Ultrahigh-ductility interface treatment mortar adaptive to fabricated steel structure and preparation method of ultrahigh-ductility interface treatment mortar

By using composite cementitious materials and nanowhisker modified PVA fibers in prefabricated steel structures, the problem of poor adhesion performance on the steel structure is solved, the bonding strength and ductility are improved, and the Crack risk and diversified construction have been achieved, meeting the sealing, fire protection, thermal and decorative performance needs of prefabricated steel structures.

CN118955052APending Publication Date: 2024-11-15临海市忠信新型建材有限公司
View PDF 0 Cites 2 Cited by

Patent Information

Application Number
CN202411062529.6
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-08-05
Publication Date
2024-11-15

AI Technical Summary

Technical Problem

In prefabricated steel structures, existing mortar cannot effectively bond to the surface of the steel structure, resulting in poor bonding performance, high risk of cracks and cracks, and a single construction process.

Method used

Using composite cementitious materials, graded sand, polycarboxylic acid water reducer, silicone defoamer, cellulose ether and nanowhisker modified PVA fibers, ultra-high ductility interface treatment mortar can be prepared by stirring and mixing, and can achieve a variety of Melting construction methods.

Benefits of technology

It improves the bonding performance and ductility of the mortar, reduces the risks of cracks and cracks, realizes mechanized production and diversified construction, and enhances the flexibility and efficiency of construction.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure BDA0004978391390000091
    Figure BDA0004978391390000091
  • Figure BDA0004978391390000101
    Figure BDA0004978391390000101
Patent Text Reader

Abstract

The invention provides ultrahigh-ductility interface treatment mortar adaptive to an assembled steel structure and a preparation method of the ultrahigh-ductility interface treatment mortar, and the mortar is prepared from the following components in parts by weight: 530-770 parts of a composite cementing material, 450-550 parts of graded sand, 0.4-0.6 part of a water reducing agent, 1-2.5 parts of a defoaming agent, 2-4 parts of cellulose ether, 2.5-5 parts of a composite volume stabilizer and 1-3.5 parts of nano-whisker modified PVA (Polyvinyl Alcohol) fibers, the composite cementing material comprises VAE (Vinyl Acetate Ethylene) redispersible latex powder and ordinary Portland cement; the composite volume stabilizer comprises a micro-expanding agent, a shrinkage reducing agent and nano SiO2. The mortar has excellent bonding performance and ductility performance, can effectively resist deformation and firmly bond the surface of a steel structure, and also reduces the generation of cracks and the risk of cracking. The preparation method of the mortar is simple, mechanical production is easy to realize, the construction process is diversified, and mechanical spraying can also be realized in a mode of combining roll coating, brush coating and blade coating.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the technical field of building materials, and in particular to an ultra-high ductility interface treatment mortar suitable for assembled steel structures and a preparation method thereof. Background Art

[0002] At present, general buildings and building components need to use mortar plastering layers. Mortar plastering layers can not only protect buildings and walls, but also resist the erosion of natural environments such as wind, rain, and snow on buildings, and improve the durability of buildings. It will also have a dense, smooth and beautiful decorative effect; and all of this is based on the effective bonding between the mortar plastering layer and the substrate, which requires the use of interface treatment mortar. Interface treatment mortar is a material that can not only firmly bond to the base layer, but also its surface can be well covered by new mortar bonding, and has a two-way affinity. Interface treatment mortar can be classified into three categories according to the material: organic, inorganic, and organic and inorganic composite; according to the finished product form, it can be divided into three types: solid, liquid, and solid-liquid dual components. Dry-mixed mortar interface treatment mortar contains water-retaining agent and high molecular polymer, and is in powder form, which needs to be diluted with water when used.

[0003] With the rapid development of prefabricated steel structures, the area of ​​newly built steel structures will also grow rapidly. In the promotion and application of steel-structured houses, the wall system needs to meet the requirements of sealing performance, fire resistance, thermal performance, sound insulation performance, and decorative performance. These requirements are often met by building materials such as mortars with different performances in traditional residential buildings. However, in the steel structure enclosure system, the surface of the steel structure with an anti-corrosion coating is very dense, smooth, and has a very low water absorption rate. The use of ordinary mortar cannot solve the problem of poor bonding performance with various cement-based mortars such as plaster mortar, bonding mortar, and inorganic thermal insulation mortar. Therefore, it is of great significance to study an interface treatment mortar suitable for steel structures. Summary of the invention

[0004] The technical problem to be solved by the present invention is: in view of the shortcomings of the prior art, a super-high ductility interface treatment mortar suitable for assembled steel structures and a preparation method thereof are provided, the mortar has excellent bonding and ductility properties, can resist external deformation and effectively bond the surface of the steel structure, and also reduce the risk of crack generation and cracking. The mortar preparation method is simple, easy to realize mechanized production, and has a variety of construction processes. Rolling, brushing, and scraping are used simultaneously, and mechanical spraying can also be realized.

[0005] In order to solve the above technical problems, the technical solution of the present invention is:

[0006] An ultra-high ductility interface treatment mortar suitable for assembled steel structures comprises the following components in parts by weight:

[0007] 530-770 parts of composite cementitious material, 450-550 parts of graded sand, 0.4-0.6 parts of water reducer, 1-2.5 parts of defoamer, 2-4 parts of cellulose ether, 2.5-5 parts of composite volume stabilizer, 1-3.5 parts of nano whisker modified PVA fiber; the composite cementitious material comprises VAE redispersible latex powder and ordinary silicate cement; the composite volume stabilizer comprises micro expansion agent, shrinkage reducing agent, nano SiO 2 .

[0008] Preferably, in the composite cementitious material, the mass ratio of the VAE redispersible latex powder to ordinary Portland cement is 1:(2.5-5).

[0009] Preferably, the graded sand is a mixture of 40-70 mesh sand and 70-100 mesh sand, and the mass ratio of 40-70 mesh sand to 70-100 mesh sand is 1:(0.5-2.5); further, preferably 1:(1.8-2.2).

[0010] Preferably, the nano whisker modified PVA fiber is a PVA fiber that is double-modified by nano silicon nitride whiskers and calcium carbonate whiskers. Furthermore, the preparation method of the nano whisker modified PVA fiber comprises the following steps:

[0011] 1. Mix silane coupling agent KH-560, silicon nitride whisker and PVA fiber in a mass ratio of 1: (1-1.5): (10-15), heat treat in a vacuum environment at 180-200° C. for 1-2 h, cool naturally after the heat treatment and place in an environment of (20±2)° C. and (35±5)% RH to obtain nano silicon nitride whisker modified PVA fiber for standby use;

[0012] 2. Mix a 10% triethoxymethylsilane solution, calcium carbonate whiskers and the nano-silicon nitride whisker-modified PVA fiber obtained in step 1 in a mass ratio of 1: (0.5-1): (0.1-0.5), treat in a 40°C water bath for 1-2 hours, then cool to room temperature and centrifuge, and disperse the centrifugal precipitate after drying to obtain the nano-whisker-modified PVA fiber.

[0013] Preferably, the silicon nitride whiskers are α-silicon nitride whiskers with a diameter of 20-30 μm and a length of 80-120 μm; and / or the PVA fibers are 5-6 mm in length and 20-30 μm in diameter; and / or the vacuum degree during the heat treatment is 0.15-0.2 MPa; and / or the calcium carbonate whiskers are aragonite calcium carbonate whiskers with a length of 20-30 μm, a diameter of 0.5-1.2 μm and a purity of 98%.

[0014] Preferably, the mass ratio of the silane coupling agent KH560, α-silicon nitride whisker, and PVA fiber is 1:(1-1.2):(10-15).

[0015] Preferably, the mass ratio of the 10% triethoxymethylsilane solution, calcium carbonate whiskers, and nano-silicon nitride whisker-modified PVA fibers is 1:(0.5-0.8):(0.1-0.2).

[0016] Preferably, the micro-expanding agent, shrinkage reducing agent, nano-SiO 2 The mass ratio is 1:(0.3-0.6):(0.3-0.7).

[0017] Preferably, it includes one or more of the following features:

[0018] The micro-expansion agent is a calcium micro-expansion agent, and the calcium micro-expansion agent is one of anhydrous calcium sulphoaluminate and calcium oxide;

[0019] The shrinkage reducing agent is one or a mixture of diethylene glycol monobutyl ether and dipropylene glycol monobutyl ether;

[0020] The water reducer is a polycarboxylic acid water reducer; and / or the defoamer is an organosilicon defoamer.

[0021] Preferably, the molecular weight of the cellulose ether is 100,000-200,000; the cellulose ether is one of hydroxyethyl methyl cellulose and hydroxypropyl methyl cellulose.

[0022] In order to better solve the above technical problems, the present invention also discloses the following technical solutions:

[0023] A method for preparing ultra-high ductility interface treatment mortar suitable for assembled steel structures comprises the following steps:

[0024] According to the metering ratio, the composite cementitious material, graded sand, water reducing agent, defoaming agent, cellulose ether, composite volume stabilizer and nano whisker modified PVA fiber are stirred and mixed uniformly to obtain an ultra-high ductility interface treatment mortar.

[0025] The ultra-high ductility interface treatment mortar can be used by adding water and stirring. The specific method of use is as follows: the ultra-high ductility interface treatment mortar of the present invention is mixed with water at a water-to-material ratio of 26-29%, the stirring speed is 200±5r / min, the stirring time is 5±1min, and it is allowed to stand for 1-2min to obtain a freshly mixed interface treatment mortar slurry, which can be used.

[0026] There are various construction methods for the above-mentioned newly mixed interface treatment mortar slurry during the specific construction, and any construction method including spraying, brushing, scraping and rolling can be realized. The thickness of a single construction layer is controlled at 2-3mm, and the interval between two construction processes shall not exceed 1-2d.

[0027] Due to the adoption of the above technical solution, the beneficial effects of the present invention are:

[0028] The present invention provides an ultra-high ductility interface treatment mortar suitable for assembled steel structures and a preparation method thereof. The mortar is compounded by composite cementitious materials, graded sand, polycarboxylic acid water reducer, silicone defoamer, cellulose ether, composite volume stabilizer and nano whisker modified PVA fiber. The prepared mortar has excellent bonding performance and ductility, can resist external deformation, effectively bond the surface of the steel structure and the surface of the steel structure coating, and also reduce the risk of crack generation and cracking. The preparation method provided by the present invention is simple, easy to realize mechanized production, and has a variety of construction processes. The methods of rolling, brushing, and scraping are carried out simultaneously, and mechanical spraying can also be realized. DETAILED DESCRIPTION

[0029] In order to more clearly understand the above-mentioned objectives, features and advantages of the present invention, the scheme of the present invention will be further described below. It should be noted that the embodiments of the present invention and the features in the embodiments can be combined with each other without conflict.

[0030] In the following description, many specific details are set forth to facilitate a full understanding of the present invention, but the present invention may also be implemented in other ways different from those described herein; it is obvious that the embodiments in the specification are only part of the embodiments of the present invention, rather than all of the embodiments.

[0031] In the following examples, unless otherwise specified, the raw materials are commercially available.

[0032] Example 1

[0033] A method for preparing ultra-high ductility interface treatment mortar suitable for assembled steel structures comprises the following steps:

[0034] S1. Mix silane coupling agent KH-560, silicon nitride whisker (α-silicon nitride whisker with a diameter of 20 μm and a length of 80 μm), and PVA fiber (length of 5 mm and diameter of 20 μm) in a mass ratio of 1:1:10, and heat treat it at 190°C for 2 h in a vacuum environment with a vacuum degree of 0.15 MPa. After the heat treatment, cool it naturally and place it in an environment of (20±2)°C and (35±5)% RH to obtain nano silicon nitride whisker modified PVA fiber for standby use;

[0035] S2, a 10% mass concentration of triethoxymethylsilane solution, calcium carbonate whiskers (aragonite calcium carbonate whiskers with a length of 20 μm, a diameter of 0.5 μm, and a purity of 98%) and the nano-silicon nitride whisker modified PVA fiber obtained in step 1 are mixed in a mass ratio of 1:0.5:0.1, treated in a 40°C water bath for 2 hours, then cooled to room temperature and centrifuged, and the centrifugal precipitate is dried at 40-45°C and then dispersed to obtain nano-whisker modified PVA fiber;

[0036] S3, by weight, 600 parts of composite cementitious materials (the mass ratio of VAE redispersible latex powder to ordinary Portland cement is 1:3), 500 parts of graded sand (the mass ratio of 40-70 mesh sand to 70-100 mesh sand is 2:3), 0.5 parts of polycarboxylic acid water reducer, 2 parts of silicone defoamer, 3 parts of hydroxyethyl methyl cellulose (molecular weight is 100,000), 3 parts of composite volume stabilizer (calcium oxide, diethylene glycol monobutyl ether, nano-SiO 2 The mass ratio of the two is 1:0.3:0.3), 2 parts of nano whisker modified PVA fiber are stirred and mixed evenly to obtain an ultra-high ductility interface treated mortar.

[0037] Example 2

[0038] A method for preparing ultra-high ductility interface treatment mortar suitable for assembled steel structures comprises the following steps:

[0039] S1. Mix silane coupling agent KH-560, silicon nitride whisker (α-silicon nitride whisker with a diameter of 20 μm and a length of 80 μm), and PVA fiber (length of 5 mm and diameter of 20 μm) in a mass ratio of 1:1.1:11, and heat-treat them at 190°C in a vacuum environment with a vacuum degree of 0.15 MPa. After the heat treatment, cool them naturally and place them in an environment of (20±2)°C and (35±5)% RH to obtain nano-silicon nitride whisker-modified PVA fiber for standby use.

[0040] S2, a 10% mass concentration of triethoxymethylsilane solution, calcium carbonate whiskers (aragonite calcium carbonate whiskers with a length of 20 μm, a diameter of 0.5 μm, and a purity of 98%) and the nano-silicon nitride whisker modified PVA fiber obtained in step 1 are mixed in a mass ratio of 1:0.6:0.1, treated in a 40°C water bath for 2 hours, then cooled to room temperature and centrifuged, and the centrifugal precipitate is dried at 40-45°C and then dispersed to obtain nano-whisker modified PVA fiber;

[0041] S3, by weight, 620 parts of composite cementitious materials (the mass ratio of VAE redispersible latex powder to ordinary Portland cement is 1:4), 530 parts of graded sand (the mass ratio of 40-70 mesh sand to 70-100 mesh sand is 1:2), 0.5 parts of polycarboxylic acid water reducer, 1.5 parts of silicone defoamer, 2.5 parts of cellulose ether (hydroxypropyl methylcellulose, molecular weight of 100,000), 3.5 parts of composite volume stabilizer (anhydrous calcium sulphoaluminate, diethylene glycol monobutyl ether, nano-SiO 2 The mass ratio of the nano whisker is 1:0.4:0.3), 2 parts of nano whisker modified PVA fiber are stirred and mixed evenly to obtain an ultra-high ductility interface treated mortar.

[0042] Example 3

[0043] A method for preparing ultra-high ductility interface treatment mortar suitable for assembled steel structures comprises the following steps:

[0044] S1. Mix silane coupling agent KH-560, silicon nitride whisker (α-silicon nitride whisker with a diameter of 20 μm and a length of 80 μm), and PVA fiber (length of 5 mm and diameter of 20 μm) in a mass ratio of 1:1.1:12, heat treat in a vacuum environment with a vacuum degree of 0.2 MPa at 190°C, cool naturally after the heat treatment and place in an environment of (20±2)°C and (35±5)% RH to obtain nano silicon nitride whisker modified PVA fiber for standby use;

[0045] S2, a 10% mass concentration of triethoxymethylsilane solution, calcium carbonate whiskers (aragonite calcium carbonate whiskers with a length of 20 μm, a diameter of 0.5 μm, and a purity of 98%) and the nano-silicon nitride whisker modified PVA fiber obtained in step 1 are mixed in a mass ratio of 1:0.7:0.1, treated in a 40°C water bath for 2 hours, then cooled to room temperature and centrifuged, and the centrifugal precipitate is dried at 40-45°C and then dispersed to obtain nano-whisker modified PVA fiber;

[0046] S3, by weight, 620 parts of composite cementitious materials (the mass ratio of VAE redispersible latex powder to ordinary Portland cement is 1:3.2), 500 parts of graded sand (the mass ratio of 40-70 mesh sand to 70-100 mesh sand is 1:2.2), 0.5 parts of polycarboxylic acid water reducer, 1.5 parts of silicone defoamer, 3 parts of cellulose ether (hydroxyethyl methyl cellulose, molecular weight of 100,000), 3.5 parts of composite volume stabilizer (calcium oxide, diethylene glycol monobutyl ether, nano-SiO 2 The mass ratio of the nano whisker is 1:0.3:0.5), 3 parts of nano whisker modified PVA fiber are stirred and mixed evenly to obtain an ultra-high ductility interface treated mortar.

[0047] Example 4

[0048] A method for preparing ultra-high ductility interface treatment mortar suitable for assembled steel structures comprises the following steps:

[0049] S1. Mix silane coupling agent KH-560, silicon nitride whisker (α-silicon nitride whisker with a diameter of 20 μm and a length of 80 μm), and PVA fiber (length of 5 mm and diameter of 20 μm) in a mass ratio of 1:1.2:15, and heat-treat them at 190°C in a vacuum environment with a vacuum degree of 0.15 MPa. After the heat treatment, cool them naturally and place them in an environment of (20±2)°C and (35±5)% RH to obtain nano-silicon nitride whisker-modified PVA fiber for standby use.

[0050] S2, a 10% mass concentration of triethoxymethylsilane solution, calcium carbonate whiskers (aragonite calcium carbonate whiskers with a length of 20 μm, a diameter of 0.5 μm, and a purity of 98%) and the nano-silicon nitride whisker modified PVA fiber obtained in step 1 are mixed in a mass ratio of 1:0.8:0.2, treated in a 40°C water bath for 2 hours, then cooled to room temperature and centrifuged, and the centrifugal precipitate is dried at 40-45°C and then dispersed to obtain nano-whisker modified PVA fiber;

[0051] S3, by weight, 700 parts of composite cementitious materials (the mass ratio of VAE redispersible latex powder to ordinary Portland cement is 1:5), 520 parts of graded sand (the mass ratio of 40-70 mesh sand to 70-100 mesh sand is 1:1.8), 0.6 parts of polycarboxylic acid water reducer, 2.5 parts of silicone defoamer, 4 parts of cellulose ether (hydroxypropyl methylcellulose, molecular weight of 200,000), 4 parts of composite volume stabilizer (anhydrous calcium sulphoaluminate, dipropylene glycol monobutyl ether, nano-SiO 2 The mass ratio of the raw materials is 1:0.6:0.5), 3.5 parts of nano whisker modified PVA fiber are stirred and mixed evenly to obtain an ultra-high ductility interface treated mortar.

[0052] In order to verify the effect of nano whisker modified PVA fiber on the performance of ultra-high ductility interface mortar, further explanation is given below in combination with comparative examples 1-5.

[0053] Comparative Example 1

[0054] Compared with Example 1, the PVA fiber of this comparative example is only modified by nano silicon nitride whiskers, and other conditions are the same as those of Example 1.

[0055] Comparative Example 2

[0056] Compared with Example 1, the PVA fiber of this comparative example is only modified by calcium carbonate whiskers, and other conditions are the same as those of Example 1.

[0057] Comparative Example 3

[0058] Compared with Example 1, the PVA fiber of this comparative example is not modified by whiskers, and other conditions are the same as those of Example 1.

[0059] Comparative Example 4

[0060] Compared with Example 1, the nanowhisker modified PVA fiber of this comparative example is not heat treated, and other conditions are the same as those of Example 1.

[0061] Comparative Example 5

[0062] Compared with Example 1, the interface treatment mortar in this comparative example does not add nano whisker modified PVA fibers, and other conditions are the same as those in Example 1.

[0063] In order to verify the effect of the composite volume stabilizer on the performance of the interface treated mortar, further explanation is given below in conjunction with Comparative Example 6.

[0064] Comparative Example 6

[0065] Compared with Example 1, in this comparative example, no SiO is added to the composite volume stabilizer. 2 , other conditions are the same as in Example 1.

[0066] Comparative Example 7

[0067] Compared with Example 1, in this comparative example, diethylene glycol monobutyl ether is not added to the composite volume stabilizer, and other conditions are the same as those in Example 1.

[0068] Comparative Example 8

[0069] Compared with Example 1, in this comparative example, calcium oxide is not added to the composite volume stabilizer, and other conditions are the same as those in Example 1.

[0070] Application Examples

[0071] The interface treatment mortar powder prepared in the above embodiments and comparative examples was mixed with water at a water-to-material ratio of 25%, with a stirring speed of 200±5r / min and a stirring time of 5±1min. The mixture was allowed to stand for 2min to obtain a freshly mixed interface treatment mortar slurry.

[0072] The performance of the freshly mixed interface treated mortar slurry was tested. The test method and test results are as follows:

[0073] 1. Tensile bond strength, consistency value, free shrinkage rate: Tested in accordance with JGJ / T70-2009 "Test Method for Basic Properties of Building Mortar".

[0074] 2. Lateral deformation: Test according to the method in Appendix A of JC / T 1004-2017 "Ceramic Tile Grout".

[0075] 3. Compression-fold ratio: Test the compressive strength and flexural strength according to the JC / T 1004-2017 "Ceramic Tile Sealant" standard, and calculate the compression-fold ratio.

[0076] The test results are shown in Table 1 and Table 2.

[0077] Table 1

[0078]

[0079]

[0080] Table 2

[0081] Consistency value / mm Free shrinkage / % Transverse deformation / mm Compression ratio Construction Example 1 113 0.08 5.12 2.74 good Example 2 112 0.06 5.24 2.84 good Example 3 118 0.09 4.98 2.79 good Example 4 114 0.08 5.23 2.91 good Comparative Example 1 115 0.12 1.00 3.06 good Comparative Example 2 113 0.11 1.25 2.98 good Comparative Example 3 111 0.19 2.12 3.45 good Comparative Example 4 112 0.15 1.89 3.56 good Comparative Example 5 110 0.16 1.57 3.21 good Comparative Example 6 115 0.16 2.36 3.15 good Comparative Example 7 112 0.17 2.52 3.26 good Comparative Example 8 114 0.19 1.54 3.17 good

[0082] It can be seen from the test results in Table 1 and Table 2 that, compared with the comparative example, the present invention adds an appropriate amount of nano whisker modified PVA fiber to the mortar matrix for modification, and adds diethylene glycol monobutyl ether, SiO 2 , and calcium oxide, and at the same time adding graded sand, polycarboxylic acid water reducer, silicone defoaming agent, etc., the prepared mortar has good bonding properties, can resist external deformation, effectively bond the surface of steel structures and the surface of steel structure coatings, and also reduce the risk of cracks and cracking. It has good volume stability and excellent mechanical properties.

[0083] Comparative Examples 1-5 are compared with Example 1. In Example 1, PVA fibers modified by calcium carbonate whiskers and silicon nitride whiskers are added to form a relatively stable network structure in the mortar matrix, thereby improving the volume stability of the mortar, releasing crack stress, and appropriately improving the ductility of the mortar. In addition, the PVA fibers are modified by silicon nitride whiskers and calcium carbonate whiskers, and the microstructure of silicon nitride whiskers helps to increase the bonding force of the mortar, making the bonding between the mortar and the substrate more firm. At the same time, the presence of calcium carbonate whiskers can improve the chemical and physical interactions with the cement matrix, and enhance the consistency and bonding strength.

[0084] Compared with Example 1, Comparative Examples 6-8 use a single type of volume stabilizer, and the volume stability of the mortar is significantly reduced; while Example 1 uses diethylene glycol monobutyl ether, SiO 2 , calcium oxide, and a composite volume stabilizer. Diethylene glycol monobutyl ether is a surfactant that can reduce the surface tension of the mortar and improve its fluidity. It provides a lubricating effect in the mortar, making it easier to operate and evenly fill during construction. SiO 2 It has excellent bonding properties, which can enhance the adhesion between mortar and substrate, and improve the interaction between cement particles. 2The microstructure provides more binding sites and promotes the structural formation of cement paste; calcium oxide forms calcium hydroxide during the hydration process, which helps to regulate the expansion of the mortar, thereby offsetting the volume change caused by drying shrinkage. The three work together to not only improve the mechanical properties of the mortar, but also increase the volume stability of the mortar.

[0085] Specific examples are used herein to illustrate the principles and implementation methods of the present invention. The description of the above embodiments is only used to help understand the method of the present invention and its core ideas, including the best mode, and also enable any technician in the field to practice the present invention, including making and using any device or system, and implementing any combined method. It should be pointed out that for ordinary technicians in this technical field, without departing from the principle of the present invention, the present invention can also be improved and modified, and these improvements and modifications also fall within the scope of protection of the claims of the present invention. The scope of patent protection of the present invention is defined by the claims and may include other embodiments that can be thought of by those skilled in the art. If these other embodiments have structural elements similar to the literal expression of the claims, or if they include equivalent structural elements that are not substantially different from the literal expression of the claims, then these other embodiments should also be included in the scope of the claims.

Claims

1. An ultra-high ductility interface treatment mortar suitable for assembled steel structures, It is characterized in that In parts by weight, it includes the following components: 530-770 parts of composite cementitious material, 450-550 parts of graded sand, 0.4-0.6 parts of water reducing agent, 1-2.5 parts of defoaming agent, 2-4 parts of cellulose ether, 2.5-5 parts of composite volume stabilizer, 1-3.5 parts of nano whisker modified PVA fiber; the composite cementitious material comprises VAE redispersible latex powder and ordinary silicate cement; the composite volume stabilizer comprises micro expansion agent, shrinkage reducing agent, nano SiO 2 .

2. According to claim 1, an ultra-high ductility interface treatment mortar suitable for assembled steel structures, It is characterized in that In the composite cementitious material, the mass ratio of the VAE redispersible latex powder to ordinary Portland cement is 1:(2.5-5).

3. The ultra-high ductility interface treatment mortar suitable for assembled steel structures according to claim 1, It is characterized in that The graded sand is a mixture of 40-70 mesh sand and 70-100 mesh sand, and the mass ratio of 40-70 mesh sand to 70-100 mesh sand is 1:(0.5-2.5).

4. The ultra-high ductility interface treatment mortar suitable for assembled steel structures according to claim 1, It is characterized in that The nano whisker modified PVA fiber is a PVA fiber that is double-modified by nano silicon nitride whiskers and calcium carbonate whiskers.

5. The ultra-high ductility interface treatment mortar suitable for assembled steel structures according to claim 4, It is characterized in that The preparation method of the nano whisker modified PVA fiber comprises the following steps:

1. Mix silane coupling agent KH-560, silicon nitride whisker and PVA fiber in a mass ratio of 1: (1-1.5): (10-15), heat treat in a vacuum environment at 180-200° C. for 1-2 h, cool naturally after the heat treatment and place in an environment of (20±2)° C. and (35±5)% RH to obtain nano silicon nitride whisker modified PVA fiber for standby use; 2. Mix a 10% triethoxymethylsilane solution, calcium carbonate whiskers and the nano-silicon nitride whisker-modified PVA fiber obtained in step 1 in a mass ratio of 1: (0.5-1): (0.1-0.5), treat in a 40°C water bath for 1-2 hours, then cool to room temperature and centrifuge, and disperse the centrifugal precipitate after drying to obtain the nano-whisker-modified PVA fiber.

6. The ultra-high ductility interface treatment mortar suitable for assembled steel structures according to claim 5, It is characterized in that The silicon nitride whisker is an α-silicon nitride whisker with a diameter of 20-30 μm and a length of 80-120 μm; and / or the PVA fiber has a length of 5-6 mm and an average diameter of 20-30 μm; and / or the vacuum degree during the heat treatment is 0.15-0.2 MPa; and / or the calcium carbonate whisker is an aragonite calcium carbonate whisker with a length of 20-30 μm, a diameter of 0.5-1.2 μm and a purity of 98%.

7. The ultra-high ductility interface treatment mortar suitable for assembled steel structures according to claim 1, It is characterized in that The micro-expanding agent, shrinkage reducing agent, nano-SiO 2 The mass ratio is 1:(0.3-0.6):(0.3-0.7).

8. The ultra-high ductility interface treatment mortar suitable for assembled steel structures according to claim 7, It is characterized in that Include one or more of the following characteristics: The micro-expansion agent is a calcium micro-expansion agent, and the calcium micro-expansion agent is one of anhydrous calcium sulphoaluminate and calcium oxide; The shrinkage reducing agent is one or a mixture of diethylene glycol monobutyl ether and dipropylene glycol monobutyl ether; The water reducer is a polycarboxylate water reducer; The defoamer is an organosilicon defoamer.

9. The ultra-high ductility interface treatment mortar suitable for assembled steel structures according to claim 1, It is characterized in that The molecular weight of the cellulose ether is 100,000-200,000; the cellulose ether is one of hydroxyethyl methyl cellulose and hydroxypropyl methyl cellulose.

10. A method for preparing an ultra-high ductility interface treatment mortar suitable for assembled steel structures according to any one of claims 1 to 9, It is characterized in that The following steps are involved: According to the metering ratio, the composite cementitious material, graded sand, water reducing agent, defoaming agent, cellulose ether, composite volume stabilizer and nano whisker modified PVA fiber are stirred and mixed uniformly to obtain an ultra-high ductility interface treatment mortar.

Citation Information

Cited By

  • Moisturizing anti-cracking high-ductility concrete and preparation method thereof

    CN119661164A

  • Moisturizing and crack-resistant high-ductility concrete and preparation method thereof

    CN119661164B