Multi-shell bowl-like mesoporous carbon sphere as well as preparation method and application thereof
By preparing multi-husked bowl-shaped mesoporous carbon spheres, the problem of persistence of electromagnetic shielding performance caused by poor structural uniformity of porous carbon microspheres is solved, and efficient electromagnetic wave absorption and stable electromagnetic shielding effect are achieved.
Patent Information
- Application Number
- CN202411034028.7
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-07-30
- Publication Date
- 2024-11-15
AI Technical Summary
The structural uniformity of existing porous carbon microspheres is poor, resulting in poor persistence of electromagnetic shielding performance.
The preparation method of multi-husked bowl-shaped mesoporous carbon balls is adopted. By using tetraethyl silicate, resorcinol and formaldehyde in an alkaline solution, the SiO2/phenolic resin composite is formed and the SiO2/phenolic resin composite is formed in argon gas. After calcining under atmosphere, the SiO2 template is removed in the etching solution to form a multi-husked bowl-shaped mesoporous carbon sphere.
By adding raw materials in step by step and controlling reaction conditions, a regular multi-shell structure and high porosity are formed, which improves the uniformity of the material and electromagnetic wave absorption performance, and achieves a stable electromagnetic shielding effect.
Smart Images

Figure CN118954476A_ABST
Abstract
Description
Technical Field
[0001] The invention belongs to the technical field of development of electromagnetic shielding materials, and relates to a multi-shell bowl-shaped mesoporous carbon sphere and a preparation method and application thereof. Background Art
[0002] With the rapid development of electronic equipment technology, the electromagnetic radiation and interference problems it generates are becoming increasingly serious. Long-term exposure to electromagnetic environments will cause irreversible harm to human health, manifested as neurological disorders and functional disorders. When precision electronic instruments are subject to electromagnetic interference, it will have a negative impact on the operation of the instrument, manifested as reduced accuracy and unstable operation. Therefore, the development of efficient electromagnetic wave absorbing materials is of great significance. Compared with traditional absorbing materials, current absorbing materials have higher requirements for electromagnetic absorption performance, requiring advantages such as "lightweight, broadband, thin thickness, strong absorption, and thermal stability". As a new type of carbon material, porous carbon microspheres not only have rich pore structures and high specific surface area, but also have the advantages of low cost, large output, and simple preparation method. They can be used as cheap, lightweight and efficient electromagnetic absorbers.
[0003] The research on carbon microspheres has gone through the development stage from solid, hollow to hollow mesoporous structure. Studies have shown that the introduction of complex pore structure can effectively improve impedance matching and dielectric loss characteristics. For example, Qiang et al. prepared C@C microspheres with yolk structure. The yolk structure is conducive to enhancing the loss effect of electromagnetic waves, and the strongest reflection loss value can reach ~39.4dB (Qiang R, Du Y, Wang Y, et al. Rational design of yolk~shell C@C microspheres for the effective enhancement in microwave absorption. Carbon, 2016, 98, 599~606). Yang et al. used hydrogen peroxide to etch the carbon shell and create mesopores on the surface of hollow carbon spheres to optimize impedance matching. At a thickness of 2.2 mm, the effective absorption band reached 5.6 GHz (Yang L, Zhou X, Jia Z, et al. Selective tailoring of covalent bonds on graphitized hollow carbon spheres towards controllable porous structure and wideband electromagnetic absorption. Carbon, 2020, 167: 843-851). Tao et al. prepared three-shell hollow porous carbon spheres by liquid phase method, which helped to improve the conductivity and polarization loss of the material. At a thickness of 1.6 mm, the effective absorption bandwidth was 5.17 GHz (Tao J, Zhou J, Yao Z, et al. Multi-shell hollow porous carbon nanoparticles with excellent microwave absorption properties. Carbon, 2021, 172, 542-555).
[0004] In summary, porous carbon microspheres have shown great potential in the field of electromagnetic wave absorption. However, the structural uniformity of current porous carbon microspheres is poor, resulting in poor durability of the electromagnetic shielding performance of the material. Summary of the invention
[0005] In view of the problems existing in the prior art, the present invention provides a multi-shell bowl-shaped mesoporous carbon sphere and a preparation method and application thereof, thereby solving the technical problem that the structural uniformity of the porous carbon microspheres in the prior art is poor, resulting in poor durability of the electromagnetic shielding performance of the material.
[0006] The present invention is achieved through the following technical solutions:
[0007] A method for preparing multi-shell bowl-shaped mesoporous carbon spheres comprises the following steps:
[0008] S1: adding tetraethyl silicate, resorcinol and formaldehyde to an alkaline solution, stirring and reacting once, and then adding tetraethyl silicate, resorcinol and formaldehyde to the reaction solution, stirring and reacting twice, to obtain a precursor;
[0009] S2: After calcining the precursor in an argon atmosphere, the obtained product is placed in an etching solution for etching to obtain the multi-shell bowl-shaped mesoporous carbon sphere absorbing material.
[0010] Preferably, in step S1, the reaction time of the stirring reaction is 5 to 10 hours.
[0011] Preferably, in step S1, before a stirring reaction is performed, the ratio of tetraethyl silicate, resorcinol and formaldehyde is (1.4-4.2) mL: (0.2-0.6) g: (0.28-0.84) mL.
[0012] Preferably, in step S1, the reaction time of the secondary stirring reaction is 16 to 24 hours.
[0013] Preferably, in step S1, after a stirring reaction, tetraethyl silicate, resorcinol and formaldehyde are added in a ratio of (0.5-2.0) mL: 0.05 g: 0.07 mL.
[0014] Preferably, in step S2, during the calcination treatment, the heating rate is 5°C / min, the calcination temperature is 600-1000°C, and the holding time is 2-5h.
[0015] Preferably, in step S2, the etching solution is a hydrofluoric acid solution, and the mass fraction of the hydrofluoric acid solution is 5% to 25%.
[0016] Preferably, in step S2, the etching time is 8 to 12 hours.
[0017] A multi-shell bowl-shaped mesoporous carbon sphere is prepared by the above method.
[0018] The above-mentioned multi-shell bowl-shaped mesoporous carbon sphere is used in electromagnetic shielding equipment.
[0019] Compared with the prior art, the present invention has the following beneficial technical effects:
[0020] The invention discloses a method for preparing multi-shell bowl-shaped mesoporous carbon spheres. Tetraethyl silicate is used as a silicon source, and resorcinol and formaldehyde undergo polycondensation under alkaline conditions to form phenolic resin, which is the main component of the carbon spheres. First, tetraethyl silicate, resorcinol and formaldehyde are introduced into an alkaline solution, and a preliminary SiO2 / phenolic resin composite is formed through a stirring reaction. Subsequently, these raw materials are added again for a secondary stirring reaction to enhance the shell structure and mesoporous properties of the composite. This step-by-step addition of raw materials helps to form a multi-shell structure. Then, calcination is performed under an argon atmosphere to convert the phenolic resin into carbon, while the SiO2 template remains intact, forming a composite structure of SiO2@SiO2 / C@SiO2@SiO2 / C. Finally, the calcined product is placed in an etching solution to selectively remove the SiO2 template. Due to the difference in thermal and chemical stability between SiO2 and carbon, the etching process can be precisely controlled, leaving a concave carbon skeleton and forming a multi-shelled bowl-shaped mesoporous carbon sphere. The uniformity of the material is effectively ensured by distributing the layered structure and the etching process. This method avoids complex equipment and harsh reaction conditions, making large-scale production possible. The raw materials are widely available and the cost is relatively low, which is conducive to industrial application. By controlling the reaction conditions and steps, it can be ensured that the obtained carbon spheres have good dispersion and uniform size. The multi-shell structure and high porosity give the carbon spheres a larger specific surface area and richer interface effects, which are conducive to the absorption and scattering of electromagnetic waves. The regular structure makes the behavior of carbon spheres in electromagnetic fields more predictable and controllable, providing a stable performance foundation for practical applications.
[0021] Further, in step S1, the reaction time of the stirring reaction is 5 to 10 hours, and the reaction time of 5 to 10 hours ensures that tetraethyl silicate, resorcinol and formaldehyde can be fully mixed and chemically reacted in the alkaline solution. This sufficient reaction time helps to form a stable and uniform SiO2 / phenolic resin composite precursor, laying the foundation for the subsequent multi-shell structure construction. By controlling the reaction time, the structure and morphology of the precursor can be finely regulated. A longer reaction time helps to form a more dense and ordered composite structure, thereby maintaining a good morphology and structural integrity during the subsequent calcination and etching process. Appropriate reaction time can maximize the use of raw materials and improve the yield of the product. At the same time, sufficient reaction also helps to reduce the generation of by-products and improve the purity and quality of the product, which is crucial for the preparation of high-performance multi-shell bowl-shaped mesoporous carbon spheres. Setting a fixed reaction time range helps to maintain the stability of the process. In industrial production, stable process conditions are of great significance for ensuring product quality and consistency. By controlling the reaction time, the preparation process can be made more controllable and repeatable. The effect of the primary stirring reaction directly affects the subsequent secondary stirring reaction as well as the calcination and etching treatments. Sufficient reaction time helps to form a more uniform and stable precursor, providing a good foundation for subsequent shell construction and pore formation. In summary, setting the time for the primary stirring reaction in step S1 to 5 to 10 hours has a significant beneficial effect on the preparation of high-quality, high-performance multi-shell bowl-shaped mesoporous carbon spheres. The setting of this time range is based on a deep understanding of the reaction mechanism and process conditions, and aims to optimize the performance of the product by finely controlling the reaction process.
[0022] Further, in step S1, before a stirring reaction, the ratio of tetraethyl silicate, resorcinol and formaldehyde is (1.4-4.2) mL: (0.2-0.6) g: (0.28-0.84) mL. The setting of this ratio helps to form a stable and uniform SiO2 / phenolic resin composite precursor in an alkaline solution. Tetraethyl silicate, as a silicon source, undergoes a polycondensation reaction with resorcinol and formaldehyde under alkaline conditions to form a composite with a specific structure. The appropriate ratio can ensure sufficient contact and reaction between the reactants, thereby optimizing the structure and morphology of the precursor. In the subsequent secondary stirring reaction, the same ratio of tetraethyl silicate, resorcinol and formaldehyde is continued to be added, which can further enhance the shell structure of the composite. This step-by-step addition of raw materials, combined with an appropriate ratio setting, helps to form a clear and regular multi-shell structure, providing a structural basis for the final multi-shell bowl-shaped mesoporous carbon sphere. The appropriate ratio of reactants can ensure the formation of uniform composite particles during the reaction process, thereby improving the uniformity and dispersibility of the product, which is crucial for the preparation of high-performance absorbing materials, because uniformity and dispersibility directly affect the electromagnetic wave absorption performance and stability of the material. The appropriate ratio of reactants helps to form a rich pore structure and high specific surface area in the subsequent calcination and etching treatment. Porosity and specific surface area are important indicators for evaluating the performance of mesoporous materials, and are of great significance for improving the electromagnetic wave absorption performance of materials. By optimizing the ratio of reactants, the porosity and specific surface area of the product can be adjusted to meet different application requirements. A fixed ratio of reactants helps to maintain the stability and repeatability of the process. In industrial production, stable process conditions are crucial to ensure product quality and consistency. By controlling the ratio of reactants, the preparation process can be made more controllable and repeatable, which is conducive to large-scale production. In summary, the ratio of tetraethyl silicate, resorcinol and formaldehyde in step S1 is set to (1.4-4.2) mL: (0.2-0.6) g: (0.28-0.84) mL, which is set based on a deep understanding of the reaction mechanism and product performance. The selection of this ratio helps to optimize the precursor structure, promote the formation of multi-shell structures, improve the uniformity and dispersibility of the product, optimize the porosity and specific surface area, and maintain the stability and repeatability of the process.
[0023] Further, in step S1, the reaction time of the secondary stirring reaction is 16 to 24 hours, and the main purpose of the secondary stirring reaction is to further construct a shell structure on the precursor. The longer reaction time (16 to 24 hours) provides more sufficient time for the reaction between tetraethyl silicate, resorcinol and formaldehyde, so that the shell structure can be formed more densely and evenly, which helps to maintain the integrity and clarity of the shell in the subsequent calcination and etching treatment. During the secondary stirring reaction, as the shell is constructed, a pore structure will gradually form inside the precursor. The longer reaction time helps the formation and expansion of these pore structures, so that the final multi-shell bowl-shaped mesoporous carbon spheres have higher porosity and richer pore structure, which is crucial to improving the electromagnetic wave absorption performance of the material. Sufficient reaction time helps to reduce the generation of by-products and improve the purity and quality of the product. In the secondary stirring reaction, the reaction between the raw materials is more thorough, which is conducive to the formation of a more stable and excellent precursor. The fixed reaction time range helps to maintain the stability of the process. In industrial production, stable process conditions are the key to ensuring product quality and consistency. By controlling the time of the secondary stirring reaction, the preparation process can be made more controllable and repeatable. The effect of the secondary stirring reaction directly affects the subsequent calcination and etching treatments. A longer reaction time can ensure that the precursor has a better structure and morphology, providing a good foundation for subsequent shell removal and pore formation. This helps to finally prepare multi-shell bowl-shaped mesoporous carbon spheres with excellent performance. In summary, the time for the secondary stirring reaction in step S1 is set to 16 to 24 hours, which is based on a deep understanding of the reaction mechanism and product performance. The setting of this time range helps to enhance shell construction, optimize pore structure, improve product quality, maintain process stability, and provide a strong guarantee for the successful implementation of subsequent steps.
[0024] Further, in step S1, after a stirring reaction, tetraethyl silicate, resorcinol and formaldehyde are added in a ratio of (0.5-2.0) mL: 0.05 g: 0.07 mL. By adding the reactants again, a new shell can be continuously constructed on the surface of the formed SiO2 / phenolic resin composite. This step-by-step addition method helps to form a multilayer structure, so that the final multi-shell bowl-shaped mesoporous carbon sphere has a more complex structure and better performance. The appropriate ratio can ensure good uniformity and continuity between the newly added shell and the original shell, thereby avoiding problems such as shell shedding or cracking in subsequent treatments. The newly added tetraethyl silicate, resorcinol and formaldehyde will form a new pore structure during the reaction. These pores are interconnected with the original pores to form a richer pore network, which helps to increase the specific surface area and porosity of the material, thereby improving its electromagnetic wave absorption performance. By adjusting the proportion of the newly added reactants and the reaction conditions, the size and distribution of the pores can be further regulated to meet the needs of different application scenarios. Longer reaction time and appropriate reactant ratio help ensure sufficient contact and reaction between reactants, thereby improving the purity and quality of the product. The formation of multilayer shell structure helps to enhance the structural stability of carbon spheres, so that they can maintain good morphology and performance during subsequent processing and use. By precisely controlling the ratio of reactants and reaction time, fine regulation of the preparation process can be achieved, thereby optimizing process conditions and improving product stability and consistency. This step-by-step addition of reactants is easy to realize automation and continuous operation in industrial production, which is conducive to large-scale production and cost reduction. In summary, in step S1, after a stirring reaction, tetraethyl silicate, resorcinol and formaldehyde are continued to be added in a ratio of (0.5-2.0) mL: 0.05 g: 0.07 mL, which is intended to promote the formation of multi-shell structure, optimize pore structure, improve product quality and stability, and enhance process controllability and repeatability. These beneficial effects work together on the final multi-shell bowl-shaped mesoporous carbon sphere absorber, giving it more excellent performance and wider application prospects.
[0025] Further, in step S2, during the calcination process, the heating rate is 5°C / minute, the calcination temperature is 600-1000°C, and the holding time is 2-5h. The heating rate of 5°C / minute is relatively slow, which helps to evenly increase the temperature in the furnace and reduce the problem of excessive temperature gradient caused by too fast heating. This helps to ensure that the material is heated evenly during the calcination process and avoid defects caused by local overheating or overcooling. The slower heating rate can also reduce the thermal stress generated by the material during the heating process and reduce the risk of cracking of the material due to stress concentration. The holding time is set to 2-5h, which ensures that there is enough time for the reactants to react chemically at the calcination temperature, which helps to form a more uniform and dense product structure and improve the performance of the product. The calcination temperature is 600-1000°C, which can make the phenolic resin decompose and completely convert into carbon material, and make it have a good degree of graphitization, thereby improving the dielectric loss characteristics. By setting the above-mentioned heating rate, calcination temperature and holding time, the purity, density, strength and electromagnetic wave absorption performance of the product can be significantly improved.
[0026] Further, in step S2, the etching solution is a hydrofluoric acid solution, the mass fraction of the hydrofluoric acid solution is 5% to 25%, and the 10wt% hydrofluoric acid solution has moderate corrosiveness, and can etch the target material at an appropriate rate without excessively corroding the substrate material. Compared with a higher concentration of hydrofluoric acid solution, a concentration of 10wt% reduces the potential damage to the substrate material, which is beneficial to protecting the integrity of the non-etched area. The lower concentration of hydrofluoric acid solution is relatively less harmful to the operator during operation, reducing the risk of safety accidents. High concentration of hydrofluoric acid is highly corrosive and toxic, requiring more stringent protective measures. 10wt% hydrofluoric acid solution is more convenient and safer during storage, transportation and handling, reducing the need for special equipment and protective measures. Using a lower concentration of hydrofluoric acid solution can reduce the cost of raw materials, because its preparation and purchase cost is usually lower than that of a high concentration solution. In some etching processes, by adjusting the concentration of the etching solution and combining other process parameters (such as temperature, time, stirring speed, etc.), a more optimized etching effect can be achieved, thereby reducing costs while meeting performance requirements.
[0027] Furthermore, in step S2, the etching time is 8 to 12 hours. A longer etching time helps to ensure that the etching depth reaches the predetermined requirements. In the chemical etching process, the etching depth is proportional to the etching time, so the etching depth can be accurately controlled by controlling the etching time. Sufficient etching time can ensure that the silicon dioxide template agent is completely removed to avoid the influence of residue on subsequent processes or product performance. A longer etching time helps to reduce the non-uniformity in the etching process. In the early stage of etching, the etching rate may be inconsistent due to factors such as reactant concentration and temperature distribution, but as the etching time increases, these differences will gradually decrease, making the etching results more uniform. By controlling the etching time, the surface morphology of the etched material can be optimized. BRIEF DESCRIPTION OF THE DRAWINGS
[0028] In order to more clearly illustrate the technical solutions of the embodiments of the present invention, the drawings required for use in the embodiments are briefly introduced below. It should be understood that the following drawings only show certain embodiments of the present invention and therefore should not be regarded as limiting the scope. For ordinary technicians in this field, other related drawings can be obtained based on these drawings without creative work.
[0029] Figure 1 It is a schematic diagram of a process for preparing a multi-shell bowl-shaped mesoporous carbon sphere in the present invention;
[0030] Figure 2 The XRD spectra (a) and Raman spectra (b) of mesoporous carbon spheres at different silicon template addition amounts in Examples 1 to 4 of the present invention;
[0031] Figure 3 These are SEM and TEM photos of mesoporous carbon spheres at different silicon template addition amounts in Examples 1 to 4 of the present invention, wherein a is the sample of Example 1, b is the sample of Example 2, c is the sample of Example 3, and d is the sample of Example 4;
[0032] Figure 4 The surface scanning spectrum and EDS spectrum of the mesoporous carbon spheres prepared in Example 3 of the present invention;
[0033] Figure 5 The isothermal adsorption-desorption curves and pore size distribution maps of mesoporous carbon spheres at different silicon template addition amounts in Examples 1 to 4 of the present invention, wherein a is the sample of Example 1, b is the sample of Example 2, c is the sample of Example 3, and d is the sample of Example 4;
[0034] Figure 6 The electromagnetic parameter curves of mesoporous carbon spheres under different silicon template addition amounts in Examples 1 to 4 of the present invention, wherein a is the sample of Example 1, b is the sample of Example 2, c is the sample of Example 3, and d is the sample of Example 4;
[0035] Figure 7 These are reflection loss curves of mesoporous carbon spheres at different thicknesses with different silicon template addition amounts in Examples 1 to 4 of the present invention, where a is the sample in Example 1, b is the sample in Example 2, c is the sample in Example 3, and d is the sample in Example 4. DETAILED DESCRIPTION
[0036] In order to enable those skilled in the art to understand the characteristics and effects of the present invention, the following is a general description and definition of the terms and expressions mentioned in the specification and claims. Unless otherwise specified, all technical and scientific terms used in the text are the common meanings understood by those skilled in the art for the present invention. In the event of a conflict, the definition in this specification shall prevail.
[0037] The theories or mechanisms described and disclosed herein, whether correct or incorrect, should not limit the scope of the present invention in any way, that is, the present invention can be implemented without being limited by any specific theory or mechanism.
[0038] Herein, all features such as values, quantities, contents and concentrations defined in the form of numerical ranges or percentage ranges are for simplicity and convenience only. Accordingly, the description of numerical ranges or percentage ranges should be considered to have included and specifically disclosed all possible secondary ranges and individual values within the range (including integers and fractions).
[0039] In this document, unless otherwise specified, “includes,” “including,” “contains,” “has,” or similar terms cover the meanings of “consisting of” and “mainly consisting of,” for example, “A includes a” covers the meanings of “A includes a and other” and “A only includes a.”
[0040] In this document, in order to make the description concise, not all possible combinations of various technical features in various embodiments or examples are described. Therefore, as long as there is no contradiction in the combination of these technical features, the various technical features in various embodiments or examples can be combined arbitrarily, and all possible combinations should be considered to be within the scope of this specification.
[0041] like Figure 1 As shown, the present invention provides a method for preparing multi-shell bowl-shaped mesoporous carbon spheres, comprising the following steps:
[0042] S1: Tetraethyl silicate, resorcinol and formaldehyde are added to an alkaline solution, wherein the ratio of tetraethyl silicate, resorcinol and formaldehyde is (1.4-4.2) mL: (0.2-0.6) g: (0.28-0.84) mL. After a stirring reaction for 5 to 10 hours, tetraethyl silicate, resorcinol and formaldehyde are continuously added to the reaction solution, and a second stirring reaction is carried out for 16 to 24 hours. Here, the ratio of tetraethyl silicate, resorcinol and formaldehyde added is (0.5 to 2.0) mL: 0.05 g: 0.07 mL to obtain a precursor; the alkaline solution is prepared by water, ethanol and ammonia water.
[0043] S2: After the precursor is calcined in an argon atmosphere, wherein the heating rate is 5°C / min, the calcination temperature is 600-1000°C, and the insulation time is 2-5h, the obtained product is placed in a hydrofluoric acid etching solution with a mass fraction of 5%-25% and etched for 8-12h to obtain the multi-shell bowl-shaped mesoporous carbon spheres.
[0044] In addition, the present invention also discloses a multi-shell bowl-shaped mesoporous carbon sphere prepared by the above method and the application of the material in electromagnetic shielding equipment.
[0045] The present invention utilizes a hard template method to first synthesize a SiO2@SiO2 / phenolic resin@SiO2@SiO2 / phenolic resin precursor, which is then converted into SiO2@SiO2 / C@SiO2@SiO2 / C through high-temperature heat treatment. After removing the SiO2 template, the carbon skeleton is depressed to form multi-shelled bowl-shaped mesoporous carbon spheres. This method has the advantages of simple process, low cost, high yield, and low equipment requirements, and is suitable for large-scale production. The prepared multi-shelled bowl-shaped mesoporous carbon spheres have the advantages of good dispersibility, uniform size, clear shell, high porosity, and regular structure. The bowl-shaped mesoporous carbon spheres obtained by this method exhibit excellent dielectric loss performance and broadband electromagnetic wave absorption effect, with an absorption intensity of up to 59.1dB and an effective absorption bandwidth of up to 8.5GHz.
[0046] The present invention will be further described below in conjunction with specific embodiments. It should be understood that these embodiments are only used to illustrate the present invention and are not intended to limit the scope of the present invention. In addition, it should be understood that after reading the content taught by the present invention, those skilled in the art can make various changes or modifications to the present invention, and these equivalent forms fall within the scope limited by the appended claims of the application equally.
[0047] The following examples use conventional instruments and equipment in the art. The experimental methods in the following examples where specific conditions are not specified are usually carried out under conventional conditions or under conditions recommended by the manufacturer. The various raw materials used in the following examples are conventional commercial products unless otherwise specified, and their specifications are conventional specifications in the art. In the specification of the present invention and the following examples, unless otherwise specified, "%" means weight percentage, "part" means weight part, and ratio means weight ratio.
[0048] Example 1
[0049] A method for preparing multi-shell bowl-shaped mesoporous carbon spheres by a simple hard template method comprises the following steps:
[0050] Step 1, add 2.8 mL of TEOS, 0.4 g of resorcinol and 0.56 mL of formaldehyde solution into a mixed solution containing 70 mL of ethanol, 10 mL of deionized water and 3 mL of ammonia water, and stir to react for 6 hours;
[0051] Step 2: After the reaction is completed, 0.5 mL of TEOS, 0.05 g of resorcinol and 0.07 mL of formaldehyde solution are added, and the reaction is continued with stirring for 24 hours. After the reaction is completed, the precursor is obtained by centrifugal washing;
[0052] Step 3, placing the precursor obtained in the previous step in a tube furnace under high temperature conditions, calcining at 700° C. for 2 h under argon atmosphere protection conditions, with a heating rate of 5° C. / min, to convert the phenolic resin into carbon;
[0053] Step 4, placing the product obtained in step 3 in a 10 wt% hydrofluoric acid solution, stirring for 12 hours, and removing the SiO2 template.
[0054] Example 2
[0055] The difference between this embodiment and embodiment 1 is:
[0056] Step 2: After the reaction is completed, 1.0 mL of TEOS, 0.05 g of resorcinol and 0.07 mL of formaldehyde solution are added, and the reaction is continued with stirring for 24 hours. After the reaction is completed, the precursor is obtained by centrifugal washing.
[0057] Example 3
[0058] The difference between this embodiment and embodiment 1 is:
[0059] Step 2: After the reaction is completed, 1.5 mL of TEOS, 0.05 g of resorcinol and 0.07 mL of formaldehyde solution are added, and the reaction is continued with stirring for 24 hours. After the reaction is completed, the precursor is obtained by centrifugal washing.
[0060] Example 4
[0061] Step 2: After the reaction is completed, 2.0 mL of TEOS, 0.05 g of resorcinol and 0.07 mL of formaldehyde solution are added, and the reaction is continued with stirring for 24 hours. After the reaction is completed, the precursor is obtained by centrifugal washing.
[0062] Figure 2 is the X-ray diffraction pattern of the mesoporous carbon spheres prepared in Examples 1 to 4; Figure 2 From a, we can see that all samples have a broad graphitized carbon (002) crystal plane diffraction peak at 2θ = 23.6°; Figure 2 b It can be seen that all samples are at 1349 cm ~1 and 1597cm ~1 The D peak and G peak of carbon material appeared at the bottom, indicating that the prepared mesoporous carbon spheres are typical carbon materials and have a certain degree of graphitization.
[0063] Figure 3 These are SEM and TEM photos of the mesoporous carbon spheres prepared in Examples 1 to 4; it can be seen from the figures that the mesoporous carbon spheres exhibit a regular bowl-shaped structure with good dispersion and uniformity, and the contours of different shells in the bowl are clearly visible; with the increase in the amount of silicon template added, the distance between the inner and outer carbon shells increases, and the proportion of bowl-shaped carbon spheres gradually increases.
[0064] Figure 4 This is the surface scan spectrum and EDS spectrum of Example 3; it can be seen from the figure that the main components of the mesoporous carbon spheres are C and O, and the O element comes from the O left in the phenolic resin.
[0065] Figure 5 The isothermal adsorption-desorption curves and pore size distribution diagrams of the mesoporous carbon spheres prepared in Examples 1 to 4 are shown in the figure. It can be seen from the figure that all the mesoporous carbon spheres have a high specific surface area, and the surface area first increases and then decreases with the change of the amount of silicon template added. The highest specific surface area can reach 1455.1 m 2 / g; the pore size is within the mesoporous range.
[0066] Figure 6 The electromagnetic parameter curves of the mesoporous carbon spheres prepared in Examples 1 to 4 are shown in the figure. It can be seen from the figure that the dielectric constant of the sample has a direct relationship with its microstructure. As the amount of silicon template added increases, the shell spacing increases, and the dielectric constant shows a gradually decreasing trend. The real part of the initial dielectric constant of the sample in Example 1 is 8.3, and the imaginary part is 6.6; the real part of the initial dielectric constant of the sample in Example 2 is 8.0, and the imaginary part is 6.2; the real part of the initial dielectric constant of the sample in Example 3 is 6.5, and the imaginary part is 4.4; the real part of the initial dielectric constant of the sample in Example 4 is 6.1, and the imaginary part is 4.0.
[0067] Figure 7The reflection loss curves of the mesoporous carbon spheres prepared in Examples 1 to 4 at different thicknesses are shown in the figure. The mesoporous carbon spheres exhibit excellent electromagnetic wave absorption performance. The sample obtained in Example 2 has an absorption band of 8.5 GHz (9.4 to 17.9 GHz) at a thickness of 3.00 mm, and is a broadband electromagnetic wave absorption material. The sample obtained in Example 3 has a reflection loss intensity of 59.2 dB at a thickness of 3.85 mm, and an effective bandwidth absorption of 5.3 GHz (9.4 to 17.9 GHz).
[0068] Example 5
[0069] A method for preparing multi-shell bowl-shaped mesoporous carbon spheres comprises the following steps:
[0070] S1: Add tetraethyl silicate, resorcinol and formaldehyde to an alkaline solution, wherein the ratio of tetraethyl silicate, resorcinol and formaldehyde is 1.4mL:0.2g:0.28mL, and carry out a stirring reaction for 5 hours. Then, continue to add tetraethyl silicate, resorcinol and formaldehyde to the reaction solution, and carry out a second stirring reaction for 16 hours. The ratio of tetraethyl silicate, resorcinol and formaldehyde added here is 0.5mL:0.05g:0.07mL. The reaction is completed to obtain a precursor.
[0071] S2: After the precursor is calcined in an argon atmosphere, wherein the heating rate is 5°C / min, the calcination temperature is 600°C, and the insulation time is 2h, the obtained product is placed in a hydrofluoric acid etching solution with a mass fraction of 5% and etched for 8h to obtain the multi-shell bowl-shaped mesoporous carbon spheres.
[0072] Example 6
[0073] A method for preparing multi-shell bowl-shaped mesoporous carbon spheres comprises the following steps:
[0074] S1: Add tetraethyl silicate, resorcinol and formaldehyde to an alkaline solution, wherein the ratio of tetraethyl silicate, resorcinol and formaldehyde is 3mL:0.4g:0.5mL, and carry out a stirring reaction for 6 hours. Then, continue to add tetraethyl silicate, resorcinol and formaldehyde to the reaction solution, and carry out a second stirring reaction for 20 hours. The ratio of tetraethyl silicate, resorcinol and formaldehyde added here is 1mL:0.05g:0.07mL. The reaction is completed to obtain a precursor.
[0075] S2: After the precursor is calcined in an argon atmosphere, wherein the heating rate is 5°C / min, the calcination temperature is 800°C, and the insulation time is 3h, the obtained product is placed in a hydrofluoric acid etching solution with a mass fraction of 10h and etched for 10h to obtain the multi-shell bowl-shaped mesoporous carbon spheres.
[0076] Example 7
[0077] A method for preparing multi-shell bowl-shaped mesoporous carbon spheres comprises the following steps:
[0078] S1: Add tetraethyl silicate, resorcinol and formaldehyde to an alkaline solution, wherein the ratio of tetraethyl silicate, resorcinol and formaldehyde is 4.2mL:0.6g:0.84mL, and carry out a stirring reaction for 10 hours. Then, continue to add tetraethyl silicate, resorcinol and formaldehyde to the reaction solution, and carry out a second stirring reaction for 24 hours. The ratio of tetraethyl silicate, resorcinol and formaldehyde added here is 2.0mL:0.05g:0.07mL. The reaction is completed to obtain a precursor.
[0079] S2: After the precursor is calcined in an argon atmosphere, wherein the heating rate is 5°C / min, the calcination temperature is 1000°C, and the insulation time is 5h, the obtained product is placed in a hydrofluoric acid etching solution with a mass fraction of 25% and etched for 12h to obtain the multi-shell bowl-shaped mesoporous carbon spheres.
[0080] The present invention provides a method for preparing multi-shelled bowl-shaped hollow mesoporous carbon spheres as wave absorbing materials by a simple hard template method, and the morphology and shell spacing of the mesoporous carbon spheres are adjusted by adjusting the amount of secondary template added. The obtained product has excellent dielectric loss performance and electromagnetic wave absorption performance. The present invention provides a new method for preparing multi-shelled bowl-shaped mesoporous carbon spheres, which has the advantages of simple process, low cost, high yield, etc., and can be applied to actual industrial production.
[0081] The above is only a preferred embodiment of the present invention. It should be pointed out that for ordinary technicians in this technical field, several improvements and modifications can be made without departing from the principle of the present invention. These improvements and modifications should also be regarded as the scope of protection of the present invention.
[0082] Finally, it should be noted that the above embodiments are only used to illustrate the technical solution of the present invention rather than to limit the scope of protection of the present invention. Although the present invention has been described in detail with reference to the preferred embodiments, those skilled in the art should understand that the technical solution of the present invention can be modified or replaced by equivalents without departing from the essence and scope of the technical solution of the present invention.
Claims
1. A method for preparing multi-shell bowl-shaped mesoporous carbon spheres, It is characterized in that The following steps are involved: S1: adding tetraethyl silicate, resorcinol and formaldehyde to an alkaline solution, stirring and reacting once, and then adding tetraethyl silicate, resorcinol and formaldehyde to the reaction solution, stirring and reacting twice, to obtain a precursor; S2: After calcining the precursor in an argon atmosphere, the obtained product is placed in an etching solution for etching to obtain the multi-shell bowl-shaped mesoporous carbon sphere absorbing material.
2. The method for preparing multi-shell bowl-shaped mesoporous carbon spheres according to claim 1, It is characterized in that In step S1, the reaction time of the stirring reaction is 5 to 10 hours.
3. The method for preparing multi-shell bowl-shaped mesoporous carbon spheres according to claim 1, It is characterized in that In step S1, before a stirring reaction is performed, the ratio of tetraethyl silicate, resorcinol and formaldehyde is (1.4-4.2) mL: (0.2-0.6) g: (0.28-0.84) mL.
4. The method for preparing multi-shell bowl-shaped mesoporous carbon spheres according to claim 1, It is characterized in that In step S1, the reaction time of the secondary stirring reaction is 16 to 24 hours.
5. The method for preparing multi-shell bowl-shaped mesoporous carbon spheres according to claim 1, It is characterized in that In step S1, after a stirring reaction, tetraethyl silicate, resorcinol and formaldehyde are added in a ratio of (0.5-2.0) mL: 0.05 g: 0.07 mL.
6. The method for preparing multi-shell bowl-shaped mesoporous carbon spheres according to claim 1, It is characterized in that In step S2, during the calcination treatment, the heating rate is 5°C / min, the calcination temperature is 600-1000°C, and the holding time is 2-5h.
7. The method for preparing multi-shell bowl-shaped mesoporous carbon spheres according to claim 1, It is characterized in that In step S2, the etching solution is a hydrofluoric acid solution, and the mass fraction of the hydrofluoric acid solution is 5% to 25%.
8. The method for preparing multi-shell bowl-shaped mesoporous carbon spheres according to claim 1, It is characterized in that In step S2, the etching time is 8 to 12 hours.
9. A multi-shell bowl-shaped mesoporous carbon sphere, It is characterized in that It is prepared by the method according to any one of claims 1 to 8.
10. Use of the multi-shell bowl-shaped mesoporous carbon sphere described in claim 9 in electromagnetic shielding equipment.
Citation Information
Patent Citations
Single-layer and multi-layer hollow carbon nanosphere and preparation method and application thereof
CN104843665A
Hollow carbon particles using resorcinol-based polymer as precursor, method for producing the same and use thereof
JP2007254243A
Cited By
Preparation method of five-membered ring-rich interconnected spherical porous carbon material and seawater electro-catalysis application of five-membered ring-rich interconnected spherical porous carbon material
CN121225586A