Environment-friendly high-strength automobile roof and preparation method thereof

Through the multi-layer structure of environmentally friendly high-strength automobile ceiling, combined with toughened fiber felt and composite ethylene-vinyl acetate copolymer glue layer, the existing automobile ceiling materials emit harmful substances at high temperatures and the hazards during processing are solved, and the existing automobile ceiling materials are realized. High tear resistance and sound absorption performance reduce the VOC value in the car and keep the air in the car fresh.

CN118952771AActive Publication Date: 2024-11-15JINHUA HUAR AUTOMOBILE TRIMMING CO LTD
View PDF 5 Cites 0 Cited by

Patent Information

Application Number
CN202411034961.4
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-07-31
Publication Date
2024-11-15
Estimated Expiration
2044-07-31

AI Technical Summary

Technical Problem

Existing automotive ceiling materials are prone to emit harmful volatiles at high temperatures, affecting air quality, and the fine particles generated during processing are harmful to production personnel, and the material is not brittle enough, which limits its use.

Method used

The environmentally friendly high-strength automotive ceiling adopts a multi-layer structure, including non-woven fabric layer, toughened fiber felt and composite ethylene-vinyl acetate copolymer glue layer, improves the adhesion and tear resistance of materials through hot pressing and molding technology, and in Nanotitanium dioxide and activated carbon are added to the composite material to adsorb and degrade aldehydes.

Benefits of technology

It realizes a car ceiling with high tear resistance, good environmental protection and excellent sound absorption performance, avoids hazards during processing, reduces the VOC value in the car, keeps the air in the car fresh, and the material is lightweight.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118952771A_ABST
    Figure CN118952771A_ABST
Patent Text Reader

Abstract

The invention relates to the technical field of automobile interiors, and particularly discloses an environment-friendly high-strength automobile roof. The invention relates to a composite material which comprises a non-woven fabric layer, a first adhesive layer cast on the surface of the non-woven fabric layer, a first toughening fiber felt adhered to the surface of the first adhesive layer, a second adhesive layer cast on the surface of the first toughening fiber felt, a polyurethane base material adhered to the surface of the second adhesive layer, and a third adhesive layer cast on the surface of the polyurethane base material from bottom to top, the second toughening fiber felt is adhered to the surface of the third adhesive layer; the fourth adhesive layer is cast on the surface of the second toughening fiber felt; the first toughening fiber felt and the second toughening fiber felt are both made of toughening fibers; and the first adhesive layer, the second adhesive layer, the third adhesive layer and the fourth adhesive layer are all made of composite ethylene-vinyl acetate copolymer. The multi-layer structure of the automobile ceiling has the characteristics of tight bonding, interlayer separation prevention, good external rigidity and no deformation, and the automobile ceiling is excellent in sound absorption performance, odorless, safe and environment-friendly.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the technical field of automobile interior decoration, and in particular to an environmentally friendly high-strength automobile roof and a preparation method thereof. Background Art

[0002] China has become a major automobile production and sales country, with annual automobile production and sales exceeding 20 million vehicles. Although existing automobile roofs can basically meet the needs of the automobile industry, they also face the disadvantage that the materials cannot be recycled after being discarded, which will have a huge impact on the environment.

[0003] The car roof is a crucial component of the interior of the whole car. In addition to the interior decoration, it can also effectively insulate the car from heat and sound. The existing car roof is made of metal, with a painted surface and soft decoration inside. This type of car roof easily absorbs heat in summer, causing the temperature inside the car to rise quickly. The internal heat is not easy to dissipate, which increases the cost of using air conditioning during travel and is not conducive to environmental protection.

[0004] At the same time, with the development of society and the advancement of technology, people have put forward newer and higher requirements for car roofs. Polyurethane substrates have the properties of heat insulation, noise reduction, shock resistance, flame retardancy, aesthetics and practicality, and are currently widely used. However, when the temperature is high, the board is easy to emit harmful volatiles after being heated, affecting the air quality and interior environment of the driving room, and the product is relatively brittle, which limits its use.

[0005] Existing car roofs use composite fiber materials to improve the brittleness of polyurethane. Although the above composite materials can basically meet the needs of the automotive industry, there are fine particles generated during the processing that will cause certain harm to production personnel. Long-term exposure will cause diseases such as pneumoconiosis, which is irreversible.

[0006] How to prepare a car roof that is not only environmentally friendly but also has excellent rigidity and bending strength and excellent compressive strength is the current cutting-edge scientific research direction of car roofs. Summary of the invention

[0007] The purpose of the present invention is to solve the shortcomings of the prior art and to propose an environmentally friendly high-strength automobile roof and a preparation method thereof.

[0008] An environmentally friendly high-strength automobile roof comprises, from bottom to top: a non-woven fabric layer, a first adhesive layer cast on the surface of the non-woven fabric layer, a first toughened fiber felt bonded to the surface of the first adhesive layer, a second adhesive layer cast on the surface of the first toughened fiber felt, a polyurethane substrate bonded to the surface of the second adhesive layer, a third adhesive layer cast on the surface of the polyurethane substrate, a second toughened fiber felt bonded to the surface of the third adhesive layer, and a fourth adhesive layer cast on the surface of the second toughened fiber felt.

[0009] The materials used for the first toughened fiber felt and the second toughened fiber felt are both toughened fiber felts made of toughened fibers; and the materials used for the first adhesive layer, the second adhesive layer, the third adhesive layer and the fourth adhesive layer are all composite ethylene-vinyl acetate copolymer.

[0010] Preferably, the polyurethane substrate is prepared by the following specific operation: the polyether polyol is continuously stirred, and triethanolamine, catalyst, pore opening agent, foaming agent, water, silicone oil, and activated carbon fiber are added in sequence during the stirring process. After the addition is complete, stir at 5-15° C. for 10-20 minutes, then add toluene diisocyanate, adjust the temperature to 5-10° C., stir evenly, solidify, and cool.

[0011] Preferably, the molecular weight of the polyether polyol is 2500-3500 and the hydroxyl value is 25-30 mg KOH / g.

[0012] Preferably, the catalyst is dibutyltin dilaurate.

[0013] Preferably, the blowing agent is HFC-245fa (the main active ingredient is pentafluoropropane).

[0014] Preferably, the pore opening agent is at least one of Evonik O-501, Evonik O-500 and Meside AK9905.

[0015] Preferably, the mass ratio of polyether polyol, triethanolamine, catalyst, pore opener, foaming agent, water, silicone oil, activated carbon fiber and toluene diisocyanate is 30-60: 0.1-1: 0.01-0.1: 1-2: 1-2: 5-10: 1-2: 5-15: 30-50.

[0016] Preferably, the diameter of the toughening fibers is 3-10 μm.

[0017] Preferably, the toughened fiber is prepared by the following specific operation: adding ultra-high molecular weight polyethylene to decalin, stirring at 90-95°C for 1-2h, adding silicate cement and chitosan and stirring evenly, extruding from the spinneret hole of the spinneret, cooling, solidifying, and drying to remove the solvent.

[0018] Preferably, the molecular weight of the ultra-high molecular weight polyethylene is 3-4 million, and the particle size of the silicate cement is 5-15 μm.

[0019] Preferably, the mass ratio of ultra-high molecular weight polyethylene, silicate cement and chitosan is 10-20:1-5:1-2.

[0020] Preferably, the composite ethylene-vinyl acetate copolymer is prepared by the following specific operation: ethylene-vinyl acetate copolymer, carboxyl-terminated polyamidoamine, nano titanium dioxide, activated carbon, pentaerythritol tetraacrylate, tert-butyl peroxide-2-ethylhexyl ester and antioxidant are uniformly mixed and extruded at 180-220°C.

[0021] Preferably, the mass ratio of ethylene-vinyl acetate copolymer, carboxyl-terminated polyamidoamine, nano titanium dioxide, activated carbon, pentaerythritol tetraacrylate, tert-butyl peroxide-2-ethylhexyl ester and antioxidant is 40-60:1-3:1-2:5-15:1-2:1-2:1-2.

[0022] The preparation method of the above-mentioned environmentally friendly high-strength automobile roof includes the following steps: stacking the layers of materials in sequence, hot pressing at 130-150°C, the molding pressure is 8-10MPa, the molding time is 10-20s, and cooling and shaping is 10-20s.

[0023] Beneficial effects:

[0024] 1. The present invention adopts ultra-high molecular weight polyethylene, silicate cement and chitosan for composite spinning, so that the obtained toughened fiber felt has better adhesion and bonding with the composite ethylene-vinyl acetate copolymer than glass fiber; and then after high-temperature pressing, it not only has good rigidity, but also does not crack during use, and has high tear strength, which greatly improves the economic benefits and has good practicality, application prospects and value.

[0025] 2. The present invention does not use glass fiber, which not only has high tear resistance, but also effectively avoids the fine particles generated during the processing that may cause certain harm to production personnel. While improving the quality, it greatly improves the structural strength and performance of the automobile roof. The compounding of toughened fiber felt and polyurethane substrate can simultaneously achieve lightweight and environmental protection of the product, solve the weaknesses of existing automobile roof materials, and is an ideal new material to replace automobile roofs.

[0026] 3. The present invention adds nano titanium dioxide and activated carbon to the composite ethylene-vinyl acetate copolymer, which can make the ceiling have the ability to adsorb and degrade aldehyde substances. During the use of the automobile ceiling, the VOC value in the car can be reduced, the environmental protection effect is good, and the air in the car remains fresh.

[0027] 4. The multi-layer structure of the automobile roof of the present invention has the characteristics of tight adhesion, preventing separation between layers, good external rigidity and no deformation, and excellent sound absorption performance, no odor, safety and environmental protection, and is suitable for large-scale promotion and use. BRIEF DESCRIPTION OF THE DRAWINGS

[0028] Figure 1 It is a comparison chart of the tensile strength and elongation at break of the automobile roof obtained in Example 5 and Comparative Examples 1-2.

[0029] Figure 2 It is a comparison chart of the tear strength and compression permanent deformation rate of the automobile roof obtained in Example 5 and Comparative Examples 1-2. DETAILED DESCRIPTION

[0030] The present invention will be further explained below in conjunction with specific embodiments.

[0031] Example 1

[0032] An environmentally friendly high-strength automobile roof comprises, from bottom to top: a non-woven fabric layer, a first adhesive layer cast on the surface of the non-woven fabric layer, a first toughened fiber felt bonded to the surface of the first adhesive layer, a second adhesive layer cast on the surface of the first toughened fiber felt, a polyurethane substrate bonded to the surface of the second adhesive layer, a third adhesive layer cast on the surface of the polyurethane substrate, a second toughened fiber felt bonded to the surface of the third adhesive layer, and a fourth adhesive layer cast on the surface of the second toughened fiber felt.

[0033] The materials used for the first toughening fiber felt and the second toughening fiber felt are both toughening fiber felts made of toughening fibers with a diameter of 3-10 μm; and the materials used for the first adhesive layer, the second adhesive layer, the third adhesive layer and the fourth adhesive layer are all composite ethylene-vinyl acetate copolymer.

[0034] The thickness of the polyurethane substrate is 10 mm, the thickness of the toughened fiber felt is 0.1 mm, and the thickness of the first adhesive layer, the second adhesive layer, the third adhesive layer, and the fourth adhesive layer are all 0.1 mm.

[0035] The polyurethane substrate was prepared by the following specific operation: 30 kg of polyether polyol with a molecular weight of 3000 and a hydroxyl value of 28 mg KOH / g was continuously stirred, and 0.1 kg of triethanolamine, 0.01 kg of dibutyltin dilaurate, 1 kg of Evonik O-501, 1 kg of blowing agent HFC-245fa, 5 kg of water, 1 kg of silicone oil, and 5 kg of activated carbon fiber were added in sequence during the stirring process. After the addition was complete, it was stirred at a temperature of 5°C for 10 minutes, and 30 kg of toluene diisocyanate was added, stirred evenly at a temperature of 5°C, and sent into a mold for curing, demolding, and cooling.

[0036] The toughened fiber was prepared by the following specific operation: 10 kg of ultra-high molecular weight polyethylene with a molecular weight of 3 million was added to 40 kg of decalin, stirred at a temperature of 90°C for 1 hour, 1 kg of silicate cement with a particle size of 5-15 μm and 1 kg of chitosan were added and stirred evenly, extruded from the spinneret hole of the spinneret, cooled, solidified, and dried to remove the solvent.

[0037] The composite ethylene-vinyl acetate copolymer is prepared by the following specific operation: 40 kg of ethylene-vinyl acetate copolymer, 1 kg of terminal carboxyl polyamide amine, 1 kg of nano titanium dioxide, 5 kg of activated carbon, 1 kg of pentaerythritol tetraacrylate, 1 kg of tert-butyl peroxide-2-ethylhexyl ester, and 1 kg of antioxidant are mixed evenly and fed into an extruder for extrusion at a temperature of 180°C.

[0038] The preparation method of the above-mentioned environmentally friendly high-strength automobile roof includes the following steps: stacking the layers of materials in sequence, hot pressing at 130° C., the molding pressure is 8 MPa, the molding time is 10 seconds, cooling and shaping for 10 seconds, and cutting.

[0039] Example 2

[0040] An environmentally friendly high-strength automobile roof comprises, from bottom to top: a non-woven fabric layer, a first adhesive layer cast on the surface of the non-woven fabric layer, a first toughened fiber felt bonded to the surface of the first adhesive layer, a second adhesive layer cast on the surface of the first toughened fiber felt, a polyurethane substrate bonded to the surface of the second adhesive layer, a third adhesive layer cast on the surface of the polyurethane substrate, a second toughened fiber felt bonded to the surface of the third adhesive layer, and a fourth adhesive layer cast on the surface of the second toughened fiber felt.

[0041] The materials used for the first toughening fiber felt and the second toughening fiber felt are both toughening fiber felts made of toughening fibers with a diameter of 3-10 μm; and the materials used for the first adhesive layer, the second adhesive layer, the third adhesive layer and the fourth adhesive layer are all composite ethylene-vinyl acetate copolymer.

[0042] The thickness of the polyurethane substrate is 15 mm, the thickness of the toughened fiber felt is 0.2 mm, and the thickness of the first adhesive layer, the second adhesive layer, the third adhesive layer, and the fourth adhesive layer are all 0.2 mm.

[0043] The polyurethane substrate was prepared by the following specific operation: 60 kg of polyether polyol with a molecular weight of 3000 and a hydroxyl value of 28 mg KOH / g was continuously stirred, and 1 kg of triethanolamine, 0.1 kg of dibutyltin dilaurate, 2 kg of Evonik O-500, 2 kg of foaming agent HFC-245fa, 10 kg of water, 2 kg of silicone oil, and 15 kg of activated carbon fiber were added in sequence during the stirring process. After the addition was complete, it was stirred at a temperature of 15°C for 20 minutes, 50 kg of toluene diisocyanate was added, stirred evenly at a temperature of 10°C, and sent into a mold for curing, demolding, and cooling.

[0044] The toughened fiber was prepared by the following specific operation: 20 kg of ultra-high molecular weight polyethylene with a molecular weight of 4 million was added to 60 kg of decalin, stirred at a temperature of 95°C for 2 hours, 5 kg of silicate cement with a particle size of 5-15 μm and 2 kg of chitosan were added and stirred evenly, extruded from the spinneret hole of the spinneret, cooled, solidified, and dried to remove the solvent.

[0045] The composite ethylene-vinyl acetate copolymer is prepared by the following specific operation: 60 kg of ethylene-vinyl acetate copolymer, 3 kg of terminal carboxyl polyamide amine, 2 kg of nano titanium dioxide, 15 kg of activated carbon, 2 kg of pentaerythritol tetraacrylate, 2 kg of tert-butyl peroxide-2-ethylhexyl ester, and 2 kg of antioxidant are mixed evenly and fed into an extruder for extrusion at a temperature of 220°C.

[0046] The preparation method of the above-mentioned environmentally friendly high-strength automobile roof includes the following steps: stacking the layers of materials in sequence, hot pressing at 150°C, with a molding pressure of 10MPa, a molding time of 20s, cooling and shaping for 20s, and cutting.

[0047] Example 3

[0048] An environmentally friendly high-strength automobile roof comprises, from bottom to top: a non-woven fabric layer, a first adhesive layer cast on the surface of the non-woven fabric layer, a first toughened fiber felt bonded to the surface of the first adhesive layer, a second adhesive layer cast on the surface of the first toughened fiber felt, a polyurethane substrate bonded to the surface of the second adhesive layer, a third adhesive layer cast on the surface of the polyurethane substrate, a second toughened fiber felt bonded to the surface of the third adhesive layer, and a fourth adhesive layer cast on the surface of the second toughened fiber felt.

[0049] The materials used for the first toughening fiber felt and the second toughening fiber felt are both toughening fiber felts made of toughening fibers with a diameter of 3-10 μm; and the materials used for the first adhesive layer, the second adhesive layer, the third adhesive layer and the fourth adhesive layer are all composite ethylene-vinyl acetate copolymer.

[0050] The thickness of the polyurethane substrate is 11 mm, the thickness of the toughened fiber felt is 0.18 mm, and the thickness of the first adhesive layer, the second adhesive layer, the third adhesive layer, and the fourth adhesive layer are all 0.13 mm.

[0051] The polyurethane substrate was prepared by the following specific operation: 50 kg of polyether polyol with a molecular weight of 3000 and a hydroxyl value of 28 mg KOH / g was continuously stirred, and 0.2 kg of triethanolamine, 0.07 kg of dibutyltin dilaurate, 1.3 kg of Meside AK9905, 1.8 kg of foaming agent HFC-245fa, 7 kg of water, 1.7 kg of silicone oil, and 8 kg of activated carbon fiber were added in sequence during the stirring process. After the addition was complete, it was stirred at a temperature of 12°C for 12 minutes, 45 kg of toluene diisocyanate was added, stirred evenly at a temperature of 6°C, and sent into a mold for curing, demolding, and cooling.

[0052] The toughened fiber was prepared by the following specific operation: 18 kg of ultra-high molecular weight polyethylene with a molecular weight of 3.3 million was added to 45 kg of decalin, stirred at a temperature of 94°C for 80 minutes, 4 kg of silicate cement with a particle size of 5-15 μm and 1.3 kg of chitosan were added and stirred evenly, extruded from the spinneret hole of the spinneret, cooled, solidified, and dried to remove the solvent.

[0053] The composite ethylene-vinyl acetate copolymer is prepared by the following specific operation: 55 kg of ethylene-vinyl acetate copolymer, 1.5 kg of terminal carboxyl polyamide amine, 1.7 kg of nano titanium dioxide, 8 kg of activated carbon, 1.7 kg of pentaerythritol tetraacrylate, 1.2 kg of tert-butyl peroxide-2-ethylhexyl ester, and 1.7 kg of antioxidant are mixed evenly and fed into an extruder for extrusion at a temperature of 190°C.

[0054] The preparation method of the above-mentioned environmentally friendly high-strength automobile roof includes the following steps: stacking the layers of materials in sequence, hot pressing at 145°C, with a molding pressure of 7MPa, a molding time of 18s, cooling and shaping for 13s, and cutting.

[0055] Example 4

[0056] An environmentally friendly high-strength automobile roof comprises, from bottom to top: a non-woven fabric layer, a first adhesive layer cast on the surface of the non-woven fabric layer, a first toughened fiber felt bonded to the surface of the first adhesive layer, a second adhesive layer cast on the surface of the first toughened fiber felt, a polyurethane substrate bonded to the surface of the second adhesive layer, a third adhesive layer cast on the surface of the polyurethane substrate, a second toughened fiber felt bonded to the surface of the third adhesive layer, and a fourth adhesive layer cast on the surface of the second toughened fiber felt.

[0057] The materials used for the first toughening fiber felt and the second toughening fiber felt are both toughening fiber felts made of toughening fibers with a diameter of 3-10 μm; and the materials used for the first adhesive layer, the second adhesive layer, the third adhesive layer and the fourth adhesive layer are all composite ethylene-vinyl acetate copolymer.

[0058] The thickness of the polyurethane substrate is 13 mm, the thickness of the toughened fiber felt is 0.12 mm, and the thickness of the first adhesive layer, the second adhesive layer, the third adhesive layer, and the fourth adhesive layer are all 0.17 mm.

[0059] The polyurethane substrate was prepared by the following specific operation: 40 kg of polyether polyol with a molecular weight of 3000 and a hydroxyl value of 28 mg KOH / g was continuously stirred, and 0.8 kg of triethanolamine, 0.03 kg of dibutyltin dilaurate, 1.7 kg of Evonik O-500, 1.2 kg of foaming agent HFC-245fa, 9 kg of water, 1.3 kg of silicone oil, and 12 kg of activated carbon fiber were added in sequence during the stirring process. After the addition was complete, it was stirred at a temperature of 8°C for 18 minutes, and 35 kg of toluene diisocyanate was added. The mixture was stirred evenly at a temperature of 9°C, and the mixture was sent to a mold for curing, demolding, and cooling.

[0060] The pore opening agent is Evonik O-501 or Meside AK9905.

[0061] The toughened fiber was prepared by the following specific operation: 12 kg of ultra-high molecular weight polyethylene with a molecular weight of 3.7 million was added to 55 kg of decalin, stirred at a temperature of 92°C for 100 minutes, 2 kg of silicate cement with a particle size of 5-15 μm and 1.7 kg of chitosan were added and stirred evenly, extruded from the spinneret hole of the spinneret, cooled, solidified, and dried to remove the solvent.

[0062] The composite ethylene-vinyl acetate copolymer is prepared by the following specific operation: 45 kg of ethylene-vinyl acetate copolymer, 2.5 kg of terminal carboxyl polyamide amine, 1.3 kg of nano titanium dioxide, 12 kg of activated carbon, 1.3 kg of pentaerythritol tetraacrylate, 1.8 kg of tert-butyl peroxide-2-ethylhexyl ester, and 1.3 kg of antioxidant are mixed evenly and fed into an extruder for extrusion at a temperature of 210°C.

[0063] The preparation method of the above-mentioned environmentally friendly high-strength automobile roof includes the following steps: stacking the layers of materials in sequence, hot pressing at 135°C, the molding pressure is 9MPa, the molding time is 12s, cooling and shaping for 17s, and cutting.

[0064] Example 5

[0065] An environmentally friendly high-strength automobile roof comprises, from bottom to top: a non-woven fabric layer, a first adhesive layer cast on the surface of the non-woven fabric layer, a first toughened fiber felt bonded to the surface of the first adhesive layer, a second adhesive layer cast on the surface of the first toughened fiber felt, a polyurethane substrate bonded to the surface of the second adhesive layer, a third adhesive layer cast on the surface of the polyurethane substrate, a second toughened fiber felt bonded to the surface of the third adhesive layer, and a fourth adhesive layer cast on the surface of the second toughened fiber felt.

[0066] The materials used for the first toughening fiber felt and the second toughening fiber felt are both toughening fiber felts made of toughening fibers with a diameter of 3-10 μm; and the materials used for the first adhesive layer, the second adhesive layer, the third adhesive layer and the fourth adhesive layer are all composite ethylene-vinyl acetate copolymer.

[0067] The thickness of the polyurethane substrate is 12 mm, the thickness of the toughened fiber felt is 0.15 mm, and the thickness of the first adhesive layer, the second adhesive layer, the third adhesive layer, and the fourth adhesive layer are all 0.15 mm.

[0068] The polyurethane substrate was prepared by the following specific operation: 45 kg of polyether polyol with a molecular weight of 3000 and a hydroxyl value of 28 mg KOH / g was continuously stirred, and 0.5 kg of triethanolamine, 0.05 kg of dibutyltin dilaurate, 1.5 kg of Meside AK9905, 1.5 kg of foaming agent HFC-245fa, 8 kg of water, 1.5 kg of silicone oil, and 10 kg of activated carbon fiber were added in sequence during the stirring process. After the addition was complete, it was stirred at a temperature of 10°C for 15 minutes, 40 kg of toluene diisocyanate was added, stirred evenly at a temperature of 8°C, and sent into a mold for curing, demolding, and cooling.

[0069] The toughened fiber was prepared by the following specific operation: 15 kg of ultra-high molecular weight polyethylene with a molecular weight of 3.5 million was added to 50 kg of decalin, stirred at a temperature of 93°C for 90 minutes, 3 kg of silicate cement with a particle size of 5-15 μm and 1.5 kg of chitosan were added and stirred evenly, extruded from the spinneret hole of the spinneret, cooled, solidified, and dried to remove the solvent.

[0070] The composite ethylene-vinyl acetate copolymer is prepared by the following specific operation: 50 kg of ethylene-vinyl acetate copolymer, 2 kg of terminal carboxyl polyamide amine, 1.5 kg of nano titanium dioxide, 10 kg of activated carbon, 1.5 kg of pentaerythritol tetraacrylate, 1.5 kg of tert-butyl peroxide-2-ethylhexyl ester, and 1.5 kg of antioxidant are mixed evenly and fed into an extruder for extrusion at a temperature of 200°C.

[0071] The preparation method of the above-mentioned environmentally friendly high-strength automobile roof includes the following steps: stacking the layers of materials in sequence, hot pressing at 140°C, with a molding pressure of 8MPa, a molding time of 15s, cooling and shaping for 15s, and cutting.

[0072] Comparative Example 1

[0073] An environmentally friendly high-strength automobile roof comprises, from bottom to top: a non-woven fabric layer, a first adhesive layer cast on the surface of the non-woven fabric layer, a first glass fiber felt bonded to the surface of the first adhesive layer, a second adhesive layer cast on the surface of the first glass fiber felt, a polyurethane substrate bonded to the surface of the second adhesive layer, a third adhesive layer cast on the surface of the polyurethane substrate, a second glass fiber felt bonded to the surface of the third adhesive layer, and a fourth adhesive layer cast on the surface of the second glass fiber felt.

[0074] The first glass fiber mat and the second glass fiber mat are both made of glass fibers with a diameter of 3-10 μm; and the materials used for the first adhesive layer, the second adhesive layer, the third adhesive layer and the fourth adhesive layer are all composite ethylene-vinyl acetate copolymer.

[0075] The thickness of the polyurethane substrate is 12 mm, the thickness of the first glass fiber mat and the second glass fiber mat are both 0.15 mm, and the thickness of the first adhesive layer, the second adhesive layer, the third adhesive layer, and the fourth adhesive layer are all 0.15 mm.

[0076] The polyurethane substrate was prepared by the following specific operation: 45 kg of polyether polyol with a molecular weight of 3000 and a hydroxyl value of 28 mg KOH / g was continuously stirred, and 0.5 kg of triethanolamine, 0.05 kg of dibutyltin dilaurate, 1.5 kg of Meside AK9905, 1.5 kg of foaming agent HFC-245fa, 8 kg of water, 1.5 kg of silicone oil, and 10 kg of activated carbon fiber were added in sequence during the stirring process. After the addition was complete, it was stirred at a temperature of 10°C for 15 minutes, 40 kg of toluene diisocyanate was added, stirred evenly at a temperature of 8°C, and sent into a mold for curing, demolding, and cooling.

[0077] The composite ethylene-vinyl acetate copolymer is prepared by the following specific operation: 50 kg of ethylene-vinyl acetate copolymer, 2 kg of terminal carboxyl polyamide amine, 1.5 kg of nano titanium dioxide, 10 kg of activated carbon, 1.5 kg of pentaerythritol tetraacrylate, 1.5 kg of tert-butyl peroxide-2-ethylhexyl ester, and 1.5 kg of antioxidant are mixed evenly and fed into an extruder for extrusion at a temperature of 200°C.

[0078] The preparation method of the above-mentioned environmentally friendly high-strength automobile roof includes the following steps: stacking the layers of materials in sequence, hot pressing at 140°C, with a molding pressure of 8MPa, a molding time of 15s, cooling and shaping for 15s, and cutting.

[0079] Comparative Example 2

[0080] An environmentally friendly high-strength automobile roof comprises, from bottom to top: a non-woven fabric layer, a first adhesive layer cast on the surface of the non-woven fabric layer, a first toughened fiber felt bonded to the surface of the first adhesive layer, a second adhesive layer cast on the surface of the first toughened fiber felt, a polyurethane substrate bonded to the surface of the second adhesive layer, a third adhesive layer cast on the surface of the polyurethane substrate, a second toughened fiber felt bonded to the surface of the third adhesive layer, and a fourth adhesive layer cast on the surface of the second toughened fiber felt.

[0081] The materials used for the first toughening fiber felt and the second toughening fiber felt are both toughening fiber felts made of toughening fibers with a diameter of 3-10 μm; and the materials used for the first adhesive layer, the second adhesive layer, the third adhesive layer and the fourth adhesive layer are all composite ethylene-vinyl acetate copolymer.

[0082] The thickness of the polyurethane substrate is 12 mm, the thickness of the toughened fiber felt is 0.15 mm, and the thickness of the first adhesive layer, the second adhesive layer, the third adhesive layer, and the fourth adhesive layer are all 0.15 mm.

[0083] The polyurethane substrate was prepared by the following specific operation: 45 kg of polyether polyol with a molecular weight of 3000 and a hydroxyl value of 28 mg KOH / g was continuously stirred, and 0.5 kg of triethanolamine, 0.05 kg of dibutyltin dilaurate, 1.5 kg of Meside AK9905, 1.5 kg of foaming agent HFC-245fa, 8 kg of water, 1.5 kg of silicone oil, and 10 kg of activated carbon fiber were added in sequence during the stirring process. After the addition was complete, it was stirred at a temperature of 10°C for 15 minutes, 40 kg of toluene diisocyanate was added, stirred evenly at a temperature of 8°C, and sent into a mold for curing, demolding, and cooling.

[0084] The toughened fiber is prepared by the following specific operation: 15kg of ultra-high molecular weight polyethylene with a molecular weight of 3.5 million is added to 50kg of decalin, stirred at a temperature of 93°C for 90 minutes, 3kg of silicate cement with a particle size of 5-15μm is added and mixed evenly, extruded from the spinneret hole of the spinneret, cooled, solidified, and dried to remove the solvent.

[0085] The composite ethylene-vinyl acetate copolymer is prepared by the following specific operation: 50 kg of ethylene-vinyl acetate copolymer, 2 kg of terminal carboxyl polyamide amine, 1.5 kg of nano titanium dioxide, 10 kg of activated carbon, 1.5 kg of pentaerythritol tetraacrylate, 1.5 kg of tert-butyl peroxide-2-ethylhexyl ester, and 1.5 kg of antioxidant are mixed evenly and fed into an extruder for extrusion at a temperature of 200°C.

[0086] The preparation method of the above-mentioned environmentally friendly high-strength automobile roof includes the following steps: stacking the layers of materials in sequence, hot pressing at 140°C, with a molding pressure of 8MPa, a molding time of 15s, cooling and shaping for 15s, and cutting.

[0087] The tensile strength and elongation at break of the automobile roofs obtained in Example 5 and Comparative Examples 1-2 were measured with reference to GB / T 6344-2008 "Determination of tensile strength and elongation at break of soft foam polymer materials". The tear strength of the automobile roofs obtained in Example 5 and Comparative Examples 1-2 was measured with reference to GB / T 10808-2006 "Determination of tear strength of porous polymer elastic materials". The compression permanent deformation rate of the automobile roofs obtained in Example 5 and Comparative Examples 1-2 was tested with reference to GB / T6669-2008 "Determination of compression permanent deformation of soft foam polymer materials".

[0088] like Figure 1 and Figure 2 As shown, the tensile strength, tear strength and compression permanent deformation rate of the automobile roof obtained in Example 5 are all the highest, which are better than those of Comparative Examples 1-2 (P < 0.05).

[0089] The applicant believes that this is because the present invention adopts ultra-high molecular weight polyethylene and silicate cement, chitosan composite spinning, so that the obtained toughened fiber felt has better adhesion and bonding with the composite ethylene-vinyl acetate copolymer than glass fiber; and after high-temperature pressing, it not only has good rigidity, but also does not crack during use, and has high tear strength; the present invention does not use glass fiber, not only has high tear strength, but also effectively avoids the fine particles generated during the processing process, which will cause certain harm to production personnel, while improving the quality, greatly improving the structural strength and performance of the automobile roof, and the toughened fiber felt and polyurethane substrate compound can simultaneously achieve lightweight and environmental protection of the product, solve the weaknesses of existing automobile roof materials, and is an ideal new material to replace automobile roofs.

[0090] The automobile ceilings obtained in Example 5 and Comparative Examples 1-2 were installed in vehicles of the same brand and model. The performance of the automobile ceilings was tested according to the testing standards based on GB / T27630-2011 "Guidelines for Passenger Car Interior Air Quality Assessment" and HJ / T 400-2007 "Sampling and Determination Methods for Volatile Organic Compounds and Aldehydes and Ketones in Vehicles". The testing structure is shown in the following table, where "ND" indicates that the substance was not detected.

[0091]

[0092] The applicant believes that this is because Example 5 and Comparative Examples 1-2 add nano titanium dioxide and activated carbon to the composite ethylene-vinyl acetate copolymer, which enables the ceiling to have the ability to adsorb and degrade aldehyde substances. During the use of the car ceiling, the VOC value in the car can be reduced, the environmental protection effect is good, and the air in the car remains fresh.

[0093] The above description is only a preferred specific implementation manner of the present invention, but the protection scope of the present invention is not limited thereto. Any technician familiar with the technical field can make equivalent replacements or changes according to the technical scheme and inventive concept of the present invention within the technical scope disclosed by the present invention, which should be covered by the protection scope of the present invention.

Claims

1. An environmentally friendly high-strength automobile roof, characterized in that: From bottom to top, this includes: A non-woven fabric layer, a first adhesive layer cast on the surface of the non-woven fabric layer, a first toughened fiber felt bonded to the surface of the first adhesive layer, a second adhesive layer cast on the surface of the first toughened fiber felt, a polyurethane substrate bonded to the surface of the second adhesive layer, a third adhesive layer cast on the surface of the polyurethane substrate, a second toughened fiber felt bonded to the surface of the third adhesive layer, and a fourth adhesive layer cast on the surface of the second toughened fiber felt; The materials used for the first toughened fiber felt and the second toughened fiber felt are both toughened fiber felts made of toughened fibers; and the materials used for the first adhesive layer, the second adhesive layer, the third adhesive layer and the fourth adhesive layer are all composite ethylene-vinyl acetate copolymer.

2. The environmentally friendly high-strength automobile roof according to claim 1 is characterized in that: The polyurethane substrate is prepared by the following specific operation: the polyether polyol is continuously stirred, and triethanolamine, a catalyst, a pore opening agent, a foaming agent, water, silicone oil, and activated carbon fiber are added in sequence during the stirring process. After the addition is complete, the mixture is stirred at 5-15° C. for 10-20 minutes, and then toluene diisocyanate is added, the temperature is adjusted to 5-10° C., stirred evenly, cured, and cooled.

3. The environmentally friendly high-strength automobile roof according to claim 2 is characterized in that: The molecular weight of the polyether polyol is 2500-3500, and the hydroxyl value is 25-30 mg KOH / g; the catalyst is dibutyltin dilaurate; the foaming agent is HFC-245fa; and the cell opening agent is at least one of Evonik O-501, Evonik O-500 and Meside AK9905.

4. The mass ratio of polyether polyol, triethanolamine, catalyst, pore opener, foaming agent, water, silicone oil, activated carbon fiber and toluene diisocyanate is 30-60: 0.1-1: 0.01-0.1: 1-2: 1-2: 5-10: 1-2: 5-15: 30-50.

5. The environmentally friendly high-strength automobile roof according to claim 1, characterized in that: The diameter of the toughened fiber is 3-10 μm; the toughened fiber is prepared by the following specific operation: adding ultra-high molecular weight polyethylene to decalin, stirring at 90-95° C. for 1-2 hours, adding silicate cement and chitosan and stirring evenly, extruding from the spinneret hole of the spinneret, cooling, solidifying, and drying to remove the solvent.

6. The environmentally friendly high-strength automobile roof according to claim 5, characterized in that: The molecular weight of ultra-high molecular weight polyethylene is 3-4 million, and the particle size of silicate cement is 5-15μm.

7. The environmentally friendly high-strength automobile roof according to claim 5, characterized in that: The mass ratio of ultra-high molecular weight polyethylene, silicate cement and chitosan is 10-20:1-5:1-2.

8. The environmentally friendly high-strength automobile roof according to claim 1, characterized in that: The composite ethylene-vinyl acetate copolymer is prepared by the following specific operation: ethylene-vinyl acetate copolymer, carboxyl-terminated polyamide amine, nano titanium dioxide, activated carbon, pentaerythritol tetraacrylate, tert-butyl peroxide-2-ethylhexyl ester and antioxidant are uniformly mixed and extruded at 180-220°C.

9. The environmentally friendly high-strength automobile roof according to claim 8, characterized in that: The mass ratio of ethylene-vinyl acetate copolymer, carboxyl-terminated polyamidoamine, nano titanium dioxide, activated carbon, pentaerythritol tetraacrylate, tert-butyl peroxide-2-ethylhexyl ester and antioxidant is 40-60:1-3:1-2:5-15:1-2:1-2:1-2.

10. A method for preparing an environmentally friendly high-strength automobile roof according to any one of claims 1 to 9, characterized in that: The method comprises the following steps: stacking the layers in sequence, hot pressing at 130-150° C., with a molding pressure of 8-10 MPa, a molding time of 10-20 seconds, and cooling and shaping for 10-20 seconds.

Citation Information

Patent Citations

  • Polyurethane multilayer composite sheet for automotive headliner and processing method thereof

    CN101544083A

  • Roadbed side ditch RPC cover plate and preparation method thereof

    CN111995332A

  • Reinforcing and toughening fibers and preparation method thereof

    CN111996612A

  • Absorbent fillers for three-dimensional printing

    US20050059757A1

  • High-elasticity heat-resistant nylon 6 and preparation method

    WO2019210587A1