CaO-ZrO2 porous ceramic filter as well as preparation method and application thereof
By preparing a CaO-ZrO2 porous ceramic filter with composite pore rib structure, the problems of complex process, low strength and low filtration efficiency of the ceramic filter are solved, and the efficient purification effect of high-temperature molten metal filtration is achieved.
Patent Information
- Application Number
- CN202411026877.8
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-07-29
- Publication Date
- 2024-11-15
- Estimated Expiration
- 2044-07-29
AI Technical Summary
The existing ceramic filters are difficult to meet the needs of high-temperature molten metal filtration at the same time due to complex processes, low strength and low filtration efficiency.
Using the preparation method of CaO-ZrO2 porous ceramic filter, the powder is mixed with polycarboxylate, carboxymethylcellulose and binding agent and then ball milled, impregnated the mesh porous template, sprayed the slurry and sintered to form composite pores CaO-ZrO2 porous ceramic filter with rib structure.
It realizes a CaO-ZrO2 porous ceramic filter with simple process, low cost, high room temperature and high temperature strength, excellent thermal shock resistance and high filtration efficiency, and is suitable for molten metal filtration environments of 1600-1800℃.
Smart Images

Figure CN118955155A_ABST
Abstract
Description
Technical Field
[0001] The invention relates to the technical field of liquid metal purification, and in particular to a CaO-ZrO2 porous ceramic filter and a preparation method and application thereof. Background Art
[0002] The filtration of non-metallic inclusions in molten metal plays an important role in improving the quality and performance of castings. At present, most filters used for molten metal filtration are high-temperature resistant porous ceramic filters, which can effectively intercept non-metallic inclusions in molten metal through mechanical interception and deep adsorption mechanisms, and transform the molten metal from turbulent flow to laminar flow by rectifying the slag, preventing secondary optimization, and playing a role in purification and homogenization. Ceramic filters are widely used in the production process of automotive parts, diesel engine parts, compressors, wind power castings, and large castings in the metallurgical process, which has greatly improved the quality and competitiveness of my country's castings, while increasing the profits of foundry companies, which is of great significance to my country's improvement of energy utilization and reduction of carbon emissions.
[0003] Ceramic filters can be divided into foam ceramic filters and straight-hole ceramic filters according to their structure; they are mainly divided into zirconia, alumina, silicon carbide, magnesium oxide, etc. according to their materials; they can be divided into direct filters and reactive filters according to the filtering method. Zirconia ceramic filters have become the preferred filters for special steels, high value-added steels or alloy castings due to their excellent high temperature resistance, corrosion resistance, high strength, and good thermal shock resistance; calcium oxide filters are often used as reactive filters due to their excellent thermodynamic stability, desulfurization and dephosphorization performance, and carbon adsorption performance, but calcium oxide is very easy to hydrate due to its own particles, which makes its storage and preparation extremely difficult. The current zirconia or calcium oxide porous ceramic filters are difficult to simultaneously meet the characteristics of simple process and excellent performance.
[0004] At present, technicians have conducted in-depth research and technical development to solve the comprehensive performance problem of ceramic filters. For example, the Chinese patent with application number CN201210115537.3 discloses a special zirconia foam ceramic filter with high high temperature strength and good thermal shock resistance and its preparation method. A large amount of nano zirconium oxide and a small amount of nano metal zirconium and trace amounts of calcium oxide, magnesium oxide, and aluminum oxide are added to the zirconia, and the slurry is hung after ball milling and sintered at high temperature in a nitriding furnace to obtain a high-strength zirconia porous ceramic filter with good thermal shock resistance. Adding nano zirconium oxide can promote sintering and improve thermal shock stability. Nano metal zirconium generates ZrN in a nitrogen atmosphere, and utilizes the good shaping and toughness characteristics of metal materials to wet and wrap with each other between ceramics, penetrate into the gaps between ceramic phases, form a continuous membrane structure, strengthen toughness, and improve thermal shock resistance. However, this technology needs to be sintered under a controlled nitrogen atmosphere at a high temperature of 1850°C, which not only consumes a lot of energy, but also has a relatively complicated process, which greatly increases the preparation cost of zirconia porous ceramics; it is not suitable as an industrial production method for zirconia porous ceramic filters. Another example is the Chinese patent application number CN201911404444.0, which discloses a method for preparing a zirconia-based foam ceramic filter, characterized in that magnesium oxide and cerium oxide are added during the electro-melting zirconia process, and the cooling process is controlled to eliminate the volume effect of the zirconia material, slowly grow the grains, and then improve and stabilize the mechanical strength and high-temperature mechanical properties; then the electro-melted zirconia is mixed with a trace amount of tungsten carbide for sintering to improve its high-temperature erosion and corrosion resistance. Although this technical method can effectively improve the mechanical strength and high-temperature erosion and corrosion resistance of the zirconia ceramic filter, the preparation process is complicated, and it is necessary to use an arc furnace to melt zirconia and an argon furnace to provide an argon atmosphere for sintering, which consumes a lot of energy and cannot meet the important indicators of energy conservation and emission reduction in the metallurgical industry. For example, the Chinese patent application application number CN201710034200.2 discloses a calcium oxide filter and a method for preparing it, characterized in that a small amount of zirconium oxide is added to calcium oxide to increase toughness, and anhydrous resin or paraffin is used to wrap the surface of the calcium oxide particles to form a protective film, which is then pressed and sintered. This technology has the characteristics of high operating temperature, stable high temperature performance, and good anti-hydration performance, but the prepared filter has low porosity, poor strength and low filtration efficiency.
[0005] Therefore, how to provide a CaO-ZrO2 porous ceramic filter with excellent comprehensive performance that can be used for high-temperature molten metal filtration has become an urgent problem that needs to be solved by technical personnel in this field. Summary of the invention
[0006] In view of this, the present invention provides a CaO-ZrO2 porous ceramic filter and its preparation method and application, which aims to solve the technical problems of the existing ceramic filtration, such as complex process, low strength and low filtration efficiency.
[0007] In order to achieve the above-mentioned object of the invention, the present invention provides the following technical solutions:
[0008] The present invention provides a method for preparing a CaO-ZrO2 porous ceramic filter, comprising the following steps:
[0009] S1. Powder A, polycarboxylate, carboxymethyl cellulose, binder A and water are mixed and ball-milled to obtain slurry A;
[0010] Powder B, polycarboxylate, binder B and water are mixed and ball-milled to obtain slurry B;
[0011] S2, immersing the mesh porous template in slurry A, and sequentially performing slurry spinning, primary drying, and secondary drying to obtain a zirconia porous ceramic preform;
[0012] S3, spraying slurry B on the zirconia porous ceramic preform, and obtaining a CaO-ZrO2 porous ceramic body after drying;
[0013] S4. Sintering the CaO-ZrO2 porous ceramic body to obtain a CaO-ZrO2 porous ceramic filter.
[0014] Furthermore, in step S1, the powder A comprises zirconium oxide of three particle sizes, namely fine, medium and coarse, in a mass ratio of 10-20:20-30:50-70; the fine particle size D 50 The particle size is 0.5~1μm, and the medium particle size D 50 The coarse particle size D is 3 to 8 μm. 50 The thickness is 30 to 50 μm; the zirconium oxide includes one or more of yttrium-stabilized zirconium oxide, magnesium-stabilized zirconium oxide and cerium-stabilized zirconium oxide.
[0015] Furthermore, in the step S1, in the preparation of slurry A, the amount of polycarboxylate is 0.5-1.5wt% of powder A, the amount of carboxymethyl cellulose is 0.2-0.8wt% of powder A, the amount of binder A is 10-20wt% of powder A, and the amount of water is 25-35wt% of powder A; binder A includes zirconium sol; and the ball milling time is 1-4h.
[0016] Furthermore, in the step S1, in the preparation of slurry B, the amount of polycarboxylate is 0.5-1.5wt% of powder B, the amount of binder B is 2-5wt% of powder B, and the amount of water is 23-46wt% of powder A; powder B includes calcium carbonate and nano-particle zirconium oxide, and the mass ratio of calcium carbonate to nano-particle zirconium oxide is 80-95:5-20; the nano-particle zirconium oxide D 50 is 40-60nm; binder B includes starch and dextrin; and the ball milling time is 4-8h.
[0017] Furthermore, in step S2, the material of the mesh porous template includes polyurethane, 3D printing resin or nylon; the structure of the mesh porous template is 3 layers of gradient holes, and the pore diameters are divided into large, medium and small from the outside to the inside, the large pore diameter is 2 to 3 mm, the medium pore diameter is 1.2 to 1.5 mm, and the small pore diameter is 0.5 to 1 mm; the immersion time is 20 to 60 minutes.
[0018] Furthermore, in step S2, the primary drying temperature is 20-30° C., and the primary drying time is 12-18 h; the secondary drying temperature is 80-110° C., and the secondary drying time is 24-48 h.
[0019] Furthermore, in step S3, the amount of slurry B sprayed is 8 to 12 g / m 2 The spraying rate is 0.5 to 3.5 m / min; the drying temperature is 80 to 110° C., and the drying time is 12 to 24 hours.
[0020] Furthermore, in step S4, the sintering temperature is 1200-1500° C., the sintering time is 1-5 hours, and the heating rate from room temperature to the sintering temperature is 2-5° C. / min.
[0021] The invention provides a CaO-ZrO2 porous ceramic filter prepared by the preparation method.
[0022] The present invention also provides the use of the CaO-ZrO2 porous ceramic filter in high-temperature molten metal filtration.
[0023] It can be seen from the above technical solution that compared with the prior art, the beneficial effects of the present invention are as follows:
[0024] The present invention provides a CaO-ZrO2 porous ceramic filter and a preparation method and application thereof, comprising the following steps: dipping a mesh porous template in slurry A and drying the slurry to obtain a preform; spraying slurry B on the preform to obtain an embryo, and calcining the embryo to obtain the CaO-ZrO2 porous ceramic filter.
[0025] The invention has the characteristics of simple process and low cost. The manufactured product has high strength at room temperature, high strength at high temperature, excellent thermal shock resistance, good filtration efficiency and high filtration precision, and can be suitable for molten metal filtration environment of 1600-1800°C.
[0026] The CaO-ZrO2 porous ceramics prepared by the present invention have good room temperature strength and high temperature strength. First, the present invention uses reasonable particle grading to make small particles and medium particles fill the gaps between large particles, and release free water between the particle gaps, so as to configure the slurry closest to the bulk density, thereby reducing the slurry viscosity, improving rheology, and increasing the solid content. Good fluidity enables the slurry to be evenly attached to the mesh porous template to reduce defect formation, and the high solid content slurry can increase the density of the green body, thereby achieving the effect of improving the strength of the CaO-ZrO2 porous ceramics. Second, the raw materials used in the present invention are yttrium / magnesium / cerium stabilized zirconium oxide fine powder and calcium carbonate, without adding sintering aids, and after high temperature sintering, a CaO-ZrO2 porous ceramic with a zirconium oxide phase as a matrix and a calcium zirconate-calcium oxide phase as a coating is formed. The formation of calcium zirconate can not only connect and cover the calcium oxide formed by the decomposition of calcium carbonate to increase the density and strength of the green body, but also fill part of the micropores to slow down the hydration rate. Third, the nano-zirconia in slurry B can be mixed with calcium carbonate more evenly, and the mixed slurry can be adhered to the surface of the pores and ribs through air spraying, filling and repairing the defects of the zirconia preform; during high-temperature sintering, the fine zirconia particles are more active and easier to fill the holes formed by the high-temperature decomposition of calcium carbonate particles, and form calcium zirconate in situ to make the sintering neck between CaO particles wider and thicker, and the connection is tighter. Therefore, the prepared CaO-ZrO2 porous ceramics have good room temperature strength and high temperature strength.
[0027] The CaO-ZrO2 porous ceramics prepared by the present invention have good thermal shock resistance. First, when the CaO-ZrO2 porous ceramics are sintered and cooled, residual compressive stress can be formed on the surface of the calcium zirconate-calcium oxide coating in the composite structure pores and ribs because the linear expansion coefficient of the calcium zirconate-calcium oxide coating is lower than that of the zirconium oxide skeleton layer. The residual compressive stress formed in the calcium zirconate-calcium oxide coating can effectively inhibit the initiation and expansion of cracks caused by thermal stress, thereby greatly improving the thermal shock resistance of the CaO-ZrO2 porous ceramics. Second, calcium carbonate and dextrin decompose at high temperatures to form calcium oxide and a large number of micropores, so that the material can passivate the crack tip during the thermal shock process and hinder the further expansion of thermal stress cracks. Third, nano-zirconium oxide can uniformly fill CaO grains, increase the volume density of the material, and form calcium zirconate in situ around calcium oxide, thicken and enlarge the sintering neck between calcium oxide particles, increase the strength of the material, and improve the thermal shock resistance. Therefore, the prepared CaO-ZrO2 porous ceramics have good thermal shock resistance.
[0028] The CaO-ZrO2 porous ceramic prepared by the present invention has good filtration efficiency and filtration accuracy. First, for non-metallic inclusions in molten metal, the calcium zirconate-calcium oxide coating has a very strong adsorption capacity for them, can react with neutral and acidic oxides in the molten metal to form a dense and continuous calcium aluminate interface layer, can achieve the adsorption of active elements such as sulfur, phosphorus, aluminum, titanium in the molten metal and fine-tune the components in the alloy, and can also prevent the molten metal from penetrating the pores and cracks of the material and causing structural peeling. Second, in the formation process of the calcium zirconate-calcium oxide coating, there is decomposition of calcium carbonate, burnout of dextrin, and reaction sintering of calcium oxide and nano zirconium oxide, thereby forming a large number of micropores on the surface of the coating. These micropores not only improve the surface roughness of the CaO-ZrO2 porous ceramic, increase the contact area with the molten metal, reduce wettability, increase the contact angle with the molten metal, but also improve the material reaction activity, promote the reaction with inclusions, increase the attachment points for inclusion adsorption and deposition, and make fine inclusions more easily adsorbed by the filter. Fourth, the mesh porous template used in the present invention has a three-layer gradient pore structure. Compared with the traditional disordered porous ceramic filter, the three-layer gradient pore is not easy to be blocked when filtering the molten metal, and has better filtration efficiency; compared with the traditional uniform pore ceramic filter, the three-layer gradient pore can filter more fine inclusions and has higher filtration accuracy. Therefore, the prepared CaO-ZrO2 porous ceramic has good filtration efficiency and filtration accuracy.
[0029] The CaO-ZrO2 porous ceramics prepared by the present invention have lower cost and simple process. The method used for preparing the CaO-ZrO2 porous ceramics by the present invention is a template replication method, which is to prepare the CaO-ZrO2 porous ceramics by slurry coating and template burning on the surface of a 3D printed paraffin, resin or organic polymer template. Compared with the self-foaming and injection molding processes, the template replication method involved in the present invention is simpler, lower cost, and more efficient, and can achieve large-scale industrial production.
[0030] In summary, the present invention adopts the coating of zirconium oxide slurry, spraying of composite slurry and high-temperature in-situ sintering technology. On the basis of pre-sintering of zirconium oxide foam ceramics, a mixed slurry of fine zirconium oxide powder and calcium carbonate is adhered to the surface of the pore ribs by air spraying, the defects of the zirconium oxide pore ribs are filled and repaired, and finally a CaO-ZrO2 porous ceramic filter with composite pore ribs (calcium zirconate-calcium oxide coating, zirconium oxide matrix) is formed by high-temperature sintering. The formation of composite structure pore ribs can significantly improve the normal temperature / high temperature strength, thermal shock resistance and adsorption efficiency of non-metallic inclusions in molten metal of the prepared CaO-ZrO2 porous ceramic filter.
[0031] After testing, the high temperature resistance value of the CaO-ZrO2 porous ceramic filter prepared by the present invention reaches above 1800°C; the compressive strength at room temperature is between 3.2 and 4.2MPa; the high temperature (1400°C) strength is between 3.0 and 4.0MPa; the number of 1100°C oil cooling cycles is 5 to 10 times; the prepared CaO-ZrO2 porous ceramics used for molten metal filtration can increase the casting yield by up to 15%. BRIEF DESCRIPTION OF THE DRAWINGS
[0032] Figure 1 The SEM image of the pore-rib fracture of the CaO-ZrO2 porous ceramic filter prepared in Example 1;
[0033] Figure 2 This is a SEM image of the coating surface of the CaO-ZrO2 porous ceramic filter prepared in Example 1. DETAILED DESCRIPTION
[0034] The present invention provides a method for preparing a CaO-ZrO2 porous ceramic filter, comprising the following steps:
[0035] S1. Powder A, polycarboxylate, carboxymethyl cellulose, binder A and water are mixed and ball-milled to obtain slurry A;
[0036] Powder B, polycarboxylate, binder B and water are mixed and ball-milled to obtain slurry B;
[0037] S2, immersing the mesh porous template in slurry A, and sequentially performing slurry spinning, primary drying, and secondary drying to obtain a zirconia porous ceramic preform;
[0038] S3, spraying slurry B on the zirconia porous ceramic preform, and obtaining a CaO-ZrO2 porous ceramic body after drying;
[0039] S4. Sintering the CaO-ZrO2 porous ceramic body to obtain a CaO-ZrO2 porous ceramic filter.
[0040] In the present invention, in step S1, the powder A comprises three types of zirconium oxide with a mass ratio of 10-20:20-30:50-70, namely fine, medium and coarse particle sizes, and the mass ratio is preferably 13:23:64; the fine particle size D 50 The median particle size D 50 3 to 8 μm, preferably 4 to 7 μm, more preferably 5 to 6 μm; the coarse particle size D 50 The thickness is 30 to 50 μm, preferably 35 to 45 μm, and more preferably 40 μm; the zirconium oxide includes one or more of yttrium-stabilized zirconia, magnesium-stabilized zirconia and cerium-stabilized zirconia.
[0041] In the present invention, in step S1, the Y2O3 content in the yttrium-stabilized zirconia is preferably 4-10%, the CeO2 content in the cerium-stabilized zirconia is preferably 5-15%, and the MgO content in the magnesium-stabilized zirconia is preferably 5-10%.
[0042] In the present invention, in the step S1, in the preparation of slurry A, the amount of polycarboxylate is 0.5-1.5wt% of powder A, preferably 0.8-1.2wt%, and more preferably 1.0wt%; the amount of carboxymethyl cellulose is 0.2-0.8wt% of powder A, preferably 0.4-0.6wt%, and more preferably 0.5wt%; the amount of binder A is 10-20wt% of powder A, preferably 12-18wt%; more preferably 14-16wt%; the amount of water is 25-35wt% of powder A, preferably 27-32wt%, and more preferably 30wt%; the binder A includes zirconium sol; the ball milling time is 1-4h, preferably 2-3h.
[0043] In the present invention, in the step S1, in the preparation of slurry B, the amount of polycarboxylate is 0.5-1.5wt% of powder B, preferably 0.8-1.2wt%, and more preferably 1.0wt%; the amount of binder B is 2-5wt% of powder B, preferably 3-4wt%; the amount of water is 23-46wt% of powder A, preferably 25-40wt%, and more preferably 30-35wt%; powder B includes calcium carbonate and nano-particle zirconium oxide, the mass ratio of calcium carbonate to nano-particle zirconium oxide is 80-95:5-20, preferably 83-92:8-17, and more preferably 85-90:10-15; the average particle size of calcium carbonate is preferably ≤5μm, and the purity of calcium carbonate is ≥98.5%; the D of the nano-particle zirconium oxide 50 40 to 60 nm, preferably D 50 =50nm; binder B includes starch and dextrin; the ball milling time is 4 to 8h, preferably 5 to 7h, and more preferably 6h.
[0044] In the present invention, in the step S2, the material of the mesh porous template includes polyurethane, 3D printing resin or nylon; the structure of the mesh porous template is 3 layers of gradient holes, and the pore diameters are divided into large, medium and small from the outside to the inside, the large pore diameter is 2 to 3 mm, the medium pore diameter is 1.2 to 1.5 mm, and the small pore diameter is 0.5 to 1 mm; the polyurethane template is preferably a three-layer hole of 10PPI-20PPI-30PPI, and the 3D printing resin template is preferably a three-layer hole of 2.5mm-1.3mm-0.8mm; the immersion time is 20 to 60 min, preferably 30 to 50 min, and more preferably 40 min.
[0045] In the present invention, in step S2, the primary drying temperature is 20-30°C, preferably 22-28°C, and more preferably 24-26°C; the primary drying time is 12-18h, preferably 14-16h; the secondary drying temperature is 80-110°C, preferably 90-100°C; the secondary drying time is 24-48h, preferably 30-40h, and more preferably 35h.
[0046] In the present invention, in step S2, the slurrying is preferably performed by extrusion or centrifugation.
[0047] In the present invention, in step S3, the amount of slurry B sprayed is 8 to 12 g / m 2 , preferably 10g / m 2 The spraying rate is 0.5 to 3.5 m / min, preferably 1 to 3 m / min, and more preferably 2 m / min; the drying temperature is 80 to 110°C, preferably 90 to 100°C; the drying time is 12 to 24 hours, preferably 15 to 20 hours.
[0048] In the present invention, in step S4, the sintering temperature is 1200-1500°C, preferably 1400°C; the sintering time is 1-5h, preferably 2-4h, and more preferably 3h; the heating rate from room temperature to the sintering temperature is 2-5°C / min, preferably 3-4°C / min.
[0049] The invention provides a CaO-ZrO2 porous ceramic filter prepared by the preparation method.
[0050] The present invention also provides the use of the CaO-ZrO2 porous ceramic filter in high-temperature molten metal filtration.
[0051] The technical solutions provided by the present invention are described in detail below in conjunction with the embodiments, but they should not be construed as limiting the protection scope of the present invention.
[0052] Example 1
[0053] Zirconium oxide of three particle sizes, namely fine (D50=0.8μm), medium (D50=5μm) and coarse (D50=40μm), (the amounts of yttrium-stabilized zirconia, magnesium-stabilized zirconia and cerium-stabilized zirconia are the same) are graded to obtain powder A; 1wt% of polycarboxylate, 0.4wt% of carboxymethyl cellulose, 15wt% of zirconium sol and 30wt% of water are added to powder A and ball-milled for 4h to obtain slurry A; 80wt% of calcium carbonate powder and 20wt% of nano-particle size (D50=50nm) zirconium oxide powder are mixed to obtain powder B, and 1wt% of polycarboxylate, 4wt% of dextrin and 30wt% of water are added to powder B and ball-milled for 4h to obtain slurry B.
[0054] The mesh porous template was immersed in the slurry A for 20 minutes, the slurry was centrifuged, and the slurry was dried at 25° C. for 18 hours, and then dried at 110° C. for 48 hours to obtain a zirconia porous ceramic preform.
[0055] The slurry B was sprayed on the zirconia porous ceramic preform, and the amount of the sprayed slurry was 10 g / m 2 The spraying rate was 3 m / min, and then it was dried at 110 °C for 24 h to obtain a CaO-ZrO2 porous ceramic body.
[0056] The CaO-ZrO2 porous ceramic body is placed in a high-temperature furnace, heated to 1400°C at a rate of 5°C / min in an air atmosphere, kept at this temperature for 2 hours, and cooled to room temperature along with the furnace to obtain a CaO-ZrO2 porous ceramic filter.
[0057] The volume density of the CaO-ZrO2 porous ceramic filter prepared in this example is 1.2 g / cm 3 ; Porosity is 87%; Room temperature compressive strength is 4.2MPa; High temperature (1400℃) strength is 4.0MPa; High temperature resistance value is >1800℃; The residual strength retention rate after three times of 1100℃ oil cooling is 50%.
[0058] Example 2
[0059] Zirconium oxide of three particle sizes, namely fine (D50=0.8μm), medium (D50=5μm) and coarse (D50=40μm), (the amounts of yttrium-stabilized zirconia, magnesium-stabilized zirconia and cerium-stabilized zirconia are the same) are graded to obtain powder A; 1.5wt% of polycarboxylate, 0.8wt% of carboxymethyl cellulose, 15wt% of zirconium sol and 35wt% of water are added to powder A and ball-milled for 4h to obtain slurry A; 80wt% of calcium carbonate powder and 20wt% of nano-particle size (D50=50nm) zirconium oxide powder are mixed to obtain powder B, and 1.5wt% of polycarboxylate, 5wt% of dextrin and 46wt% of water are added to powder B and ball-milled for 4h to obtain slurry B.
[0060] The mesh porous template was immersed in the slurry A for 20 minutes, the slurry was centrifuged, dried at 25° C. for 18 hours, and then dried at 110° C. for 48 hours to obtain a zirconia porous ceramic preform.
[0061] The slurry B was sprayed on the zirconia porous ceramic preform, and the amount of the sprayed slurry was 10 g / m 2 The spraying rate was 3 m / min, and then it was dried at 110 °C for 24 h to obtain a CaO-ZrO2 porous ceramic body.
[0062] The CaO-ZrO2 porous ceramic body is placed in a high-temperature furnace, heated to 1500°C at a rate of 5°C / min in an air atmosphere, kept at this temperature for 2 hours, and cooled to room temperature along with the furnace to obtain a CaO-ZrO2 porous ceramic filter.
[0063] The volume density of the CaO-ZrO2 porous ceramic filter prepared in this example is 1.3 g / cm 3 ; Porosity is 83%; Room temperature compressive strength is 3.2MPa; High temperature (1400℃) strength is 3.0MPa; High temperature resistance value is >1800℃; The residual strength retention rate after three times of 1100℃ oil cooling is 30%.
[0064] Example 3
[0065] Zirconium oxide of three particle sizes, namely fine (D50=0.8μm), medium (D50=5μm) and coarse (D50=40μm), (the amounts of yttrium-stabilized zirconia, magnesium-stabilized zirconia and cerium-stabilized zirconia are the same) are graded to obtain powder A; 0.5wt% of polycarboxylate, 0.2wt% of carboxymethyl cellulose, 15wt% of zirconium sol and 25wt% of water are added to powder A, and ball milling is performed for 4h to obtain slurry A; 80wt% of calcium carbonate powder and 20wt% of nano-particle size (D50=50nm) zirconium oxide powder are mixed to obtain powder B, and 0.5wt% of polycarboxylate, 2wt% of dextrin and 23wt% of water are added to powder B, and ball milling is performed for 4h to obtain slurry B.
[0066] The mesh porous template was immersed in the slurry A for 20 minutes, squeezed and slurried, dried at 25° C. for 18 hours, and then dried at 110° C. for 48 hours to obtain a zirconia porous ceramic preform.
[0067] The slurry B was sprayed on the zirconia porous ceramic preform, and the amount of the sprayed slurry was 10 g / m 2 The spraying rate was 3 m / min, and then it was dried at 110 °C for 24 h to obtain a CaO-ZrO2 porous ceramic body.
[0068] The CaO-ZrO2 porous ceramic body is placed in a high-temperature furnace, heated to 1300°C at a rate of 5°C / min in an air atmosphere, kept at this temperature for 2 hours, and cooled to room temperature along with the furnace to obtain a CaO-ZrO2 porous ceramic filter.
[0069] The volume density of the CaO-ZrO2 porous ceramic filter prepared in this example is 1.2 g / cm 3 ; Porosity is 85%; Room temperature compressive strength is 4.0MPa; High temperature (1400℃) strength is 3.8MPa; High temperature resistance value is >1800℃; The residual strength retention rate after three times of 1100℃ oil cooling is 35%.
[0070] The above test results show that the high temperature resistance value of the CaO-ZrO2 porous ceramic filter prepared by the present invention reaches above 1800°C; the compressive strength at room temperature is between 3.2 and 4.2MPa, and the high temperature (1400°C) strength is between 3.0 and 4.0MPa, which can be used in the molten metal filtration environment of 1600 to 1800°C.
[0071] The above is only a preferred embodiment of the present invention. It should be pointed out that for ordinary technicians in this technical field, several improvements and modifications can be made without departing from the principle of the present invention. These improvements and modifications should also be regarded as the scope of protection of the present invention.
Claims
1. A method for preparing a CaO-ZrO2 porous ceramic filter, characterized in that: The following steps are involved: S1. Powder A, polycarboxylate, carboxymethyl cellulose, binder A and water are mixed and ball-milled to obtain slurry A; Powder B, polycarboxylate, binder B and water are mixed and ball-milled to obtain slurry B; S2, immersing the mesh porous template in slurry A, and sequentially performing slurry spinning, primary drying, and secondary drying to obtain a zirconia porous ceramic preform; S3, spraying slurry B on the zirconia porous ceramic preform, and obtaining a CaO-ZrO2 porous ceramic body after drying; S4. Sintering the CaO-ZrO2 porous ceramic body to obtain a CaO-ZrO2 porous ceramic filter.
2. The preparation method according to claim 1, characterized in that: In step S1, the powder A comprises three types of zirconium oxide with fine, medium and coarse particle sizes in a mass ratio of 10-20:20-30:50-70; the fine particle size D 50 The particle size is 0.5~1μm, and the medium particle size D 50 The coarse particle size D is 3 to 8 μm. 50 The thickness is 30-50 μm; the zirconium oxide includes one or more of yttrium-stabilized zirconium oxide, magnesium-stabilized zirconium oxide and cerium-stabilized zirconium oxide.
3. The preparation method according to claim 2, characterized in that: In the step S1, in the preparation of slurry A, the amount of polycarboxylate is 0.5-1.5wt% of powder A, the amount of carboxymethyl cellulose is 0.2-0.8wt% of powder A, the amount of binder A is 10-20wt% of powder A, and the amount of water is 25-35wt% of powder A; binder A includes zirconium sol; and the ball milling time is 1-4h.
4. The preparation method according to any one of claims 1 to 3, characterized in that: In the step S1, in the preparation of slurry B, the amount of polycarboxylate is 0.5-1.5wt% of powder B, the amount of binder B is 2-5wt% of powder B, and the amount of water is 23-46wt% of powder A; powder B includes calcium carbonate and nano-particle zirconium oxide, and the mass ratio of calcium carbonate to nano-particle zirconium oxide is 80-95:5-20; the nano-particle zirconium oxide D 50 is 40-60nm; binder B includes starch and dextrin; and the ball milling time is 4-8h.
5. The preparation method according to claim 4, characterized in that: In the step S2, the material of the mesh porous template includes polyurethane, 3D printing resin or nylon; the structure of the mesh porous template is 3 layers of gradient holes, and the pore diameters are divided into large, medium and small from the outside to the inside, the large pore diameter is 2 to 3 mm, the medium pore diameter is 1.2 to 1.5 mm, and the small pore diameter is 0.5 to 1 mm; the immersion time is 20 to 60 minutes.
6. The preparation method according to claim 2, 3 or 5, characterized in that: In step S2, the primary drying temperature is 20-30° C., and the primary drying time is 12-18 hours; the secondary drying temperature is 80-110° C., and the secondary drying time is 24-48 hours.
7. The preparation method according to claim 6, characterized in that: In step S3, the amount of slurry B sprayed is 8-12 g / m 2 The spraying rate is 0.5 to 3.5 m / min; the drying temperature is 80 to 110° C., and the drying time is 12 to 24 hours.
8. The preparation method according to claim 2, 3, 5 or 7, characterized in that: In the step S4, the sintering temperature is 1200-1500° C., the sintering time is 1-5 hours, and the heating rate from room temperature to the sintering temperature is 2-5° C. / min.
9. A CaO-ZrO2 porous ceramic filter prepared by the preparation method according to any one of claims 1 to 8.
10. Use of the CaO-ZrO2 porous ceramic filter according to claim 9 in high-temperature molten metal filtration.
Citation Information
Patent Citations
Preparation method of steel ladle pouring material with slag resistance
CN107382333A
Aluminum oxide-based foamed ceramic and preparation method thereof
CN107840677A
Low-thermal-conductivity calcium zirconate material and preparation method thereof
CN114057504A
Ordered pore silicon carbide porous material for porous medium combustion and preparation method of ordered pore silicon carbide porous material
CN114180986A
Production of thick zirconia film
JP1996091840A
Cited By
Zirconium oxide porous ceramic for steelmaking fusion casting
CN122127150A