Novel pyrrhotite ore collecting agent

By optimizing the distribution formula and preparation process of the new pyrite ore collector, the problems of low harvesting efficiency, poor selectivity, large usage and large environmental impact in the existing technology are solved, and high efficiency, strong selectivity and environmental protection are achieved The mineral harvesting effect is suitable for large-scale industrial applications.

CN118950270AActive Publication Date: 2024-11-15SICHUAN LIWU COPPER IND +1
View PDF 5 Cites 0 Cited by

Patent Information

Application Number
CN202411133223.5
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-08-19
Publication Date
2024-11-15
Estimated Expiration
2044-08-19

AI Technical Summary

Technical Problem

The existing pyrite collectors have shortcomings in terms of low collection efficiency, poor selectivity, large usage, large environmental impact and complex process, resulting in low mineral recovery, reduced concentrate purity, high production costs and environmental pollution problems. .

Method used

Using the new pyrite ore collector, through improved group distribution formula and preparation process, including thiol-based collectors, amide-based collectors, surfactants, organic solvents, auxiliary capture agents and pH regulators, combined with The stirring and water addition steps optimize the formula and process of the collector, improve the harvesting efficiency and selectivity, reduce dosage and environmental pollution, and simplify the preparation process.

Benefits of technology

It significantly improves the harvesting efficiency and selectivity of pyrite, reduces the amount of collector, reduces environmental pollution, simplifies the preparation process, improves the ore recovery rate and concentrate purity, reduces production costs, and is suitable for industrialization. Large-scale application.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118950270A_ABST
    Figure CN118950270A_ABST
Patent Text Reader

Abstract

The invention relates to the field of mineral processing, and discloses a novel pyrrhotite ore collecting agent which comprises 5-30 parts of a thiol-based collecting agent, 5-30 parts of an amide-based collecting agent, 2-10 parts of a surfactant, 20-50 parts of an organic solvent, 20-60 parts of water, 1-15 parts of a collecting aid and 1-10 parts of a pH regulator. According to the method, the thiol-based collecting agent and the amide-based collecting agent are introduced into the collecting agent, and efficient collecting of pyrrhotite is achieved. The collecting agent molecules have high affinity with active sites on the surface of pyrrhotite, so that the collecting efficiency of minerals is greatly improved, the technical purpose of remarkably improving the ore recovery rate is achieved, meanwhile, amphiphilic molecules are adopted as surfactants, including an anionic surfactant and a cationic surfactant, and the amphiphilic molecules can be used as the surfactants, so that the recovery rate of the minerals is greatly improved. The surfactants can effectively adjust the properties of the surfaces of the minerals, and selective separation of the pyrrhotite and other impurity minerals is achieved.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the technical field of mineral processing, in particular to a novel pyrrhotite collector. Background Art

[0002] Pyrrhotite is an iron-containing sulfide mineral that is widely found in various mineral deposits and is often used as an important raw material for extracting elements such as iron and sulfur. However, due to the complex existence of pyrrhotite in the ore, it is usually accompanied by other impurity minerals such as pyrite and quartz. Therefore, in the process of mineral processing, an effective collector is needed to achieve efficient and selective separation of pyrrhotite. However, the existing collector technology has shortcomings in many aspects.

[0003] Deficiencies of existing technology:

[0004] Low collection efficiency: Existing pyrrhotite collectors have significant deficiencies in collection efficiency, resulting in low mineral recovery rates. Traditional collectors have insufficient binding force with pyrrhotite and are unable to fully capture active sites on the mineral surface, which affects the flotation effect of the mineral. Inefficient collection not only wastes resources, but also reduces production efficiency.

[0005] Poor selectivity: The collectors currently used have poor selectivity and are difficult to effectively distinguish pyrrhotite from other associated minerals. Due to the low selectivity of the collector, impurity minerals are captured together during the flotation process, reducing the purity of the pyrrhotite concentrate. This poor selectivity complicates the subsequent purification process and increases the separation cost.

[0006] Large dosage: The use of traditional collectors requires a large dosage to achieve the desired effect. This not only increases production costs, but also has an adverse effect on subsequent tailings treatment. The large-scale use of chemical collectors may also cause environmental pollution problems and affect the ecological environment of the mining area. High dosage of collectors may also increase equipment wear and maintenance costs.

[0007] Large environmental impact: Many existing collectors contain chemical components that are harmful to the environment and can easily cause water and soil pollution during use. With the increasing environmental protection requirements, finding low-toxic and environmentally friendly collectors has become an important task in the mineral processing industry. Traditional collectors may release harmful substances during use and processing, posing a threat to the surrounding ecosystem and human health.

[0008] Complex process: The preparation and use of traditional collectors are relatively complicated, requiring multi-step reactions and strict condition control, which increases the difficulty and cost of operation and is not conducive to large-scale industrial application. The complex process not only reduces production efficiency, but also may lead to unstable process parameters and affect the consistency of product quality.

[0009] Therefore, the present invention proposes a novel pyrrhotite collector to solve the deficiencies of the prior art. Summary of the invention

[0010] In view of the shortcomings of the prior art, the present invention provides a novel pyrrhotite collector, which aims to solve the shortcomings of the existing pyrrhotite collectors in terms of low collection efficiency, poor selectivity, large dosage, large environmental impact and complex process, and provides a novel pyrrhotite collector. The collector achieves efficient and selective collection of pyrrhotite by improving the component formula and preparation process, while reducing the dosage and environmental pollution, simplifying the preparation process, and is suitable for large-scale industrial applications.

[0011] To achieve the above objectives, the present invention is implemented by the following technical scheme: a new type of pyrrhotite collector, the collector comprising the following components by weight:

[0012] Mercaptan-based collector: 5-30 parts;

[0013] Amide collector: 5-30 parts;

[0014] Surfactant: 2-10 parts;

[0015] Organic solvent: 20-50 parts;

[0016] Water: 20-60 parts;

[0017] Trapping aid: 1-15 parts;

[0018] pH adjuster: 1-10 parts.

[0019] Preferably, the specific structural formula of the thiol-based collector is R-SH, wherein R is a C8-C18 alkyl or aryl group.

[0020] Preferably, the specific structural formula of the amide collector is R-CONH2, wherein R is a C8-C18 alkyl or aryl group.

[0021] Preferably, the surfactant is an amphiphilic molecule, including one or more of anionic surfactants and cationic surfactants, and the surfactant includes sodium dodecyl sulfate and quaternary ammonium salt compounds.

[0022] Preferably, the organic solvent is an alcohol solvent, and the alcohol solvent is one or more of ethanol, n-butanol and isopropanol.

[0023] Preferably, the trapping aid is a fatty acid salt or a xanthate, and the trapping aid includes sodium dodecyl sulfate or ethoxylated alkylphenol.

[0024] Preferably, the pH regulator is one or more of sodium carbonate, sodium bicarbonate or sodium hydroxide.

[0025] Preferably, a method for preparing a novel pyrrhotite collector comprises the following steps:

[0026] (1) dissolving a thiol-based collector and an amide-based collector in an organic solvent according to a ratio and stirring uniformly;

[0027] (2) Add surfactant and capture aid and continue stirring until dissolved;

[0028] (3) gradually adding water to the mixed solution obtained in step (2), adding a pH adjuster, and stirring evenly to obtain the collector.

[0029] Preferably, the stirring temperature in step (1) is 20-40° C., and the stirring time is 10-30 minutes; and the stirring temperature in step (2) is 20-30° C., and the stirring time is 5-20 minutes.

[0030] Preferably, the speed of adding water in step (3) is 5-10 ml per minute, and the water is kept uniformly dispersed during the stirring process; the pH value of the process of adding the pH regulator in step (3) is controlled to be between 7 and 9 to optimize the effect of the collector.

[0031] Preferably, the order of adding the organic solvent in step (1) is to first add ethanol, then add n-butanol and isopropanol in sequence, and stir until dissolved after each addition.

[0032] Preferably, the order of adding the organic solvent in step (1) is to first add ethanol, then add n-butanol and isopropanol in sequence, and stir until dissolved after each addition.

[0033] The present invention provides a novel pyrrhotite collector having the following beneficial effects:

[0034] 1. The present invention achieves efficient capture of pyrrhotite by introducing a thiol-based collector and an amide-based collector into the collector. These collector molecules have a high affinity with the active sites on the surface of pyrrhotite, thereby greatly improving the capture efficiency of the mineral and achieving the technical purpose of significantly improving the ore recovery rate.

[0035] 2. The present invention uses amphiphilic molecules as surfactants, including anionic surfactants and cationic surfactants, which can effectively adjust the properties of the mineral surface and achieve the selective separation of pyrrhotite and other impurity minerals. By improving the selectivity of the target mineral in the flotation process, the technical purpose of improving the purity and recovery quality of the mineral is achieved.

[0036] 3. The present invention adds a collecting aid, such as sodium dodecyl sulfate or ethoxylated alkylphenol, which can significantly enhance the collecting performance of the main collector, so that the collector can still maintain a high working effect at a lower concentration, thereby achieving the technical purpose of reducing the amount of collector, reducing production costs and improving economic benefits.

[0037] 4. The present invention selects environmentally friendly organic solvents such as ethanol, n-butanol and isopropanol to replace the traditional environmentally harmful solvents. These organic solvents not only meet the requirements of collectors in terms of performance, but also can reduce environmental pollution during use, achieving the technical purpose of realizing environmentally friendly collectors and meeting the requirements of green mine construction. BRIEF DESCRIPTION OF THE DRAWINGS

[0038] Figure 1 The present invention is a flow chart of the preparation method of a new type of pyrrhotite collector. DETAILED DESCRIPTION

[0039] The following will be combined with the drawings in the specification of the present invention to clearly and completely describe the technical solutions in the embodiments of the present invention. Obviously, the described embodiments are only part of the embodiments of the present invention, not all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.

[0040] Example:

[0041] Please see attached Figure 1 :

[0042] Example 1: Flotation of high sulfide content ores

[0043] step:

[0044] Dissolve the collector: Dissolve 15 parts of thiol collector (R-SH, where R is a C8-C18 alkyl or aryl group) and 20 parts of amide collector (R-CONH2, where R is a C8-C18 alkyl or aryl group) in 30 parts of ethanol. Stir evenly, control the temperature at 25°C, and stir for 20 minutes to ensure that the collector is completely dissolved and evenly distributed.

[0045] Add surfactant and trapping aid: Add 5 parts of anionic surfactant sodium dodecyl sulfate and 8 parts of ethoxylated alkylphenol. Continue stirring until completely dissolved, control the temperature at 25°C, and stir for 10 minutes. Surfactants can reduce interfacial tension, and trapping aids can improve capture efficiency.

[0046] Add water and adjust pH: gradually add 40 parts of water to the mixed solution obtained in step (2), and add 5 parts of sodium carbonate at the same time, and stir evenly. Add water at a rate of 7 ml per minute to maintain uniform dispersion and control the pH value at 8.5. Sodium carbonate is used as a pH regulator to optimize the flotation environment.

[0047] Summary: This embodiment is suitable for processing ores with high sulfide content. By optimizing the formula of collector and collector aid, the flotation efficiency and selectivity are improved, the mixing of impurity minerals is reduced, and the concentrate grade is improved.

[0048] Example 2: Flotation of low-grade ores

[0049] step:

[0050] Dissolve the collector: Dissolve 10 parts of thiol-based collector and 10 parts of amide-based collector in 40 parts of isopropanol. Stir evenly, control the temperature at 30°C, and stir for 15 minutes. Isopropanol, as an organic solvent, can effectively dissolve and disperse the collector.

[0051] Add surfactant and collector aid: Add 3 parts of cationic surfactant quaternary ammonium salt compound and 5 parts of sodium dodecyl sulfate. Continue stirring until completely dissolved, control the temperature at 25°C, and stir for 10 minutes. Surfactants can enhance the adsorption capacity of collectors on the mineral surface.

[0052] Add water and adjust pH: gradually add 50 parts of water to the mixed solution obtained in step (2), and add 8 parts of sodium bicarbonate at the same time, and stir evenly. Add water at a rate of 8 ml per minute, and control the pH value at 8. Sodium bicarbonate adjusts the pH value of the pulp and provides a suitable flotation environment.

[0053] Summary: This embodiment is suitable for low-grade ores. By adjusting the formula of the collector and the collector aid, the recovery rate of the low-grade ore in the flotation process is improved, and the valuable minerals in the ore are effectively extracted.

[0054] Example 3: Flotation of iron ore

[0055] step:

[0056] Dissolve the collector: Dissolve 20 parts of thiol-based collector and 25 parts of amide-based collector in 25 parts of n-butanol. Stir evenly, control the temperature at 35°C, and stir for 25 minutes. n-Butanol, as an organic solvent, can provide good solubility and stability.

[0057] Add surfactant and collector aid: add 7 parts of sodium dodecyl sulfate and 10 parts of ethoxylated alkylphenol. Continue stirring until completely dissolved, control the temperature at 30°C, and stir for 15 minutes. The collector aid improves the collector's collection performance.

[0058] Add water and adjust pH: gradually add 30 parts of water to the mixed solution obtained in step (2), and add 6 parts of sodium hydroxide at the same time, and stir evenly. Add water at a rate of 9 ml per minute, and control the pH value at 9. Sodium hydroxide adjusts the pH value to ensure the optimal activity of the collector.

[0059] Summary: This embodiment is suitable for the flotation of iron ore. By optimizing the formula of collector and collector aid and selecting a suitable organic solvent, the flotation efficiency and selectivity are improved, and the mineral recovery rate and concentrate grade are significantly improved.

[0060] Example 4: Flotation of fine ore

[0061] step:

[0062] Dissolve the collector: Dissolve 5 parts of thiol-based collector and 5 parts of amide-based collector in 50 parts of ethanol. Stir evenly, control the temperature at 20°C, and stir for 10 minutes. Ethanol, as an organic solvent, can provide good solubility and dispersion effects.

[0063] Add surfactant and trapping aid: Add 2 parts of sodium dodecyl sulfate and 4 parts of quaternary ammonium salt compounds. Continue stirring until completely dissolved, control the temperature at 25°C, and stir for 10 minutes. The combination of surfactant and trapping aid can significantly improve the capture capacity of fine-grained minerals.

[0064] Add water and adjust pH: gradually add 60 parts of water to the mixed solution obtained in step (2), and add 4 parts of sodium carbonate at the same time, and stir evenly. Add water at a rate of 10 ml per minute, and control the pH value at 8.5. Sodium carbonate adjusts the pH value to improve the stability of the collector and the flotation efficiency.

[0065] Summary: This embodiment is specially designed for fine-grained ores. Through the combination of high-concentration organic solvent and low-concentration collector, the capture capacity and separation effect of fine-grained minerals are improved, ensuring efficient flotation.

[0066] Example 5: Flotation of high oxide ores

[0067] step:

[0068] Dissolve the collector: Dissolve 25 parts of thiol-based collector and 30 parts of amide-based collector in 20 parts of n-butanol. Stir evenly, control the temperature at 40°C, and stir for 30 minutes. n-Butanol, as an organic solvent, can provide excellent dissolving properties.

[0069] Add surfactant and collector aid: Add 10 parts of sodium dodecyl sulfate and 15 parts of ethoxylated alkylphenol. Continue stirring until completely dissolved, control the temperature at 30°C, and stir for 20 minutes. The collector aid enhances the collector's collection performance.

[0070] Add water and adjust pH: gradually add 20 parts of water to the mixed solution obtained in step (2), and add 10 parts of sodium bicarbonate at the same time, and stir evenly. Add water at a rate of 5 ml per minute, and control the pH value at 7.5. Sodium bicarbonate adjusts the pH value to provide the best flotation environment.

[0071] Summary: This embodiment is suitable for high-oxide ores. Through the combination of high-concentration collectors and collector aids, the flotation efficiency and selectivity of oxide ores are improved, and the mineral recovery rate and concentrate purity are significantly improved.

[0072] Summary:

[0073] Through the above five different embodiments, the novel pyrrhotite collector of the present invention demonstrates wide applicability and high efficiency under different ore types and flotation conditions. Each embodiment significantly improves the capture efficiency and selectivity, optimizes the flotation process, reduces the dosage and environmental impact, and ensures the simplicity and efficiency of the preparation process by scientifically and rationally selecting and combining the collector, the trapping aid, the organic solvent and the pH regulator. These embodiments fully reflect the innovation and practicality of the present invention and provide a reliable and efficient solution for the field of mineral processing.

[0074] Comparative experiment:

[0075] Comparative experiment 1: Collection efficiency comparison

[0076] Existing technology:

[0077] Collector: Use traditional xanthate collector (such as sodium butyl xanthate) at a dosage of 20 parts.

[0078] pH adjuster: Use ammonium sulfate to adjust the pH to 8.0.

[0079] Experimental steps:

[0080] Slurry preparation: crush the ore to -74μm and adjust the slurry concentration to 30%.

[0081] Add collector: Add 20 parts of sodium butyl xanthate to the slurry and stir for 10 minutes.

[0082] Adjust pH: Add ammonium sulfate to adjust pH to 8.0 and continue stirring for 5 minutes.

[0083] Flotation: Flotation is performed and the froth product is collected, dried and weighed.

[0084] The present invention:

[0085] Collector: The novel pyrrhotite collector of the present invention is used, and the specific formula is as follows:

[0086] Mercaptan collector: 15 parts

[0087] Amide collector: 15 parts

[0088] Surfactant: 5 parts

[0089] Organic solvent (ethanol): 30 parts

[0090] Water: 40 parts

[0091] Trapping aid (sodium lauryl sulfate): 10 parts

[0092] pH adjuster (sodium carbonate): 5 parts

[0093] pH value is controlled at 8.5

[0094] Experimental steps:

[0095] Slurry preparation: crush the ore to -74μm and adjust the slurry concentration to 30%.

[0096] Add collector: Add the new collector to the slurry and stir for 15 minutes.

[0097] Adjust pH: Add sodium carbonate to adjust pH to 8.5 and continue stirring for 5 minutes.

[0098] Flotation: Flotation is performed and the froth product is collected, dried and weighed.

[0099] Experimental data table:

[0100]

[0101] Summary: The experimental results show that the ore recovery rate and mineral purity of the collector of the present invention are significantly higher than those of the collector of the prior art, while the flotation time is shorter and the production cost is lower, which proves the superiority of the present invention in terms of collection efficiency.

[0102] Contrast experiment 2: Selective contrast

[0103] Existing technology:

[0104] Collector: Use the traditional butyl xanthate collector, the amount of collector is 25 parts.

[0105] pH adjuster: Use sodium hydroxide to adjust the pH to 7.5.

[0106] Experimental steps:

[0107] Slurry preparation: crush the ore to -74μm and adjust the slurry concentration to 30%.

[0108] Add collector: Add 25 parts of sodium butyl xanthate to the slurry and stir for 10 minutes.

[0109] Adjust pH: Add sodium hydroxide to adjust pH to 7.5 and continue stirring for 5 minutes.

[0110] Flotation: Flotation is performed and the froth product is collected, dried and weighed.

[0111] The present invention:

[0112] Collector: The novel pyrrhotite collector of the present invention is used, and the specific formula is as follows:

[0113] Mercaptan collector: 20 parts

[0114] Amide collector: 10 parts

[0115] Surfactant: 4 parts

[0116] Organic solvent (n-butanol): 25 parts

[0117] Water: 30 parts

[0118] Trapping aid (ethoxylated alkylphenol): 8 parts

[0119] pH adjuster (sodium bicarbonate): 6 parts

[0120] pH value is controlled at 8.0

[0121] Experimental steps:

[0122] Slurry preparation: crush the ore to -74μm and adjust the slurry concentration to 30%.

[0123] Add collector: Add the new collector to the slurry and stir for 15 minutes.

[0124] Adjust pH: Add sodium bicarbonate to adjust pH to 8.0 and continue stirring for 5 minutes.

[0125] Flotation: Flotation is performed and the froth product is collected, dried and weighed.

[0126] Experimental data table:

[0127]

[0128] Summary: The experimental results show that the collector of the present invention has higher selectivity for pyrrhotite during the flotation process, significantly reduces the content of impurity minerals, significantly improves the purity of the minerals, and has lower production costs, demonstrating the obvious advantages of the present invention in terms of selectivity and economy.

[0129] Comparative experiment 3: Dosage comparison

[0130] Existing technology:

[0131] Collector: Use a traditional thiophosphate collector (such as dibutyl thiophosphate) at a dosage of 30 parts.

[0132] pH adjuster: Use sodium hydroxide to adjust the pH to 9.0.

[0133] Experimental steps:

[0134] Slurry preparation: crush the ore to -74μm and adjust the slurry concentration to 30%.

[0135] Add collector: Add 30 parts of dibutyl thiophosphate to the slurry and stir for 10 minutes.

[0136] Adjust pH: Add sodium hydroxide to adjust pH to 9.0 and continue stirring for 5 minutes.

[0137] Flotation: Flotation is performed and the froth product is collected, dried and weighed.

[0138] The present invention:

[0139] Collector: The novel pyrrhotite collector of the present invention is used, and the specific formula is as follows:

[0140] Mercaptan collector: 10 parts

[0141] Amide collector: 10 parts

[0142] Surfactant: 3 parts

[0143] Organic solvent (isopropanol): 40 parts

[0144] Water: 50 parts

[0145] Trapping aid (sodium lauryl sulfate): 7 parts

[0146] pH adjuster (sodium carbonate): 5 parts

[0147] pH value is controlled at 8.5

[0148] Experimental steps:

[0149] Slurry preparation: crush the ore to -74μm and adjust the slurry concentration to 30%.

[0150] Add collector: Add the new collector to the slurry and stir for 15 minutes.

[0151] Adjust pH: Add sodium carbonate to adjust pH to 8.5 and continue stirring for 5 minutes.

[0152] Flotation: Flotation is performed and the froth product is collected, dried and weighed.

[0153] Experimental data table:

[0154]

[0155] Summary: The experimental results show that the collector of the present invention can maintain a high ore recovery rate and mineral purity while significantly reducing the dosage, and the production cost is greatly reduced, which reflects the advantages of the present invention in terms of collector dosage and economic benefits.

[0156] Comparative experiment 4: Environmental protection comparison

[0157] Existing technology:

[0158] Collector: Use the traditional ethionine collector, the amount of collector is 20 parts. pH adjuster: Use sodium hydroxide to adjust the pH value to 8.0.

[0159] Experimental steps:

[0160] Slurry preparation: crush the ore to -74μm and adjust the slurry concentration to 30%.

[0161] Add collector: Add 20 parts of ethionine to the slurry and stir for 10 minutes. Adjust pH: Add sodium hydroxide to adjust pH to 8.0 and continue stirring for 5 minutes. Flotation: Perform flotation, collect the foam product, dry and weigh.

[0162] The present invention:

[0163] Collector: The novel pyrrhotite collector of the present invention is used, and the specific formula is as follows: Mercaptan-based collector: 10 parts

[0164] Amide collector: 10 parts

[0165] Surfactant: 3 parts

[0166] Organic solvent (n-butanol): 25 parts

[0167] Water: 35 parts

[0168] Trapping aid (ethoxylated alkylphenol): 8 parts

[0169] pH adjuster (sodium bicarbonate): 6 parts

[0170] pH value is controlled at 8.0

[0171] Experimental steps:

[0172] Slurry preparation: crush the ore to -74μm and adjust the slurry concentration to 30%.

[0173] Add collector: Add the new collector to the slurry and stir for 15 minutes.

[0174] Adjust pH: Add sodium bicarbonate to adjust pH to 8.0 and continue stirring for 5 minutes. Flotation: Perform flotation, collect the foam product, dry and weigh.

[0175] Experimental data table:

[0176]

[0177]

[0178] Summary: The experimental results show that the chemical oxygen demand (COD) and biochemical oxygen demand (BOD) generated by the collector of the present invention during use are significantly reduced, the toxicity of water bodies is reduced, and the production cost is lower, indicating that the present invention is superior to the existing technology in terms of environmental protection and economy, and reduces pollution to the environment.

[0179] Summary:

[0180] Through the above four comparative experiments, the novel pyrrhotite collector of the present invention demonstrates significant advantages in different aspects. The experimental results show that the present invention not only far exceeds the existing technology in terms of collection efficiency and selectivity, but also shows obvious superiority in reducing the amount of collector, reducing environmental pollution and simplifying the preparation process. The specific experimental data fully demonstrates the innovation and practicality of the present invention, and provides an efficient, environmentally friendly and economical solution for the field of mineral processing.

[0181] Although embodiments of the present invention have been shown and described, it will be appreciated by those skilled in the art that various changes, modifications, substitutions and variations may be made to the embodiments without departing from the principles and spirit of the present invention, and that the scope of the present invention is defined by the appended claims and their equivalents.

Claims

1. A new type of pyrrhotite collector, It is characterized in that The collector comprises the following components by weight: Mercaptan collector: 5-30 parts, wherein the specific structural formula of the mercaptan collector is R-SH, wherein R is a C8-C18 alkyl or aryl group; Amide collector: 5-30 parts, wherein the specific structural formula of the amide collector is R-CONH2, wherein R is a C8-C18 alkyl or aryl group; Surfactant: 2-10 parts, wherein the surfactant is an amphiphilic molecule, including one or more of anionic surfactants and cationic surfactants, and the surfactant includes sodium lauryl sulfate and quaternary ammonium salt compounds; Organic solvent: 20-50 parts, wherein the organic solvent is an alcohol solvent, and the alcohol solvent is one or more of ethanol, n-butanol and isopropanol; Water: 20-60 parts; Trapping aid: 1-15 parts; pH adjuster: 1-10 parts.

2. A novel pyrrhotite collector according to claim 1, It is characterized in that The trapping aid is a fatty acid salt or a xanthate, and the trapping aid includes sodium lauryl sulfate or ethoxylated alkylphenol.

3. A novel pyrrhotite collector according to claim 1, It is characterized in that The pH regulator is one or more of sodium carbonate, sodium bicarbonate or sodium hydroxide.

4. A method for preparing the novel pyrrhotite collector according to any one of claims 1 to 3, It is characterized in that The following steps are involved: (1) dissolving a thiol-based collector and an amide-based collector in an organic solvent according to a ratio and stirring uniformly; (2) Add surfactant and capture aid and continue stirring until dissolved; (3) gradually adding water to the mixed solution obtained in step (2), adding a pH adjuster, and stirring evenly to obtain the collector.

5. A method for preparing a novel pyrrhotite collector according to claim 8, It is characterized in that The stirring temperature in step (1) is 20-40° C. and the stirring time is 10-30 minutes; the stirring temperature in step (2) is 20-30° C. and the stirring time is 5-20 minutes.

6. A method for preparing a novel pyrrhotite collector according to claim 4, It is characterized in that The speed of adding water in step (3) is 5-10 ml per minute, and the water is kept evenly dispersed during the stirring process; the pH value of the process of adding the pH regulator in step (3) is controlled to be between 7 and 9.

7. A method for preparing a novel pyrrhotite collector according to claim 4, It is characterized in that The order of adding the organic solvent in step (1) is to first add ethanol, then add n-butanol and isopropanol in sequence, and stir until dissolved after each addition.

8. A method for preparing a novel pyrrhotite collector according to claim 4, It is characterized in that In the step (2), the order of adding the surfactant and the trapping aid is to first add the anionic surfactant, then add the cationic surfactant, and finally add the trapping aid, and stir evenly after each addition.

Citation Information

Patent Citations

  • Sulfide ore flotation combined reagent and method

    CN114042536A

  • Zinc sulfide flotation collector and application thereof

    CN115569739A

  • Pyrrhotite combined collecting agent and preparation method and application thereof

    CN118179751A

  • Process to treat ores and collector composition therefor

    EP3636346A1

  • Process to treat metal or mineral ores and collector composition therefor

    WO2018172307A1