoblasts, Sr promotes the proliferation and differentiation of mesenchymal stem cells into osteoblasts by promoting gene expression, and promotes bone formation through the action of osteoblasts; for osteoclasts, Sr promotes the expression of osteoprotegerin (OPG) gene to increase the content of osteoprotegerin, and osteoprotegerin can not only inhibit the differentiation and maturation of osteoclasts, but also accelerate the apoptosis of osteoclasts, thereby reducing bone absorption. The copper ions contained in the strontium-copper doped β-tricalcium phosphate powder of the present invention can be used as angiogenic agents and antibacterial agents. The antibacterial mechanism of copper ions mainly includes the following four aspects: ① The positively charged copper ions are adsorbed on the negatively charged bacterial outer membrane through electrostatic action, disrupting the normal metabolism of bacteria and causing metabolic disorders and death; ② The copper ions penetrate the cell membrane and enter the bacteria, causing cytoplasmic extravasation and death; ③ The copper ions destroy the activity of the respiratory chain, reduce energy generation, and thus affect the replication of bacterial genes and cause bacterial death; ④ The copper ions can produce peroxide-like reactive oxygen species (ROS), killing bacteria through oxidative stress reactions. Appropriate concentrations of copper ions have the effect of stimulating the proliferation and differentiation of endothelial cells, and by simulating hypoxia, stabilizing the structure of hypoxia-inducible factor, upregulating the expression of angiogenesis-related factors such as vascular endothelial growth factor, promoting angiogenesis, and then promoting osteogenesis. Its biodegradation rate can not only be regulated according to the relative content of the two phases in the solidified product, the amount of strontium / copper, and the molar ratio of strontium copper / phosphorus, but also is higher than the degradation rate of single-phase apatite bone cement, giving bone cement the ability to resist bacteria and induce angiogenesis while maintaining high mechanical properties. It can be seen that the antibacterial degradable calcium phosphate bone cement of the present invention has the characteristics of antibacterial and good biocompatibility. Through experiments, the antibacterial degradable calcium phosphate bone cement of the present invention has high and long-term stable mechanical properties, suitable setting time, adjustable strontium / copper content and calcium strontium copper / phosphorus ratio, controllable degradation rate, and can slowly release strontium copper ions that promote bone tissue regeneration, induce angiogenesis, and are antibacterial. Compared with traditional single-phase calcium phosphate bone cement doped with antibiotics, it has significant advantages and is expected to be more widely used in clinical practice. BRIEF DESCRIPTION OF THE DRAWINGS
[0024] Figure 1 This is a sample picture of the antibacterial and degradable calcium phosphate bone cement obtained in Example 1 of the present invention after solidification;
[0025] Figure 2 is the XRD spectrum of the samples obtained in Examples 1 to 3 of the present invention after curing for 3 days;
[0026] FIG3(a) is a microscopic morphology of the sample obtained in Example 1 of the present invention after curing for 3 days; FIG3(b) is a microscopic morphology of the sample obtained in Example 2 of the present invention after curing for 3 days; FIG3(c) is a microscopic morphology of the sample obtained in Example 3 of the present invention after curing for 3 days;
[0027] Figure 4 Schematic diagram of the in vitro degradation rate of the cured samples obtained in Examples 1 to 3 of the present invention and the comparative example;
[0028] Figure 5 It is a schematic diagram of the amount of strontium ions released when the samples obtained in Examples 1 to 3 of the present invention are immersed in a phosphate buffer solution for different days;
[0029] Figure 6 It is a schematic diagram of the copper ion release of the samples obtained in Examples 1 to 3 of the present invention when immersed in a phosphate buffer solution for different days;
[0030] Figure 7 It is the compressive strength of the samples obtained in Examples 1 to 3 of the present invention after curing for 3 days.
[0031] Figure 8 It is the compressive strength of the samples obtained in Examples 4 to 6 of the present invention after curing for 3 days.
[0032] Fig. 9 It is the compressive strength of the samples obtained in Examples 7 to 9 of the present invention after curing for 3 days. DETAILED DESCRIPTION
[0033] The technical solution of the present invention is further described below in conjunction with the accompanying drawings and embodiments.
[0034] The present invention adds tricalcium phosphate doped with strontium and copper into the solid powder of bone cement, and regulates the degradation rate by adjusting the amount of tricalcium phosphate added and the amount of ion doping, thereby ensuring that the bone cement has good biocompatibility while also having good antibacterial property and bone induction.
[0035] The specific scheme of the present invention is as follows:
[0036] The raw materials of the antibacterial and degradable calcium phosphate bone cement of the present invention include solid-phase powder components and solidifying liquid, wherein the solid-phase powder components include tetracalcium phosphate (TTCP) powder, anhydrous calcium hydrogen phosphate powder (DCPA) and strontium copper-doped beta-tricalcium phosphate powder (referred to as (Sr / Cu)-β-TCP); the solidifying liquid is a dilute phosphoric acid aqueous solution with a concentration w of 0.5 to 1 mol / L.
[0037] In the above scheme of the present invention, the amount of dilute phosphoric acid aqueous solution required for solidifying liquid per 0.7g solid phase powder component is in the range of 330μL to 360μL. The particle size of TTCP powder is in the range of 0.1μm to 100μm. The particle size of DCPA powder is in the range of 0.2μm to 10μm. The particle size range of ((Sr / Cu)-β-TCP powder is 0.2μm~10μm. The molar ratio of TTCP to DCPA is 1:1. The mass ratio of the total mass of TTCP and DCPA powder to the mass ratio of ((Sr / Cu)-β-TCP powder is (7~9):(1~3). In the strontium-copper doped β-tricalcium phosphate powder, the strontium doping n(Sr) / n(Ca+Sr+Cu) is 2%~8%, the copper doping n(Cu) / n(Ca+Sr+Cu) is 2%~8%, and the total doping n(Sr+Cu) / n(Ca+Sr+Cu) of strontium and copper does not exceed 10%. The raw material proportions of tricalcium phosphate with different strontium and copper contents are shown in Table 1.
[0038] Table 1
[0039]
[0040] The method for preparing the antibacterial degradable calcium phosphate bone cement of the present invention comprises:
[0041] The solid phase powder component and the solidifying liquid are blended to form a bone cement slurry;
[0042] The bone cement slurry is pre-cured and molded in an environment of 36-37° C. and a relative humidity of 75% to 100% for 30 minutes to 2 hours to obtain a pre-cured molded body, and then finally cured in a use environment to form the antibacterial and degradable calcium phosphate bone cement of the present invention.
[0043] Embodiment 1:
[0044] The preparation method of the antibacterial degradable calcium phosphate bone cement of this embodiment comprises the following steps:
[0045] (1) Mixing the solid phase original powders, weighing TTCP and DCPA powders with a molar ratio of 1:1, mixing them evenly and recording them as TD, and weighing TD powder and 8Sr2Cu-TCP powder with a mass ratio of 8:2, mixing them evenly as the solid phase powder component.
[0046] (2) Weigh 0.7 g of the solid powder component and 340 μL of 0.75 M dilute phosphoric acid aqueous solution, and mix with a spatula for 30 seconds to form a uniform bone cement slurry.
[0047] Embodiment 2:
[0048] The preparation method of the antibacterial degradable calcium phosphate bone cement of this embodiment comprises the following steps:
[0049] (1) Mixing the solid phase original powders, weighing TTCP and DCPA powders with a molar ratio of 1:1, mixing them evenly and recording them as TD, and weighing TD powder and 5Sr5Cu-TCP powder with a mass ratio of 8:2, mixing them evenly as the solid phase powder component.
[0050] (2) Weigh 0.7 g of the solid powder component and 340 μL of 0.75 M dilute phosphoric acid aqueous solution, and mix with a spatula for 30 seconds to form a uniform bone cement slurry.
[0051] Embodiment 3:
[0052] The preparation method of the antibacterial degradable calcium phosphate bone cement of this embodiment comprises the following steps:
[0053] (1) Mixing the solid phase original powders, weighing TTCP and DCPA powders with a molar ratio of 1:1, mixing them evenly and recording them as TD, and weighing TD powder and 5Sr5Cu-TCP powder with a mass ratio of 8:2, mixing them evenly as the solid phase powder component.
[0054] (2) Weigh 0.7 g of the solid powder component and 350 μL of 0.75 M dilute phosphoric acid aqueous solution, and mix with a spatula for 30 seconds to form a uniform bone cement slurry.
[0055] Embodiment 4:
[0056] The preparation method of the antibacterial degradable calcium phosphate bone cement of this embodiment comprises the following steps:
[0057] (1) Mixing the solid phase original powders, weighing TTCP and DCPA powders with a molar ratio of 1:1, mixing them evenly and recording them as TD, and then weighing TD powder and 8Sr2Cu-TCP powder with a mass ratio of 9:1, mixing them evenly as the solid phase powder component.
[0058] (2) Weigh 0.7 g of the solid powder component and 330 μL of 1 M dilute phosphoric acid aqueous solution, and mix with a spatula for 30 seconds to form a uniform bone cement slurry.
[0059] Embodiment 5:
[0060] The preparation method of the antibacterial degradable calcium phosphate bone cement of this embodiment comprises the following steps:
[0061] (1) Mixing the solid phase original powders, weighing TTCP and DCPA powders with a molar ratio of 1:1, mixing them evenly and recording them as TD, and then weighing TD powder and 5Sr5Cu-TCP powder with a mass ratio of 9:1, mixing them evenly as the solid phase powder component.
[0062] (2) Weigh 0.7 g of the solid powder component and 330 μL of 1 M dilute phosphoric acid aqueous solution, and mix with a spatula for 30 seconds to form a uniform bone cement slurry.
[0063] Embodiment 6:
[0064] The preparation method of the antibacterial degradable calcium phosphate bone cement of this embodiment comprises the following steps:
[0065] (1) Mixing the solid phase original powders, weighing TTCP and DCPA powders with a molar ratio of 1:1, mixing them evenly and recording them as TD, and weighing TD powder and 2Sr8Cu-TCP powder with a mass ratio of 9:1, mixing them evenly as the solid phase powder component.
[0066] (1) Weigh 0.7 g of the solid powder component and 330 μL of 1 M dilute phosphoric acid aqueous solution, and mix with a spatula for 30 seconds to form a uniform bone cement slurry.
[0067] Embodiment 7:
[0068] The preparation method of the antibacterial degradable calcium phosphate bone cement of this embodiment comprises the following steps:
[0069] (1) Mixing the solid phase original powders, weighing TTCP and DCPA powders with a molar ratio of 1:1, mixing them evenly and recording them as TD, and weighing TD powder and 8Sr2Cu-TCP powder with a mass ratio of 7:3, mixing them evenly as the solid phase powder component.
[0070] (2) Weigh 0.7 g of the solid powder component and 360 μL of 0.5 M dilute phosphoric acid aqueous solution, and mix with a spatula for 30 seconds to form a uniform bone cement slurry.
[0071] Embodiment 8:
[0072] The preparation method of the antibacterial degradable calcium phosphate bone cement of this embodiment comprises the following steps:
[0073] (1) Mixing the solid phase original powders, weighing TTCP and DCPA powders with a molar ratio of 1:1, mixing them evenly and recording them as TD, and weighing TD powder and 5Sr5Cu-TCP powder with a mass ratio of 7:3, mixing them evenly as the solid phase powder component.
[0074] (2) Weigh 0.7 g of the solid powder component and 360 μL of 0.5 M dilute phosphoric acid aqueous solution, and mix with a spatula for 30 seconds to form a uniform bone cement slurry.
[0075] Embodiment 9:
[0076] The preparation method of the antibacterial degradable calcium phosphate bone cement of this embodiment comprises the following steps:
[0077] (1) Mixing the solid phase original powders, weighing TTCP and DCPA powders with a molar ratio of 1:1, mixing them evenly and recording them as TD, and weighing TD powder and 2Sr8Cu-TCP powder with a mass ratio of 7:3, mixing them evenly as the solid phase powder component.
[0078] (2) Weigh 0.7 g of the solid powder component and 360 μL of 0.5 M dilute phosphoric acid aqueous solution, and mix with a spatula for 30 seconds to form a uniform bone cement slurry.
[0079] Comparative Example
[0080] The preparation method of the bone cement of this comparative example comprises the following steps:
[0081] (1) Mixing the solid phase original powders, weighing TTCP and DCPA powders with a molar ratio of 1:1, mixing them evenly and recording them as TD, and weighing TD powder and β-TCP powder with a mass ratio of 8:2, mixing them evenly as the solid phase powder component.
[0082] (2) Weigh 0.7 g of solid powder and 330 μL of 0.75 M dilute phosphoric acid aqueous solution, and mix with a spatula for 30 seconds to form a uniform bone cement slurry.
[0083] The bone cement slurries of Examples 1 to 9 and the comparative example were respectively filled into a stainless steel cylindrical mold with a diameter of 6 mm and a height of 12 mm and compacted under a pressure of 2 kg. The prepared cylindrical samples were inserted into a glass tube with a diameter of 6.5 mm and a height of 13 mm, and then placed in an environment with a temperature of 36 to 37° C. and a relative humidity of 100% for curing. After pre-curing for 30 minutes, the samples were taken out and quickly immersed in SBF simulated body fluid for curing. The four bone cements were tested for physical and chemical properties and in vitro degradation experiments.
[0084] According to the present invention and specific embodiments, the effect is illustrated as shown in the figure:
[0085] Figure 1 This is a schematic diagram of the sample obtained after curing in Example 1. It can be seen that the sample is intact after curing, and the surface is smooth and undamaged, indicating that the bone cement of the present invention has good mechanical strength. Figure 2 This is the X-ray diffraction pattern after curing for 3 days. Figure 2 It can be seen that the solidification product is mainly composed of tricalcium phosphate and hydroxyapatite. Figure 3(a) to Figure 3(c) The SEM image of the cured product shows that hydroxyapatite is formed.
[0086] In order to evaluate the in vitro degradation of composite bone cement, the cured cylindrical samples were dried and weighed, and the initial weight was recorded as m0. They were immersed in phosphate buffer solution (PBS, pH = 7.40), and the ratio of the surface area of the sample to the volume of the degradation solution was 0.2 g / mL. The centrifuge tube containing the sample and the degradation solution was placed in an oven at 37°C. The samples were taken out every week for a total of 4 weeks. When the samples were collected, they were thoroughly washed and dried with deionized water and ethanol. The PBS solution was changed once a week. The degradation rate was evaluated by measuring the change in mass at different immersion times. Specifically, the samples were taken out from the solution and dried to constant weight at 65°C in a vacuum oven. The weight loss rate of the material in PBS is calculated as follows: where m0 is the original weight of the sample, m t It is the mass after degradation. Each group of samples is tested at least 3 times.
[0087]
[0088] like Figure 4 The figure shows the in vitro degradation rate of the embodiment and the comparative example. It can be seen from the figure that ion doping can effectively increase the degradation rate of cement. In order to further study the release law of ions in composite cement, the release of strontium and copper ions of bone cement in PBS degradation solution was detected by inductively coupled plasma atomic emission spectrometry (ICP). Figure 5 and Figure 6 The figure shows the cumulative release of strontium ions and copper ions. It can be seen that as the number of immersion days increases, the cumulative ion release increases linearly and can be released continuously.
[0089] Figure 7 The compressive strength of the sample after curing for 3 days is between 36 and 45 MPa, and the compressive strength of the bone cement is good. Figure 8 The compressive strength of the samples of Examples 4 to 6 after three days of curing is 28-35Mpa. Fig. 9 This is the compressive strength of the samples of Examples 7 to 9 after three days of curing. The strength is 26-33 Mpa, and all the samples have a certain strength.
[0090] It can be seen from the above scheme that the raw material system of the antibacterial and degradable bioactive bone cement prepared by the present invention is simple, consisting of only three-phase powder, the ion content can be regulated, the degradation rate can be controlled, and the special pharmacological strontium and copper ions can be slowly released without toxic side effects. While maintaining the strength of the cement, it has degradability, dual bioactive ion stimulation to accelerate early angiogenesis and bone regeneration, and the antibacterial properties of CPC are expected to be applied to the clinical treatment of bone defects.
[0091] The above description is only a preferred embodiment of the present invention and is not intended to limit the present invention. Any modifications, equivalent substitutions, improvements, etc. made within the spirit and principle of the present invention should be included in the protection scope of the present invention.
Claims
1. An antibacterial and degradable calcium phosphate bone cement, characterized in that: The raw materials include a solid phase powder component and a solidified liquid, and the solid-liquid ratio of the solid phase powder component to the solidified liquid is 0.7g:(330μL-360μL); The solid phase powder component includes tetracalcium phosphate powder, anhydrous calcium hydrogen phosphate powder and strontium copper doped β-tricalcium phosphate powder, wherein the molar ratio of the tetracalcium phosphate powder to the anhydrous calcium hydrogen phosphate powder is 1:1, and the mass ratio of the sum of the mass of the tetracalcium phosphate powder and the anhydrous calcium hydrogen phosphate powder to the mass of the strontium copper doped β-tricalcium phosphate powder is (7-9):(1-3).
2. An antibacterial and degradable calcium phosphate bone cement according to claim 1, characterized in that: The particle size of the tetracalcium phosphate powder ranges from 0.1 μm to 100 μm.
3. The antibacterial and degradable calcium phosphate bone cement according to claim 1, characterized in that: The particle size of the anhydrous calcium hydrogen phosphate powder ranges from 0.2 μm to 10 μm.
4. The antibacterial and degradable calcium phosphate bone cement according to claim 1, characterized in that: The particle size of the strontium copper doped beta-tricalcium phosphate powder ranges from 0.2 μm to 10 μm.
5. The antibacterial and degradable calcium phosphate bone cement according to claim 1, characterized in that: The solidifying liquid is a phosphoric acid aqueous solution with a concentration of 0.5 to 1 mol / L.
6. The antibacterial and degradable calcium phosphate bone cement according to claim 1, characterized in that: In the strontium-copper doped beta-tricalcium phosphate powder, the molar amount of strontium accounts for 2% to 8% of the total molar amount of calcium, strontium and copper.
7. The antibacterial and degradable calcium phosphate bone cement according to claim 1, characterized in that: In the strontium-copper doped beta-tricalcium phosphate powder, the molar amount of copper accounts for 2% to 8% of the total molar amount of calcium, strontium and copper.
8. An antibacterial and degradable calcium phosphate bone cement according to claim 6 or 7, characterized in that: In the strontium-copper doped beta-tricalcium phosphate powder, the total molar amount of strontium and copper accounts for no more than 10% of the total molar amount of calcium, strontium and copper.
9. The method for preparing the antibacterial degradable calcium phosphate bone cement according to any one of claims 1 to 8, characterized in that: include: The solid phase powder component and the solidifying liquid are blended to form a bone cement slurry; The bone cement slurry is solidified to form the antibacterial and degradable calcium phosphate bone cement.
10. The method for preparing the antibacterial and degradable calcium phosphate bone cement according to claim 9, characterized in that: When the bone cement slurry is cured: Pre-curing the bone cement slurry in an environment of 36-37° C. and 75%-100% relative humidity for 30 minutes-2 hours to obtain a pre-cured molded body; The pre-cured molded body is then finally cured in the use environment of the antibacterial and degradable calcium phosphate bone cement.
Citation Information
Patent Citations
Process for preparing degradable strontium-doped biphasic calcium phosphate bioactive bone cement
CN101444638A
Composite biological material capable of injecting bioglass-calcium phosphate bone cement and preparation
CN103143063A
Calcium phosphate-based bone cement with antibacterial property and preparation method thereof
CN104857568A
Preparation method of calcium phosphate bone cement simultaneously releasing zinc ions and silicate ions
CN105311680A
Tricalcium phosphate bone cement added with various inorganic ion doped hydroxyapatite and preparation method of tricalcium phosphate bone cement