Modified foamy copper porous material and application thereof in enhanced oil removal

By electrochemically modifying the foam copper material, an oil-philic and hydrophobic porous ball structure is formed, combined with the synergistic effect of air bubbles, the problem of poor oil absorption effect of existing oil removal materials is solved, and efficient and economical oil-water separation is achieved, and in petroleum Reusable oil removal solutions are provided in chemical industry.

CN118949909APending Publication Date: 2024-11-15EAST CHINA UNIV OF SCI & TECH
View PDF 7 Cites 0 Cited by

Patent Information

Application Number
CN202410313056.6
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-03-19
Publication Date
2024-11-15

AI Technical Summary

Technical Problem

Existing oil-removing materials lack the problem of poor oil absorption effect, low separation efficiency, non-reusable and prone to secondary pollution to the environment, especially when dealing with oil-containing sewage in petrochemicals, there is a lack of cost-effective solutions.

Method used

By electrochemically modifying the foam copper material, an oleophilic and hydrophobic porous ball structure is formed. The synergistic effect of the spherical structure and bubbles is used to achieve efficient adsorption and separation of oil droplets, and the oil absorption rate is enhanced through rotation, and the material can be reused.

Benefits of technology

It achieves efficient, economical and reusable oil-water separation, improves oil absorption and oil absorption rate, avoids environmental pollution, and is suitable for long-term or repeated oil removal scenarios.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118949909A_ABST
    Figure CN118949909A_ABST
Patent Text Reader

Abstract

The invention relates to a modified foamy copper porous material and application thereof in enhanced oil removal, the material is a porous ball made of porous foamy copper modified by a surface electrochemical roughening method, the particle size range of the material is 10-35 mm, the aperture range is 0.1-2 mm, the porosity is greater than 80%, and the through hole rate is greater than 90%. The oil-water separation is enhanced through the synergistic effect of the porous structure and the bubbles. After the porous material is immersed in an oil-water mixture, the porous material is filled with bubbles, oil drops are adsorbed and stored in the porous material, and oil-water separation is realized. The porous ball has extremely strong oil removal performance and has a good application prospect in the field of oily sewage treatment.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to a modified foam copper porous material and application thereof in enhanced oil removal, belonging to the field of oily wastewater treatment in petrochemical industry. Background Art

[0002] With the rapid development of industrialization in the fields of petrochemicals, oil pollution has become a global environmental problem. The treatment of oil spills, industrial leaks and oil pollution in daily life urgently requires efficient and economical solutions. Based on the actual needs of environmental governance and resource utilization of pollutants, the development of new, efficient and environmentally friendly methods for removing trace oil from oily wastewater has become a research hotspot in the field of water governance today, with huge environmental value, economic benefits and industrial significance.

[0003] As part of the development of oil removal methods, the development of oil removal materials is of great significance for solving the problem of oil pollution. At present, although some oleophilic polymer fibers can achieve the adsorption and separation of oil droplets from oil-water mixtures, they usually have problems such as poor oil absorption effect, low separation efficiency, non-reusability and easy secondary pollution to the environment. The hydrophobic / oleophilic surface with extreme wettability obtained by modification method as a separation medium provides an efficient and convenient solution to the problem of oily wastewater separation. In addition, porous materials have high specific surface area and adjustable pore structure, which can provide sufficient space to adsorb, separate and store a large amount of oil substances, making them ideal oil adsorption and separation treatment materials. Some natural porous oil-absorbing materials (such as cotton, wool, natural sponges, etc.) have a small oil absorption capacity, absorb water while absorbing oil, and are easily eroded by microorganisms, so they are not suitable for long-term use. Some artificial porous materials (such as graphene and carbon nanotubes, etc.) have extremely high oil absorption efficiency and rate, and can be reused many times after cleaning, but the manufacturing cost is extremely high.

[0004] Foam metal is a metal material with a porous structure. Compared with other porous materials, foam metal has the advantages of high strength, high porosity, low manufacturing cost and strong reusability. However, due to the influence of its surface properties and structure, it usually exhibits oleophobicity in water, and its oil absorption capacity and oil absorption rate are poor, but its surface has the characteristics of being easy to process. Therefore, based on the copper mesh metal mesh matrix, its oleophilicity in water can be enhanced by surface treatment (such as coating with a modified coating or chemical modification), so that it can show a good oil-water separation effect in water. This provides an efficient and convenient solution for solving the separation and collection problems of oily wastewater and developing economical, high oil absorption, high oil absorption rate and reusable oil removal materials and methods. Summary of the invention

[0005] The purpose of the present invention is to overcome the deficiencies in the prior art and provide a modified copper foam porous material and its application in enhanced oil removal to solve the problems mentioned in the above background.

[0006] The technical solution adopted by the present invention is as follows:

[0007] A modified copper foam porous material, characterized in that the material is a modified copper foam porous ball with a spherical particle size of 10-35 mm, and is prepared by the following steps:

[0008] (1) Pretreatment of copper foam: After cutting the copper foam material into a spherical shape, ultrasonic cleaning is performed in acetone, anhydrous ethanol and deionized water for 10-15 min in sequence;

[0009] (2) Electrochemical roughening of the surface of copper foam: 2-3 g of palmitic acid is dissolved in 100 ml of ethanol. The copper foam obtained in step (1) is used as an anode and an aluminum sheet of the same size is used as a cathode. The copper foam is inserted into the palmitic acid ethanol solution and electrochemically oxidized for 10-30 min at room temperature with an electrode spacing of 2-5 cm and a voltage of 5-10 V. The copper foam is taken out and washed with anhydrous ethanol, placed in a vacuum drying oven, and dried at 50-70° C. for 15-30 min to obtain an oleophilic and hydrophobic modified copper foam porous material.

[0010] Preferably, the porous material has a bulk density of 0.1-1 g / cm 3 , porous balls with a porosity greater than 80%, a through-porosity greater than 90%, and a pore size of 0.1-2mm.

[0011] The present invention also provides an application of a modified copper foam porous material in enhanced oil removal, characterized in that the application method is as follows:

[0012] (a) vibrating or rotating the porous material in air to allow air to enter the internal pores of the porous material;

[0013] (b) slowly and steadily immersing the porous material into the oil-water mixture to lock sufficient bubbles inside the pores;

[0014] (c) When the oil-water mixture contacts the porous material, the oil droplets are adsorbed by the porous material and stored inside the material;

[0015] (d) After the porous material absorbs the oil droplets, the bubbles detach from the top of the porous material, causing a pressure difference inside the sphere, which further induces the oil droplets to be adsorbed and stored inside the porous material until the porous material is saturated with adsorption;

[0016] (e) After the porous material adsorbs oil droplets to saturation, its surface is covered with tiny bubbles, which continue to contact with the oil droplets. The tiny oil droplets are adsorbed and aggregated on the surface of the porous material, and eventually grow into large droplets that are easier to separate, and slide off the surface of the porous ball, thereby achieving the separation of oil droplets in oily wastewater.

[0017] Preferably, in the step c), after the oil-water mixture contacts the porous material, the porous material is rotated at a speed of 600-1000 r / min.

[0018] Since the porous spherical structure of the copper foam porous ball has a much greater affinity for oil droplets than for bubbles, the oil absorption and separation performance of the modified porous ball is further enhanced under the induction factor of bubble overflow as pressure drive, so that it can efficiently absorb oil droplets in the oil-water mixture and can be reused. After cleaning or other regeneration treatment, its original oil absorption performance can be maintained unchanged. When the porous ball rotates at a speed of 600-1000r / min, the existence of the cyclonic field can further enhance the oil absorption process and increase the oil absorption rate of the porous ball.

[0019] Beneficial Effects

[0020] The main advantages of the present invention are:

[0021] 1. Use porous balls made of modified copper foam as degreasing materials.

[0022] Copper foam has the characteristics of high porosity, high strength, excellent durability and chemical stability, low manufacturing cost, and strong reusability. After being modified by electrochemical methods, it has super oleophilic and super hydrophobic properties and can retain the relevant properties of the original copper foam. Therefore, the modified copper foam material has unique advantages in oil removal applications in the field of oil-water separation, and is especially suitable for scenarios that require long-term or repeated removal of oil stains.

[0023] 2. Utilize the synergistic effect of porous spherical structure and bubbles to develop a new and efficient oil removal method.

[0024] When the oil-water mixture contacts the surface of the porous material, the porous spherical structure has a much greater affinity for oil droplets than for bubbles. Therefore, with the bubble overflow as the pressure-driven induction factor, the porous sphere can achieve efficient adsorption of oil droplets from the oil-water mixture. At the same time, the tiny pores inside the porous material are like a large number of tiny capillaries, and the oil droplets have a lower surface tension than water. Therefore, under the influence of capillary action, oil droplets are more easily attracted into the pores of the porous structure than water. At the same time, the bubbles locked inside the pores of the porous material can also be regarded as "captures" for oil droplets. The bubbles in the porous structure can effectively increase the surface area of ​​the oil droplets in contact with the porous material, so that more oil droplets are absorbed into the porous material, and the oil droplets coalesce inside, reducing the difficulty of oil absorption and increasing the amount of oil absorption. This type of capture effect is particularly significant in porous foam metal materials, which is attributed to the high porosity and through-porosity of such materials. The capture effect of bubbles and the adsorption effect of porous materials work together to effectively enhance the oil absorption performance of the material. When the oil droplets are absorbed into the porous material, the surface of the porous material is wetted by the oil film, which can enhance its lipophilicity and further increase the oil absorption rate.

[0025] Here, the porous material does not hinder the movement of bubbles while adsorbing oil droplets. As the oil droplets are adsorbed, the fluidity of water in the porous structure increases, and the air density in the bubbles is much lower than the density of water and oil. Therefore, under the combined influence of their own buoyancy and the push of water, the bubbles move upward and eventually detach from the porous ball, creating a pressure difference with the overflow of the bubbles, so that the porous ball can adsorb oil droplets more efficiently. BRIEF DESCRIPTION OF THE DRAWINGS

[0026] The accompanying drawings are used to provide a further understanding of the present invention. They only constitute a part of this specification to further explain the present invention, and do not constitute a limitation of the present invention.

[0027] Figure 1 Schematic diagram of the modified copper foam porous material and degreasing method of the present invention;

[0028] Figure 2 The device diagram for realizing oil-water separation of the present invention: 1-image processing system, 2-high-speed camera, 3-rotating device, 4-modified foam copper porous ball, 5-needle tube, 6-oil-water separation tank, 7-LED lamp, 8-syringe pump;

[0029] Figure 3 It is a diagram of the oil removal process of the bubble synergistically enhanced modified foam copper porous ball in the present invention; DETAILED DESCRIPTION

[0030] The following will be combined with the drawings in the embodiments of the present invention to clearly and completely describe the technical solutions in the embodiments of the present invention. Obviously, the described embodiments are only some embodiments of the present invention, not all embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.

[0031] Embodiment 1:

[0032] A porous copper foam ball with a diameter of 30 mm, a pore size of 1.2 mm, a porosity of 85%, and a through-porosity of 95% was modified, and cleaned with acetone and ethanol in an ultrasonic environment for 10 minutes, and then the treated copper foam ball was used as an anode, and an aluminum sheet of the same size was used as a cathode, and inserted into a 0.1 mol / L palmitic acid ethanol solution with a spacing of 2 cm between the plates, and anodized for 15 minutes at a voltage of 10 V; after the reaction, the copper foam ball was taken out and repeatedly rinsed with anhydrous ethanol; finally, it was placed in a vacuum drying oven and dried at 60°C for 20 minutes to obtain an oleophilic and hydrophobic copper foam porous ball material. Figure 2 As shown, the modified copper foam porous ball is connected to a stainless steel rod with a diameter of 5mm, and the porous ball is vibrated or rotated in the air to facilitate air to enter its internal pores; then, the porous ball is slowly and steadily immersed below the surface of the oil-water mixture in the water tank, and sufficient bubbles are locked inside the ball; a 0.4mm diameter needle is placed under the water tank, facing the center of the porous ball, and the needle is connected to the injection pump, and silicone oil droplets with a viscosity of 500mPa·s are generated through the needle and injected into the water tank. Figure 3 As shown, after the silicone oil droplets contact the modified porous ball, they will enter the interior of the porous ball. At the same time, the bubbles will detach from the top of the sphere to generate pressure drive, further enhancing the oil removal process. After the modified porous ball under this modification condition absorbs a total of 0.75 ml of silicone oil, the porous ball reaches the oil absorption saturation state, indicating that the modified porous ball has excellent oil removal performance for silicone oil-water mixture.

[0033] In addition, the porous balls were taken out of the water tank, washed with ethanol solution, and the experiment was repeated. The deoiling results remained basically unchanged, proving that the prepared porous balls have excellent reusability.

[0034] Embodiment 2:

[0035] A porous foam copper ball with a diameter of 30 mm, a pore size of 0.9 mm, a porosity of 85% and a through-porosity of 90% was modified, and was cleaned in an ultrasonic environment for 10 minutes using acetone and ethanol in turn. The treated foam copper ball was then used as an anode and an aluminum sheet of the same size was used as a cathode. The anode was inserted into a 0.1 mol / L palmitic acid ethanol solution with a spacing of 3 cm between the plates, and an anodized treatment was performed at a voltage of 5 V for 20 minutes. After the reaction was completed, the foam copper ball was taken out and repeatedly rinsed with anhydrous ethanol. Finally, it was placed in a vacuum drying oven and dried at 60°C for 20 minutes to obtain an oleophilic and hydrophobic foam copper porous ball material. The modified porous ball is placed below the liquid surface of the oil-water mixture in a water tank. A 0.4 mm diameter syringe is placed under the water tank, facing the center of the porous ball. The syringe is connected to a syringe pump. Silicone oil droplets with a viscosity of 500 mPa·s are generated through the syringe and injected into the water tank. After the silicone oil droplets contact the modified porous ball, they will enter the porous ball. At the same time, bubbles detach from the top of the sphere to generate pressure drive, further enhancing the oil removal process. After the modified porous ball under this modification condition absorbs a total of 0.66 ml of silicone oil, the porous ball reaches an oil absorption saturation state, indicating that the modified porous ball has a good oil removal performance for the silicone oil-water mixture.

[0036] Embodiment 3:

[0037] A porous copper foam ball with a diameter of 30 mm, a pore size of 1 mm, a porosity of 90% and a through-porosity of 95% was modified, and was cleaned in an ultrasonic environment for 10 minutes using acetone and ethanol in turn. The treated copper foam ball was then used as an anode and an aluminum sheet of the same size was used as a cathode. The anode was inserted into a 0.15 mol / L palmitic acid ethanol solution with a spacing of 2.5 cm between the plates, and anodization was performed at a voltage of 10 V for 15 minutes. After the reaction was completed, the copper foam ball was taken out and repeatedly rinsed with anhydrous ethanol. Finally, it was placed in a vacuum drying oven and dried at 60°C for 20 minutes to obtain an oleophilic and hydrophobic copper foam porous ball material. The modified porous ball is connected to a stainless steel rod with a diameter of 5 mm, and the porous ball is vibrated or rotated in the air to facilitate air to enter its internal pores; then, the porous ball is slowly and steadily immersed in a water tank below the liquid surface of the oil-water mixture, and sufficient bubbles are locked inside the ball; after the ball is completely immersed in the oil-water mixture, a slight vibration is applied to the water to induce more air to be trapped in the pores of the porous ball; a 1.6 mm diameter syringe is placed under the water tank directly opposite the center of the porous ball, and the syringe is connected to a syringe pump. Isooctane oil droplets with a viscosity of 0.479 mPa·s are generated through the syringe and injected into the water tank. When the isooctane oil droplets contact the porous ball, the isooctane oil droplets are adsorbed by the porous material into the porous ball and stored inside the ball, and the bubbles detach from the top of the porous ball. After a total of 0.99 ml of isooctane is inhaled, the porous ball reaches an oil absorption saturation state, indicating that this modified foam copper ball and method can separate oil from water in the isooctane oil-water mixture.

[0038] In addition, when the isooctane oil droplets contacted the porous ball, the motor drove the connecting rod to make the modified porous ball rotate at a speed of 600r / min. The modified porous ball reached the oil absorption saturation state only after absorbing 1.47ml of isooctane. Compared with the rotation speed of 0, the oil absorption amount and oil absorption rate of the porous ball increased significantly, indicating that the rotation of the porous ball can further enhance the oil-water separation of the isooctane oil-water mixture.

Claims

1. A modified copper foam porous material, characterized in that: The material is a modified copper foam porous ball with a spherical particle size of 10-35 mm, which is prepared by the following steps: (1) Pretreatment of copper foam: After cutting the copper foam material into a spherical shape, ultrasonic cleaning is performed in acetone, anhydrous ethanol and deionized water for 10-15 min in sequence; (2) Electrochemical roughening of the surface of copper foam: 2-3 g of palmitic acid is dissolved in 100 ml of ethanol. The copper foam obtained in step (1) is used as an anode and an aluminum sheet of the same size is used as a cathode. The copper foam is inserted into the palmitic acid ethanol solution and electrochemically oxidized for 10-30 min at room temperature with an electrode spacing of 2-5 cm and a voltage of 5-10 V. The copper foam is taken out and washed with anhydrous ethanol, placed in a vacuum drying oven, and dried at 50-70° C. for 15-30 min to obtain an oleophilic and hydrophobic modified copper foam porous material.

2. The modified copper foam porous material according to claim 1, characterized in that: The porous material has a bulk density of 0.1-1 g / cm 3 , porous balls with a porosity greater than 80%, a through-porosity greater than 90%, and a pore size of 0.1-2mm.

3. Use of the porous material according to claim 1 in enhanced oil removal, characterized in that: The application method is as follows: (a) vibrating or rotating the porous material in air to allow air to enter the internal pores of the porous material; (b) slowly and steadily immersing the porous material into the oil-water mixture to lock sufficient bubbles inside the pores; (c) When the oil-water mixture contacts the porous material, the oil droplets are adsorbed by the porous material and stored inside the material; (d) After the porous material absorbs the oil droplets, the bubbles detach from the top of the porous material, causing a pressure difference inside the sphere, which further induces the oil droplets to be adsorbed and stored inside the porous material until the porous material is saturated with adsorption; (e) After the porous material adsorbs oil droplets to saturation, its surface will be covered with tiny bubbles. As the bubbles continue to contact the oil droplets, the tiny oil droplets will be adsorbed and aggregated on the surface of the porous material, eventually growing into larger droplets that are easier to separate and sliding off the surface of the porous ball, thus achieving the separation of oil droplets in oily wastewater.

4. The use of the porous material according to claim 3 in enhanced oil removal, characterized in that: In the step (c), after the oil-water mixture contacts the porous material, the porous material is rotated at a speed of 600-1000 r / min.

Citation Information

Patent Citations

  • Preparation of super-hydrophobic surface for metal anti-corrosive and self-cleaning effects

    CN101440510A

  • Oil-water separation copper foam and preparation method thereof

    CN103088227A

  • Method for preparing hydrophobic lipophilic cotton fabric material through structuring zinc oxide fine structure

    CN103343446A

  • Foamy copper with controllable wettability as well as preparation method and multifunctional oil-water separating method of foamy copper

    CN104264209A

  • Preparation method of durable super-hydrophobic super-oleophylic foamy copper for oil and water separation

    CN104888498A