High-fracture-toughness long-period quaternary oxide thermal barrier coating material and preparation method thereof

CN118955125AActive Publication Date: 2024-11-15XIDIAN UNIV
View PDF 6 Cites 0 Cited by

Patent Information

Application Number
CN202411006420.0
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-07-25
Publication Date
2024-11-15
Estimated Expiration
2044-07-25

AI Technical Summary

Technical Problem

[0004]为了克服上述现有技术中的缺点,本发明的目的在于提供一种长周期四元氧化物热障涂层材料及其制备方法,通过掺杂元素Me,Me为Zr、Gd、Y、Nb、Ti中的一种,优化四元氧化物的组分,利用高温固相反应合成技术,成功制备出具有优异热稳定性和高断裂韧性的热障涂层材料,能够解决现有技术中热障涂层易剥落、寿命短的技术问题;此外,本发明的制备方法工艺简单,可操作性强,适合大规模生产,通过本发明制备方法制备得到的MexHf6Ta2O17+y热障涂层材料能够用于航空航天、发电设备等高温环境中

Benefits of technology

[0023] 1. The present invention uses metal oxide raw materials with a particle size of 1-3 μm. The uniform particle size difference is small, allowing full reaction between different metal oxide powders, reducing local defects and uneven structures that may exist in the material, and improving the Homogeneity of materials and consistency of performance.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118955125A_ABST
    Figure CN118955125A_ABST
Patent Text Reader

Abstract

The invention discloses a high-fracture-toughness long-period quaternary oxide thermal barrier coating material and a preparation method thereof.The material is a quaternary single-phase solid solution oxide of a long-period structure, the chemical formula of the oxide is MexHf6Ta2O17 + y, and a doping element Me is one of Zr, Gd, Y, Nb and Ti; the thermal barrier coating material with excellent thermal stability and high fracture toughness is prepared by introducing a doping element Me, optimizing components of quaternary oxide and utilizing a high-temperature solid-phase reaction synthesis technology. The thermal barrier coating material prepared by the method has the characteristics of uniform components, high density, high chemical purity and high fracture toughness.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention belongs to the technical field of thermal barrier coating materials, and in particular relates to a high fracture toughness long period quaternary oxide thermal barrier coating material and a preparation method thereof. Background Art

[0002] With the continuous improvement of thrust-to-weight ratio of high-performance aircraft engines, engine turbine blades are required to withstand higher temperatures. In 1953, NASA proposed to coat the surface of high-temperature alloy blades with a high-temperature resistant and high-insulation protective coating system, namely thermal barrier coating. Studies have shown that a thermal barrier coating with a thickness of 250μm can reduce the substrate temperature by 110 to 170°C. Therefore, thermal barrier coatings are considered to be the most feasible technology to significantly increase the service temperature of aircraft engine turbine blades. They have become an indispensable thermal protection material for the hot end components of aircraft engine turbine blades, and to a great extent determine the performance and development level of the engine. The thermal barrier coating material currently used for aircraft engine turbine blades in service is yttria partially stabilized zirconia, but this coating will undergo phase change after long-term service in an environment above 1200°C, resulting in a sharp decrease in service life.

[0003] The Chinese invention patent with publication number CN114368969A discloses a TiSi2-doped Gd2Zr2O7 ceramic material, preparation method and thermal barrier coating. The thermal barrier coating prepared by doping the Gd2Zr2O7 thermal barrier coating ceramic material with TiSi2 has a maximum fracture toughness of only 1.83MPa·m at room temperature. 1 / 2 The invention patent with announcement number CN111925211B discloses an A2B2O7 type rare earth tantalate ceramic and its preparation method. According to the structural formula of RE2MTaO7, RE2O3 and M2O3 are dissolved in concentrated nitric acid respectively for reaction, and the pH is adjusted to not less than 1.5, and then TaOCl3 solution is added dropwise, stirring continuously, and ammonia water is added to stabilize the system pH at 9-10, and stirring is continued in a water bath environment, and then the precipitate is washed with deionized water until the pH is 7, and the obtained filter cake is placed in an oven for drying, and then sieved for use; the powder is placed in a graphite grinder, and spark plasma sintering is carried out in a sintering furnace, and then the sintered sample is annealed and decarbonized to obtain a dense RE2MTaO7 block, and the RE2MTaO7 block is about 1.7MPa·m 1 / 2 The fracture toughness of the ceramic materials in the above prior art is 2.0MPa·m 1 / 2 The following results in limited high-temperature service life and inability to be used in industrial production. Summary of the invention

[0004] In order to overcome the shortcomings of the above-mentioned prior art, the purpose of the present invention is to provide a long-period quaternary oxide thermal barrier coating material and a preparation method thereof. By doping the element Me, Me is one of Zr, Gd, Y, Nb, and Ti, the components of the quaternary oxide are optimized, and a thermal barrier coating material with excellent thermal stability and high fracture toughness is successfully prepared by using a high-temperature solid-phase reaction synthesis technology, which can solve the technical problems of easy peeling and short life of the thermal barrier coating in the prior art; in addition, the preparation method of the present invention has a simple process, strong operability, and is suitable for large-scale production. The Me prepared by the preparation method of the present invention x Hf6Ta2O 17+y Thermal barrier coating materials can be used in high temperature environments such as aerospace and power generation equipment.

[0005] In order to achieve the above object, the technical solution adopted by the present invention is as follows:

[0006] A high fracture toughness long period quaternary oxide thermal barrier coating material, the thermal barrier coating material is a quaternary single-phase solid solution oxide with a long period structure, the chemical formula of the oxide is Me x Hf6Ta2O 17+y , wherein the doping element Me is one of Zr, Gd, Y, Nb, and Ti. When Me is Zr, x=3, y=6; when Me is Y, x=4, y=6; when Me is Gd, x=2, y=3; when Me is Nb, x=2, y=5; when Me is Ti, x=2, y=4.

[0007] The raw materials of the thermal barrier coating material include Me x O y , HfO2 and Ta2O5, among which Me x O y The molar ratio of HfO2 and Ta2O5 is (1-3):6:1; the Me x O y , HfO2 and Ta2O5 have a particle size of 1-3 μm.

[0008] A method for preparing the above-mentioned high fracture toughness long period quaternary oxide thermal barrier coating material comprises the following steps:

[0009] Step 1: Mix the raw materials x O y , HfO2 and Ta2O5 were wet-milled to obtain a mixed slurry; in terms of molar ratio, Me x O y :HfO2:Ta2O5=(1-3):6:1;

[0010] Step 2: heating and evaporating the mixed slurry obtained in step 1, and then grinding to obtain a mixed powder with a particle size greater than 100 mesh;

[0011] Step 3: calcine the mixed powder obtained in step 2 in air or oxygen atmosphere at 1100-1300°C for 6-9h to obtain powdered Me x Hf6Ta2O 17+y Thermal barrier coating material, that is, high fracture toughness long period quaternary oxide thermal barrier coating material in powder form.

[0012] In step 1, Me x O y The powder purity of HfO2 and Ta2O5 is ≥99%.

[0013] In step 1, the ball milling time is 4-8 hours, zirconium oxide balls are used as ball milling media, anhydrous ethanol is used as liquid medium, the ball-to-material ratio is 3:1, and the rotation speed is 300-350 r / min.

[0014] In the step 2, a magnetic stirrer is used for heating and evaporation, the stirring speed is 1000-1500 r / min, and the heating temperature is 180-220°C.

[0015] The preparation method of the present invention also includes:

[0016] Step 4: Mix the powdered adhesive in step 3 x Hf6Ta2O 17+y The thermal barrier coating material is granulated and then sieved to obtain agglomerated powder with a sieve mesh number of 100-200 meshes;

[0017] Step 5: Pre-press the agglomerated powder obtained in step 4 to obtain a green blank; then perform cold isostatic pressing on the green blank to obtain Me x Hf6Ta2O 17+y Ceramic body;

[0018] Step 6: Take the Me obtained in step 5 x Hf6Ta2O 17+y The ceramic body is debonded, then calcined at 1500-1800℃ for 6-9h, and cooled to room temperature to obtain a block of Me x Hf6Ta2O 17+y Thermal barrier coating material, that is, a block-like high fracture toughness long-period quaternary oxide thermal barrier coating material.

[0019] In step 4, the adhesive is a polyvinyl alcohol solution or a polyvinyl pyrrolidone solution, and the mass fraction of the adhesive is 1-3%, and the mass of the adhesive added accounts for 1% of the powder Me in step 3. x Hf6Ta2O 17+y 0.2-0.6% of the mass of thermal barrier coating material.

[0020] The pre-pressing pressure in step 5 is 100-150 MPa; the cold isostatic pressing pressure is 150-280 MPa, and the holding time is 10-30 min.

[0021] The debinding operation in step 6 is specifically as follows: x Hf6Ta2O 17+y The ceramic body is placed in air or oxygen atmosphere and kept at 400-600° C. for 4-6 hours.

[0022] Compared with the prior art, the present invention has the following beneficial effects:

[0023] 1. The present invention uses metal oxide raw materials with a particle size of 1-3 μm, and the particle size is uniform and has small differences, so that different metal oxide powders can fully react with each other, reducing possible local defects and uneven structures in the material, and improving the homogeneity of the material and the consistency of performance.

[0024] 2. The present invention uses a metal oxide of one of Zr, Gd, Y, Nb, and Ti to prepare a quaternary oxide thermal barrier coating material. The selected metal ions have a small difference in radius and are easier to diffuse with each other at high temperatures, which promotes the formation of a single-phase oxide, enhances the reaction efficiency between different components during the sintering process, and can reduce sintering defects.

[0025] 3. The evaporation process adopted in the present invention enables the slurry after ball milling to remain in a uniformly mixed state during the drying process, and will not cause stratification during the precipitation process due to the different relative molecular masses of the raw materials. It ensures that the oxide raw materials can fully react during the sintering process, improves the homogeneity and performance stability of the material, meets the use requirements, and significantly improves the quality and reliability of the final product.

[0026] 4. The solid phase sintering process adopted in the present invention to synthesize the thermal barrier coating material does not introduce foreign phases, thus avoiding the contamination of the material during the preparation process, and can obtain a thermal barrier coating material with uniform composition, high density and high chemical purity.

[0027] 5. The present invention optimizes the composition of quaternary oxides by doping one of Zr, Gd, Y, Nb, and Ti to prepare a long-period quaternary oxide thermal barrier coating material. Compared with the ternary oxide thermal barrier coating material in the prior art, the fracture toughness of the material is at least 2.0 Mpa·m 1 / 2 , improving its high temperature service life.

[0028] In summary, the present invention optimizes the composition of the quaternary oxide by doping one of Zr, Gd, Y, Nb, and Ti to prepare a long-period quaternary oxide Me x Hf6Ta2O 17+yThermal barrier coating material, the material maintains a single phase, and compared with other single-phase ternary rare earth tantalate thermal barrier coating materials, the thermal barrier coating material prepared by the present invention has significantly improved fracture toughness, the improvement is more than 30%. x Hf6Ta2O 17+y Thermal barrier coating materials are expected to be applied to aircraft engine turbine blades to achieve high-temperature and long-life service of thermal barrier coatings, which has higher practical value. BRIEF DESCRIPTION OF THE DRAWINGS

[0029] Figure 1 Me provided by the present invention x Hf6Ta2O 17+y XRD pattern of thermal barrier coating materials.

[0030] Figure 2 The Zr3Hf6Ta2O provided in Example 1 of the present invention 23 SEM image of thermal barrier coating material.

[0031] Figure 3 The Zr3Hf6Ta2O provided in Example 1 of the present invention 23 TEM image of thermal barrier coating material, where: Figure 3 (a) is low resolution, Figure 3 (b) is high resolution, Figure 3 (c) is the EDX scan of Hf element. Figure 3 (d) is the EDX scan of Zr element, 3(e) is the EDX scan of Ta element, Figure 3 (f) is the EDX scan image of O element. DETAILED DESCRIPTION

[0032] The technical solution of the present invention is further described below in conjunction with the accompanying drawings and embodiments.

[0033] A high fracture toughness long period quaternary oxide thermal barrier coating material, the thermal barrier coating material is a quaternary single-phase solid solution oxide with a long period structure, the chemical formula of the oxide is Me x Hf6Ta2O 17+y , wherein the doping element Me is one of Zr, Gd, Y, Nb, and Ti, wherein when Me is Zr, x=3, y=6; when Me is Y, x=4, y=6; when Me is Gd, x=2, y=3; when Me is Nb, x=2, y=5; when Me is Ti, x=2, y=4; the raw materials of the thermal barrier coating material include Me x O y , HfO2 and Ta2O5, among which Me x O y , HfO2 and Ta2O5 in a molar ratio of (1-3):6:1; the Me xO y , HfO2 and Ta2O5 have a particle size of 1-3 μm.

[0034] A method for preparing a high fracture toughness long period quaternary oxide thermal barrier coating material comprises the following steps:

[0035] Step 1: Mix the raw materials x O y , HfO2 and Ta2O5 were wet-milled for 4-8 hours to obtain a mixed slurry; zirconia balls were used as the ball milling medium, anhydrous ethanol was used as the liquid medium, the ball-to-material ratio was 3:1, and the rotation speed was 300-350r / min; in terms of molar ratio, Me x O y :HfO2:Ta2O5=(1-3):6:1,Me x O y The powder purity of HfO2 and Ta2O5 is ≥99%; x O y , HfO2 and Ta2O5 have a particle size of 1-3 μm;

[0036] Step 2: heating and drying the mixed slurry obtained in step 1 with a magnetic stirrer to prevent the oxides from being demixed during drying due to different relative molecular weights, wherein the speed of the magnetic stirrer is 1000-1500 r / min and the heating temperature is 180-220° C., followed by grinding to obtain a mixed powder with uniform particle size greater than 100 mesh;

[0037] Step 3: The mixed powder obtained in step 2 is calcined in air or oxygen atmosphere at 1100-1300°C for 6-9h. The atoms on the surface of the solid particles diffuse with each other to react chemically, and the grains grow initially to obtain powdered Me x Hf6Ta2O 17+y Thermal barrier coating material, that is, a powdery high fracture toughness long period quaternary oxide thermal barrier coating material, the reaction equation is Me x O y +6HfO2+Ta2O5=Me x Hf6Ta2O 17+y ;

[0038] Step 4: Add the adhesive to the powdered Me in step 3 x Hf6Ta2O 17+y The thermal barrier coating material is granulated and then sieved to obtain an agglomerated powder with a sieve mesh of 100-200 mesh. The adhesive is a polyvinyl alcohol solution or a polyvinyl pyrrolidone solution, and the mass fraction of the adhesive is 1-3%. The mass of the adhesive added accounts for 3% of the powder. x Hf6Ta2O 17+y0.2-0.6% of the mass of thermal barrier coating materials;

[0039] Step 5: Using a mold with a diameter of 20 mm, the agglomerated powder obtained in step 4 is pre-pressed to obtain a blank, wherein the pre-pressing pressure is 100-150 MPa; then the blank is cold isostatically pressed to obtain Me x Hf6Ta2O 17+y The ceramic embryo body, the cold isostatic pressing pressure is 150-280MPa, and the holding time is 10-30min;

[0040] Step 6: Take the Me obtained in step 5 x Hf6Ta2O 17+y The ceramic body is placed in air or oxygen atmosphere at 400-600℃ for 4-6 hours to remove the binder, so that the adhesive decomposes and volatilizes to avoid high-temperature carbonization and contamination of the body. Then it is calcined at 1500-1800℃ for 6-9 hours, and the grains grow and combine to fill the gaps to complete densification. It is cooled to room temperature with the furnace to obtain a high-density block of Me x Hf6Ta2O 17+y Thermal barrier coating material, that is, a block-like high fracture toughness long-period quaternary oxide thermal barrier coating material.

[0041] The fracture toughness of the thermal barrier coating material in the form of a block is at least 2.0 Mpa·m 1 / 2 .

[0042] Example 1

[0043] A Zr3Hf6Ta2O 23 A thermal barrier coating material, wherein the raw materials of the thermal barrier coating material include ZrO2, HfO2 and Ta2O5, wherein the molar ratio of ZrO2, HfO2 and Ta2O5 is 3:6:1.

[0044] A Zr3Hf6Ta2O 23 A method for preparing a thermal barrier coating material comprises the following steps:

[0045] Step 1: wet-milling ZrO2, HfO2 and Ta2O5 at a raw material molar ratio of 3:6:1 at 300 r / min for 6 hours to obtain a mixed slurry; the particle sizes of ZrO2, HfO2 and Ta2O5 are all 1-3 μm, and the purity is all 99%;

[0046] Step 2: The mixed slurry obtained in step 1 is evaporated to dryness at 1000 r / min and 180° C., and then ground to obtain a mixed powder with a uniform particle size greater than 100 mesh;

[0047] Step 3: The mixed powder obtained in step 2 was calcined in an air atmosphere at 1100°C for 9 hours, and then cooled to room temperature to obtain Zr3Hf6Ta2O in powder form. 23 Thermal barrier coating materials;

[0048] Step 4: Add 2% polyvinyl alcohol solution into the powdered Zr3Hf6Ta2O 23 The thermal barrier coating material is granulated and sieved to obtain agglomerated powder with a sieve mesh of 100-200 mesh, and the mass of the adhesive added accounts for 100% of the Zr3Hf6Ta2O powder in step 3. 23 0.4% of the mass of thermal barrier coating materials;

[0049] Step 5: The agglomerated powder obtained in step 4 is pre-pressed at 150 MPa to obtain a green blank, and then the green blank is cold isostatically pressed at 280 MPa for 10 min to obtain Zr3Hf6Ta2O 23 Ceramic body;

[0050] Step 6: Zr3Hf6Ta2O obtained in step 5 23 The ceramic body was placed in an air atmosphere at 600 °C for 4 h to remove binder, then calcined at 1500 °C for 9 h, and cooled to room temperature to obtain a bulk Zr3Hf6Ta2O 23 Thermal barrier coating materials.

[0051] The bulk Zr3Hf6Ta2O 23 The fracture toughness of the thermal barrier coating material is 2.43±0.09Mpa·m 1 / 2 .

[0052] Example 2

[0053] A Gd2Hf6Ta2O 20 A thermal barrier coating material, wherein the raw materials of the thermal barrier coating material include Gd2O3, HfO2 and Ta2O5, wherein the molar ratio of Gd2O3, HfO2 and Ta2O5 is 1:6:1.

[0054] A Gd2Hf6Ta2O 20 A method for preparing a thermal barrier coating material comprises the following steps:

[0055] Step 1: wet-milling Gd2O3, HfO2 and Ta2O5 at a raw material molar ratio of 1:6:1 at 320 r / min for 7 hours to obtain a mixed slurry; the particle sizes of the Gd2O3, HfO2 and Ta2O5 are all 1-3 μm, and the purity is 99%;

[0056] Step 2: evaporate the mixed slurry obtained in step 1 to dryness at 1100 r / min and 190° C., and then grind to obtain a mixed powder with uniform particle size greater than 100 mesh;

[0057] Step 3: The mixed powder obtained in step 2 was calcined in an oxygen atmosphere at 1200°C for 6 hours, and then cooled to room temperature to obtain powdered Gd2Hf6Ta2O 20 Thermal barrier coating materials;

[0058] Step 4: Add 3% polyvinyl pyrrolidone solution into the powdered Gd2Hf6Ta2O 20 The thermal barrier coating material is granulated and sieved to obtain agglomerated powder with a sieve mesh of 100-200 mesh, and the mass of the adhesive added accounts for 100% of the powdered Gd2Hf6Ta2O 20 0.6% of the mass of thermal barrier coating materials;

[0059] Step 5: The agglomerated powder obtained in step 4 is pre-pressed at 120 MPa to obtain a green blank, and then the green blank is cold isostatically pressed at 200 MPa for 15 min to obtain Gd2Hf6Ta2O 20 Ceramic body;

[0060] Step 6: Gd2Hf6Ta2O obtained in step 5 20 The ceramic body was placed in an oxygen atmosphere at 400 °C for 6 h to remove binder, then calcined at 1800 °C for 8 h, and cooled to room temperature to obtain Gd2Hf6Ta2O in bulk. 20 Thermal barrier coating materials.

[0061] The bulk Gd2Hf6Ta2O 20 The fracture toughness of the thermal barrier coating material is 2.26±0.09Mpa·m 1 / 2 .

[0062] Example 3

[0063] A Y4Hf6Ta2O 23 A thermal barrier coating material, wherein the raw materials of the thermal barrier coating material include Y2O3, HfO2 and Ta2O5, wherein the molar ratio of Y2O3, HfO2 and Ta2O5 is 2:6:1.

[0064] A Y4Hf6Ta2O 23 A method for preparing a thermal barrier coating material comprises the following steps:

[0065] Step 1: wet-milling Y2O3, HfO2 and Ta2O5 at a raw material molar ratio of 2:6:1 at 340 r / min for 5 hours to obtain a mixed slurry; the particle sizes of Y2O3, HfO2 and Ta2O5 are all 1-3 μm, and the purity is 99%;

[0066] Step 2: The mixed slurry obtained in step 1 is evaporated to dryness at 1200 r / min and 200° C., and then ground to obtain a mixed powder with a uniform particle size greater than 100 mesh;

[0067] Step 3: The mixed powder obtained in step 2 was calcined in an air atmosphere at 1300°C for 7 hours, and then cooled to room temperature to obtain powdered Y4Hf6Ta2O 23 Thermal barrier coating materials;

[0068] Step 4: Add 3% polyvinyl alcohol solution into the powdered Y4Hf6Ta2O 23 The thermal barrier coating material is granulated and sieved to obtain agglomerated powder with a sieve mesh of 100-200 mesh, and the mass of the adhesive added accounts for 100% of the Y4Hf6Ta2O powder in step 3. 23 0.6% of the mass of thermal barrier coating materials;

[0069] Step 5: The agglomerated powder obtained in step 4 is pre-pressed at 100 MPa to obtain a green blank, and then the green blank is cold isostatically pressed at 260 MPa for 20 min to obtain Y4Hf6Ta2O 23 Ceramic body,

[0070] Step 6: Y4Hf6Ta2O obtained in step 5 23 The ceramic body was placed in an air atmosphere at 600 °C for 5 h to remove binder, then calcined at 1700 °C for 6 h and cooled to room temperature to obtain a block of Y4Hf6Ta2O 23 Thermal barrier coating materials.

[0071] The bulk Y4Hf6Ta2O 23 The fracture toughness of the thermal barrier coating material is 2.36±0.29Mpa·m 1 / 2 .

[0072] Example 4

[0073] A Nb2Hf6Ta2O 22 A thermal barrier coating material, wherein the raw materials of the thermal barrier coating material include Nb2O5, HfO2 and Ta2O5, wherein the molar ratio of Nb2O5, HfO2 and Ta2O5 is 1:6:1.

[0074] A Nb2Hf6Ta2O 22A method for preparing a thermal barrier coating material comprises the following steps:

[0075] Step 1: wet-milling Nb2O5, HfO2 and Ta2O5 at a raw material molar ratio of 1:6:1 at 350 r / min for 4 hours to obtain a mixed slurry; the particle sizes of Nb2O5, HfO2 and Ta2O5 are all 1-3 μm, and the purity is 99%;

[0076] Step 2: evaporate the mixed slurry obtained in step 1 to dryness at 1300 r / min and 210° C., and then grind to obtain a mixed powder with uniform particle size greater than 100 mesh;

[0077] Step 3: The mixed powder obtained in step 2 is calcined in an oxygen atmosphere at 1200°C for 8 hours, and then cooled to room temperature to obtain Nb2Hf6Ta2O in powder form. 22 Thermal barrier coating materials;

[0078] Step 4: Add 1% polyvinyl pyrrolidone solution into the powdered Nb2Hf6Ta2O 22 The thermal barrier coating material is granulated and sieved to obtain agglomerated powder with a sieve mesh of 100-200 mesh, and the mass of the adhesive added accounts for 100% of the Nb2Hf6Ta2O powder in step 3. 22 0.2% of the mass of thermal barrier coating materials;

[0079] Step 5: The agglomerated powder obtained in step 4 is pre-pressed at 150 MPa to obtain a green blank, and then the green blank is cold isostatically pressed at 180 MPa for 25 min to obtain Nb2Hf6Ta2O 22 Ceramic body;

[0080] Step 6: Nb2Hf6Ta2O obtained in step 5 22 The ceramic body was placed in an air atmosphere at 500 ° C for 6 h to remove binder, then calcined at 1600 ° C for 7 h, and cooled to room temperature to obtain Nb2Hf6Ta2O in bulk. 22 Thermal barrier coating materials.

[0081] The bulk Nb2Hf6Ta2O 22 The fracture toughness of the thermal barrier coating material is 2.41±0.38Mpa·m 1 / 2 .

[0082] Example 5

[0083] A Ti2Hf6Ta2O 21 A thermal barrier coating material, wherein the raw materials of the thermal barrier coating material include TiO2, HfO2 and Ta2O5, wherein the molar ratio of TiO2, HfO2 and Ta2O5 is 2:6:1.

[0084] A Ti2Hf6Ta2O 21 A method for preparing a thermal barrier coating material comprises the following steps:

[0085] Step 1: wet-mill TiO2, HfO2 and Ta2O5 at a raw material molar ratio of 2:6:1 at 320 r / min for 8 hours to obtain a mixed slurry; the particle sizes of the TiO2, HfO2 and Ta2O5 are all 1-3 μm, and the purity is 99%;

[0086] Step 2: The mixed slurry obtained in step 1 is evaporated to dryness at 1500 r / min and 220° C., and then ground to obtain a mixed powder with uniform particle size greater than 100 mesh;

[0087] Step 3: The mixed powder obtained in step 2 was calcined in an air atmosphere at 1200°C for 7 hours, and then cooled to room temperature to obtain powdered Ti2Hf6Ta2O 21 Thermal barrier coating materials;

[0088] Step 4: Add 2% polyvinyl alcohol solution into the powdered Ti2Hf6Ta2O 21 The thermal barrier coating material is granulated and sieved to obtain agglomerated powder with a sieve mesh of 100-200 mesh, and the mass of the adhesive added accounts for 100% of the powdered Ti2Hf6Ta2O 21 0.4% of the mass of thermal barrier coating materials;

[0089] Step 5: The agglomerated powder obtained in step 4 is pre-pressed at 100 MPa to obtain a green blank, and then the green blank is cold isostatically pressed at 150 MPa for 30 min to obtain Ti2Hf6Ta2O 21 Ceramic body;

[0090] Step 6: Ti2Hf6Ta2O obtained in step 5 21 The ceramic body was placed in an air atmosphere at 500 °C for 6 h to remove binder, then calcined at 1800 °C for 8 h, and cooled to room temperature to obtain a Ti2Hf6Ta2O 21 Thermal barrier coating materials.

[0091] The bulk Ti2Hf6Ta2O 21 The fracture toughness of the thermal barrier coating material is 2.44±0.33Mpa·m 1 / 2 .

[0092] Comparative Example 1

[0093] A kind of Hf6Ta2O 17 A method for preparing a thermal barrier coating material comprises the following steps:

[0094] Step 1: wet-mill the raw materials HfO2 and Ta2O5 at a molar ratio of 6:1 at 320 r / min for 7 hours to obtain a mixed slurry; the particle sizes of the HfO2 and Ta2O5 are both 1-3 μm, and the purity is both 99%;

[0095] Step 2: The mixed slurry obtained in step 1 is evaporated to dryness at 1200 r / min and 200° C., and then ground to obtain a mixed powder with a uniform particle size greater than 100 mesh;

[0096] Step 3: The mixed powder obtained in step 2 was calcined in an air atmosphere at 1200°C for 6 hours, and then cooled to room temperature to obtain powdered Hf6Ta2O 17 Thermal barrier coating materials;

[0097] Step 4: Add 1% polyvinyl alcohol solution into the powdered Hf6Ta2O 17 The thermal barrier coating material is granulated and sieved to obtain agglomerated powder with a sieve mesh of 100-200 mesh, and the mass of the adhesive added accounts for 100% of the Hf6Ta2O powder in step 3. 17 0.2% of the mass of thermal barrier coating materials;

[0098] Step 5: The agglomerated powder obtained in step 4 is pre-pressed at 120 MPa to obtain a green blank, and then the green blank is cold isostatically pressed at 200 MPa for 15 min to obtain Hf6Ta2O 17 Ceramic body;

[0099] Step 6: Hf6Ta2O obtained in step 5 17 The ceramic body was placed in an air atmosphere at 600 °C for 4 h to remove binder, then calcined at 1700 °C for 6 h and cooled to room temperature to obtain a bulk Hf6Ta2O 17 Thermal barrier coating materials.

[0100] The bulk Hf6Ta2O 17 The fracture toughness of the thermal barrier coating material is 1.78±0.05Mpa·m 1 / 2 .

[0101] See also Figure 1 From the XRD diagram, it can be seen that the bulk Me x Hf6Ta2O 17+y Thermal barrier coating materials only have quaternary oxide Me x Hf6Ta2O 17+y Pure phase, no impurity peaks representing Me oxides were observed, which indicates that all the thermal barrier coating material powders formed a solid solution and all Me ions had formed Me through solid phase reaction.x Hf6Ta2O 17+y ;Me x Hf6Ta2O 17+y The characteristic peaks of thermal barrier coating materials are compared with pure phase Hf6Ta2O 17 There is a slight shift, which is due to the Me atoms doping into Hf6Ta2O 17 The lattice distortion and the change of unit cell parameters make Me x Hf6Ta2O 17+y Thermal barrier coating materials have better fracture toughness.

[0102] See also Figure 2 From the SEM image, it can be seen that the Zr3Hf6Ta2O 23 The surface of the thermal barrier coating material is dense and non-porous, and has a large number of long strip-shaped grain structures. This type of structure can be pulled out when the crack propagates, consuming the strain energy during crack propagation, thereby hindering the further expansion of the crack, making the block Zr3Hf6Ta2O 23 The fracture toughness of the thermal barrier coating material is improved; the bulk Me prepared in Example 2-Example 5 x Hf6Ta2O 17+y The morphology and structure of the thermal barrier coating material are similar to those in Example 1.

[0103] See also Figure 3 From the TEM image, it can be seen that the bulk Zr3Hf6Ta2O prepared in Example 1 of the present invention 23 The thermal barrier coating material contains the elements Hf, Zr, Ta and O, and each element is evenly distributed without element segregation and agglomeration, thereby reducing local defects and stress concentration, and the fracture toughness of the material surface is consistent.

Claims

1. A high fracture toughness long period quaternary oxide thermal barrier coating material, characterized by: The thermal barrier coating material is a quaternary single-phase solid solution oxide with a long period structure, and the chemical formula of the oxide is Me x Hf6Ta2O 17+y , wherein the doping element Me is one of Zr, Gd, Y, Nb, and Ti. When Me is Zr, x=3, y=6; when Me is Y, x=4, y=6; when Me is Gd, x=2, y=3; when Me is Nb, x=2, y=5; when Me is Ti, x=2, y=4.

2. The high fracture toughness long period quaternary oxide thermal barrier coating material according to claim 1, characterized in that: The raw materials of the thermal barrier coating material include Me x O y , HfO2 and Ta2O5, among which Me x O y The molar ratio of HfO2 and Ta2O5 is (1-3):6:1; the Me x O y , HfO2 and Ta2O5 have a particle size of 1-3 μm.

3. A method for preparing a high fracture toughness long period quaternary oxide thermal barrier coating material as claimed in claim 1 or 2, characterized in that: The steps include: Step 1: Mix the raw materials x O y , HfO2 and Ta2O5 were wet-milled to obtain a mixed slurry; in terms of molar ratio, Me x O y :HfO2:Ta2O5=(1-3):6:1; Step 2: heating and evaporating the mixed slurry obtained in step 1, and then grinding to obtain a mixed powder with a particle size greater than 100 mesh; Step 3: calcine the mixed powder obtained in step 2 in air or oxygen atmosphere at 1100-1300°C for 6-9h to obtain powdered Me x Hf6Ta2O 17+y Thermal barrier coating material, that is, high fracture toughness long period quaternary oxide thermal barrier coating material in powder form.

4. The method for preparing a high fracture toughness long period quaternary oxide thermal barrier coating material according to claim 3, characterized in that: In step 1, Me x O y The powder purity of HfO2 and Ta2O5 is ≥99%.

5. The method for preparing a high fracture toughness long period quaternary oxide thermal barrier coating material according to claim 3, characterized in that: In step 1, the ball milling time is 4-8 hours, zirconium oxide balls are used as ball milling media, anhydrous ethanol is used as liquid medium, the ball-to-material ratio is 3:1, and the rotation speed is 300-350 r / min.

6. The method for preparing a high fracture toughness long period quaternary oxide thermal barrier coating material according to claim 3, characterized in that: In the step 2, a magnetic stirrer is used for heating and evaporation, the stirring speed is 1000-1500 r / min, and the heating temperature is 180-220°C.

7. The method for preparing a high fracture toughness long period quaternary oxide thermal barrier coating material according to claim 3, characterized in that: Also includes: Step 4: Add the adhesive to the powdered Me in step 3 x Hf6Ta2O 17+y The thermal barrier coating material is granulated and then sieved to obtain agglomerated powder with a sieve mesh number of 100-200 meshes; Step 5: Pre-press the agglomerated powder obtained in step 4 to obtain a green blank; then perform cold isostatic pressing on the green blank to obtain Me x Hf6Ta2O 17+y Ceramic body; Step 6: Take the Me obtained in step 5 x Hf6Ta2O 17+y The ceramic body is debonded, then calcined at 1500-1800℃ for 6-9h, and cooled to room temperature to obtain a block of Me x Hf6Ta2O 17+y Thermal barrier coating material, that is, a block-like high fracture toughness long-period quaternary oxide thermal barrier coating material.

8. The method for preparing a high fracture toughness long period quaternary oxide thermal barrier coating material according to claim 7, characterized in that: The adhesive in step 4 is a polyvinyl alcohol solution or a polyvinyl pyrrolidone solution, the mass fraction of the adhesive is 1-3%, and the mass of the adhesive added accounts for 1% of the powder Me in step 3. x Hf6Ta2O 17+y 0.2-0.6% of the mass of thermal barrier coating material.

9. The method for preparing a high fracture toughness long period quaternary oxide thermal barrier coating material according to claim 7, characterized in that: The pre-pressing pressure in step 5 is 100-150 MPa; the cold isostatic pressing pressure is 150-280 MPa, and the holding time is 10-30 min.

10. The method for preparing a high fracture toughness long period quaternary oxide thermal barrier coating material according to claim 7, characterized in that: The debinding operation in step 6 is specifically as follows: x Hf6Ta2O 17+y The ceramic body is placed in air or oxygen atmosphere at 400-600° C. for 4-6 hours.

Citation Information

Patent Citations

  • A type A2B2O7 rare earth tantalate ceramic and its preparation method

    CN111925211B

  • TiSi2 doped Gd2Zr2O7 ceramic material, preparation method and thermal barrier coating

    CN114368969A

  • Preparation methods of suspension and coating and thermal barrier coating

    CN112695266A

  • Tetragonal-phase high-entropy thermal barrier coating material and preparation method thereof

    CN113816751A

  • RE-Zr (Hf) co-doped gadolinium zirconate material, preparation method and thermal barrier coating

    CN115010506A