Preparation method of PVC composite material for yoga mat
By using silicon modified polyurethane and epoxy silane in the PVC composite material for yoga mat, phosphoric acid and silicon oxygen bonds are generated to form carbon film and glass-like substances, the problem of poor flame retardant effect in the prior art is solved. , while improving mechanical properties and achieving safer yoga mat materials.
Patent Information
- Application Number
- CN202411024060.7
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-07-29
- Publication Date
- 2024-11-15
- Estimated Expiration
- Not applicable · inactive patent
AI Technical Summary
The flame retardant effect of existing PVC composite materials for yoga mats is poor, making it difficult to effectively avoid flammable problems, and the mechanical properties have not been optimized.
After activation with allyl glycidyl ether, tetrahydrofuran solvent and chloroplatinic acid, 1,1,3,3-tetramethyldisiloxane was added dropwise, followed by sulfaguanidine and phenylphosphate dichloride to form silicon-containing amplification Chain agent and prepolymerized with hexamethylene diisocyanate, polyether polyol and dibutyltin dilaurate, followed by addition of silicon modified polyurethane and epoxy silane, and the treatment of a double rotomolding machine and a flat vulcanizer to form Yoga mats are made of PVC composite materials.
The decomposition of polyurethane and epoxy silane through silicon modification to form phosphoric acid and silicon oxygen bonds, forming carbon film and glass-like substances, achieving flame retardant effect, and enhancing mechanical properties, significantly improving the flame retardant and mechanical properties of the material.
Abstract
Description
Technical Field
[0001] The invention relates to the technical field of PVC composite materials, in particular to a method for preparing a PVC composite material for a yoga mat. Background Art
[0002] Polyvinyl chloride is a widely used synthetic plastic with excellent physical and chemical properties, and is widely used in various fields. However, polyvinyl chloride has the defect of being flammable and the flame retardant effect is not very good. Therefore, how to avoid this phenomenon is the key to solving the problem. For example, patent CN109810413B discloses a composite material for fitness yoga balls and a preparation method thereof. The surface of the fitness yoga ball is fine and evenly distributed with unevenness on the surface. Since it has strong buffering properties, when it accidentally touches a sharp object, the yoga ball is slowly deflated, and there is no safety hazard. The explosion-proof problem is solved, but its flame retardant effect is not optimized. Summary of the invention
[0003] 1. Technical issues to be resolved
[0004] In view of the deficiencies in the prior art, the present invention provides a method for preparing a PVC composite material for a yoga mat, which has good flame retardant and mechanical properties.
[0005] (II) Technical solution
[0006] To achieve the above object, the present invention provides the following technical solution: a method for preparing a PVC composite material for a yoga mat, wherein the method for preparing the PVC composite material for a yoga mat is:
[0007] (1) adding allyl glycidyl ether, tetrahydrofuran solvent and chloroplatinic acid to a reactor, activating at 40-55° C. for 35-40 min, then dropping 1,1,3,3-tetramethyldisiloxane for 50-60 min, continuing the reaction at 50-60° C. for 4-7 h, cooling to room temperature after completion, adding activated carbon adsorbent, ultrasonically shaking for 30-40 min, removing the catalyst chloroplatinic acid, filtering, and rotary evaporation to obtain intermediate 1;
[0008] (2) adding sulfaguanidine and phenylphosphonic acid dichloride to N,N-dimethylformamide solvent, stirring to dissolve, reacting at 16-24° C. for 6-8 hours, and after the reaction, removing the solvent by rotary evaporation, filtering, washing and drying to obtain intermediate 2;
[0009] (3) adding intermediate 2 to N,N-dimethylformamide solvent, heating in a water bath at 70-80° C., then adding intermediate 1 under constant pressure, continuing the reaction for 8-14 hours, distilling under reduced pressure after the reaction, washing and drying to obtain a silicon-containing chain extender;
[0010] (4) adding hexamethylene diisocyanate and polyether polyol into a reaction kettle, adding dibutyltin dilaurate as a catalyst, and performing prepolymerization under a nitrogen atmosphere at a temperature of 70-90° C. for 4-6 hours, and then adding a silicon-containing chain extender. After the reaction is completed, cooling to room temperature to obtain a silicon-modified polyurethane;
[0011] (5) adding the silicon-containing chain extender to the chloroform solvent, stirring and dispersing, continuing to add vinyl trichlorosilane, heating to 90-110° C., reacting for 9-12 hours, filtering, distilling the filtrate under reduced pressure, washing with deionized water, and drying to obtain olefinated silane;
[0012] (6) adding the olefinated silane to the N,N-dimethylformamide solvent, stirring evenly, and then adding the hydrogen peroxide aqueous solution thereto, stirring and reacting at 30-40° C. for 4-6 hours. After the reaction is completed, distilling under reduced pressure, filtering and drying to obtain epoxy silane;
[0013] (7) 15-20 parts by weight of maleic anhydride grafted polyvinyl chloride, 60-100 parts by weight of polyvinyl chloride resin, 2-4 parts by weight of calcium carbonate, 1-3 parts by weight of stearic acid, 8-14 parts by weight of silicon-modified polyurethane, and 4-7 parts by weight of epoxy silane are added to a double-roller plasticator, plasticized at 170-185° C. for 10-15 min, and then molded in a flat vulcanizer at 175-190° C. and 8-12 MPa for 5-10 min to obtain a PVC composite material for a yoga mat.
[0014] Preferably, the mass ratio of allyl glycidyl ether, chloroplatinic acid and 1,1,3,3-tetramethyldisiloxane in (1) is 1:0.02-0.04:1.2-1.3.
[0015] Preferably, the mass ratio of sulfaguanidine to phenylphosphonic acid dichloride in (2) is 1.3-1.5:1.
[0016] Preferably, the mass ratio of intermediate 2 to intermediate 1 in (3) is 1:0.8-1.3.
[0017] Preferably, the mass ratio of hexamethylene diisocyanate, polyether polyol, dibutyltin dilaurate catalyst and silicon-containing chain extender in (4) is 1.2-1.5:1:0.01-0.02:0.6-1.2.
[0018] Preferably, the mass ratio of the silicon-containing chain extender to vinyltrichlorosilane in (5) is 1.6-2.4:1.
[0019] Preferably, the mass ratio of olefinic silane to aqueous hydrogen peroxide solution in (6) is 1:3.2-3.6.
[0020] (III) Beneficial technical effects
[0021] The invention prepares the PVC composite material for yoga mat by adding maleic anhydride grafted polyvinyl chloride, polyvinyl chloride resin, calcium carbonate, stearic acid, silicon modified polyurethane and epoxy silane into a double-roll plastic mill, plasticizing, and then molding in a flat vulcanizer.
[0022] The alkenyl group in allyl glycidyl ether and hydrogen in 1,1,3,3-tetramethyldisiloxane are subjected to addition reaction to introduce epoxy groups to obtain intermediate 1. The terminal amino group in sulfaguanidine is reacted with chlorine in phenylphosphonic acid dichloride to obtain intermediate 2, which is further reacted with the epoxy group in intermediate 1 to generate new hydroxyl groups to obtain a silicon-containing chain extender. Hexamethylene diisocyanate and polyether polyol are prepolymerized under the action of dibutyltin dilaurate catalyst, and then the silicon-containing chain extender is added to react to obtain silicon-modified polyurethane; the hydroxyl group in the silicon-containing chain extender is reacted with chlorine in vinyltrichlorosilane, and the substitution degree of phosphorus, silicon and guanidine groups is also increased to obtain alkenyl silane, and then an aqueous hydrogen peroxide solution is added to the intermediate to carry out epoxidation reaction to obtain epoxy silane.
[0023] When the phosphorus element in silicon-modified polyurethane and epoxy silane is heated, it will decompose to generate phosphoric acid, and further polymerize into polymetaphosphoric acid. The generated polymetaphosphoric acid is a strong dehydrating agent, which can dehydrate the polymer surface to form a carbon film. This carbon film not only isolates the oxygen in the air, thereby achieving a flame retardant effect, but the guanidine group therein will decompose when heated to generate non-flammable gases such as nitrogen and carbon dioxide, isolating oxygen, thereby achieving a flame retardant effect. The silicon element contained therein has a large silicon-oxygen bond energy, which can not only absorb more heat, but also absorb heat to produce a glass-like substance that covers the surface of the material, achieving a flame retardant effect. The sulfur element contained therein can release strong acid at high temperature to promote the dehydration of the substrate into carbon, isolating external oxygen and heat sources, thereby achieving a flame retardant effect, and together constitute a flame retardant system. During the plasticizing process, the terminal hydroxyl groups in the silicon-modified polyurethane and the epoxy groups in the epoxy silane undergo a ring-opening reaction to generate new hydroxyl groups, which continue to react with the anhydride groups in the maleic anhydride-grafted polyvinyl chloride, forming a tight cross-linking network between the three, making them more tightly connected, enhancing their mechanical properties, and improving their compatibility with each other. DETAILED DESCRIPTION
[0024] Example 1
[0025] (1) adding allyl glycidyl ether, tetrahydrofuran solvent and chloroplatinic acid into a reactor, activating at 40° C. for 35 minutes, then dropping 1,1,3,3-tetramethyldisiloxane, wherein the mass ratio of allyl glycidyl ether, chloroplatinic acid and 1,1,3,3-tetramethyldisiloxane is 1:0.02:1.2, the dropping time is 50 minutes, and the reaction is continued at 50° C. for 4 hours. After the reaction is completed, it is cooled to room temperature, an activated carbon adsorbent is added, ultrasonically shaken for 30 minutes, the catalyst chloroplatinic acid is removed, filtered, and rotary evaporated to obtain an intermediate 1;
[0026] (2) adding sulfaguanidine and phenylphosphonic acid dichloride to N,N-dimethylformamide solvent, wherein the mass ratio of sulfaguanidine to phenylphosphonic acid dichloride is 1.3:1, stirring to dissolve, reacting at 16° C. for 6 h, and after the reaction, removing the solvent by rotary evaporation, filtering, washing and drying to obtain intermediate 2;
[0027] (3) adding intermediate 2 to N,N-dimethylformamide solvent, heating in a water bath at 70° C., and then adding intermediate 1 under constant pressure, wherein the mass ratio of intermediate 2 to intermediate 1 is 1:0.8, and continuing the reaction for 8 hours. After the reaction, distilling under reduced pressure, washing and drying are performed to obtain a silicon-containing chain extender;
[0028] (4) adding hexamethylene diisocyanate and polyether polyol into a reaction kettle, adding dibutyltin dilaurate catalyst, and prepolymerizing under a nitrogen atmosphere at a temperature of 70° C. for 4 hours, and then adding a silicon-containing chain extender, wherein the mass ratio of hexamethylene diisocyanate, polyether polyol, dibutyltin dilaurate catalyst, and silicon-containing chain extender is 1.2:1:0.01:0.6. After the reaction is completed, cooling to room temperature to obtain silicon-modified polyurethane;
[0029] (5) adding a silicon-containing chain extender to a chloroform solvent, stirring and dispersing, and continuing to add vinyl trichlorosilane, wherein the mass ratio of the silicon-containing chain extender to vinyl trichlorosilane is 1.6:1, heating to 90° C., reacting for 9 hours, filtering, distilling the filtrate under reduced pressure, washing with deionized water, and drying to obtain olefinated silane;
[0030] (6) adding alkenyl silane to N,N-dimethylformamide solvent, stirring evenly, and then adding aqueous hydrogen peroxide solution thereto, wherein the mass ratio of alkenyl silane to aqueous hydrogen peroxide solution is 1:3.2, stirring and reacting at 30° C. for 4 hours. After the reaction is completed, distilling under reduced pressure, filtering and drying to obtain epoxy silane;
[0031] (7) 15 parts by weight of maleic anhydride grafted polyvinyl chloride, 60 parts by weight of polyvinyl chloride resin, 2 parts by weight of calcium carbonate, 1 part by weight of stearic acid, 8 parts by weight of silicon-modified polyurethane, and 4 parts by weight of epoxy silane were added to a double-roller plasticator, plasticized at 170° C. for 10 min, and then molded in a flat vulcanizer at 175° C. and 8 MPa for 5 min to obtain a PVC composite material for yoga mats.
[0032] Example 2
[0033] (1) adding allyl glycidyl ether, tetrahydrofuran solvent and chloroplatinic acid into a reactor, activating at 55° C. for 40 min, then dropping 1,1,3,3-tetramethyldisiloxane, wherein the mass ratio of allyl glycidyl ether, chloroplatinic acid and 1,1,3,3-tetramethyldisiloxane is 1:0.04:1.3, the dropping time is 60 min, and the reaction is continued at 60° C. for 7 h. After the reaction is completed, the reaction is cooled to room temperature, an activated carbon adsorbent is added, ultrasonically shaken for 40 min, the catalyst chloroplatinic acid is removed, filtered and rotary evaporated to obtain intermediate 1;
[0034] (2) adding sulfaguanidine and phenylphosphonic acid dichloride to N,N-dimethylformamide solvent, wherein the mass ratio of sulfaguanidine to phenylphosphonic acid dichloride is 1.5:1, stirring to dissolve, reacting at 24° C. for 8 h, and after the reaction, removing the solvent by rotary evaporation, filtering, washing and drying to obtain intermediate 2;
[0035] (3) adding intermediate 2 to N,N-dimethylformamide solvent, heating in a water bath at 80° C., and then adding intermediate 1 under constant pressure, wherein the mass ratio of intermediate 2 to intermediate 1 is 1:1.3, and continuing the reaction for 14 hours. After the reaction, distilling under reduced pressure, washing and drying are performed to obtain a silicon-containing chain extender;
[0036] (4) adding hexamethylene diisocyanate and polyether polyol into a reaction kettle, adding dibutyltin dilaurate catalyst, and prepolymerizing under a nitrogen atmosphere at a temperature of 90° C. for 6 hours, and then adding a silicon-containing chain extender, wherein the mass ratio of hexamethylene diisocyanate, polyether polyol, dibutyltin dilaurate catalyst, and silicon-containing chain extender is 1.5:1:0.02:1.2. After the reaction is completed, cooling to room temperature to obtain silicon-modified polyurethane;
[0037] (5) adding a silicon-containing chain extender to a chloroform solvent, stirring and dispersing, and continuing to add vinyl trichlorosilane, wherein the mass ratio of the silicon-containing chain extender to vinyl trichlorosilane is 2.4:1, heating to 110° C., reacting for 12 h, filtering, vacuum distilling the filtrate, washing with deionized water, and drying to obtain olefinated silane;
[0038] (6) adding alkenyl silane to N,N-dimethylformamide solvent, stirring evenly, and then adding aqueous hydrogen peroxide solution thereto, wherein the mass ratio of alkenyl silane to aqueous hydrogen peroxide solution is 1:3.6, stirring and reacting at 40° C. for 6 hours. After the reaction is completed, distilling under reduced pressure, filtering and drying to obtain epoxy silane;
[0039] (7) 20 parts by weight of maleic anhydride grafted polyvinyl chloride, 100 parts by weight of polyvinyl chloride resin, 4 parts by weight of calcium carbonate, 3 parts by weight of stearic acid, 14 parts by weight of silicon-modified polyurethane, and 7 parts by weight of epoxy silane are added to a double-roller plasticator, plasticized at 185° C. for 15 min, and then molded in a flat vulcanizer at 190° C. and 12 MPa for 10 min to obtain a PVC composite material for a yoga mat.
[0040] Example 3
[0041] (1) adding allyl glycidyl ether, tetrahydrofuran solvent and chloroplatinic acid into a reactor, activating at 47° C. for 37.5 min, then dropping 1,1,3,3-tetramethyldisiloxane, wherein the mass ratio of allyl glycidyl ether, chloroplatinic acid and 1,1,3,3-tetramethyldisiloxane is 1:0.03:1.25, the dropping time is 55 min, and the reaction is continued at 55° C. for 5.5 h. After the reaction is completed, the reaction is cooled to room temperature, an activated carbon adsorbent is added, ultrasonically shaken for 35 min, the catalyst chloroplatinic acid is removed, filtered and rotary evaporated to obtain intermediate 1;
[0042] (2) adding sulfaguanidine and phenylphosphonic acid dichloride to N,N-dimethylformamide solvent, wherein the mass ratio of sulfaguanidine to phenylphosphonic acid dichloride is 1.4:1, stirring to dissolve, reacting at 20° C. for 7 h, and after the reaction, removing the solvent by rotary evaporation, filtering, washing and drying to obtain intermediate 2;
[0043] (3) adding intermediate 2 to N,N-dimethylformamide solvent, heating in a water bath at 75° C., and then adding intermediate 1 under constant pressure, wherein the mass ratio of intermediate 2 to intermediate 1 is 1:1.05, and continuing the reaction for 11 hours. After the reaction, distillation under reduced pressure is performed, washing and drying are performed to obtain a silicon-containing chain extender;
[0044] (4) adding hexamethylene diisocyanate and polyether polyol into a reaction kettle, and then adding dibutyltin dilaurate catalyst, and prepolymerizing under a nitrogen atmosphere, the prepolymerization temperature is 80° C., the time is 5 hours, and then adding a silicon-containing chain extender, wherein the mass ratio of hexamethylene diisocyanate, polyether polyol, dibutyltin dilaurate catalyst, and silicon-containing chain extender is 1.35:1:0.015:0.9. After the reaction is completed, cooling to room temperature to obtain silicon-modified polyurethane;
[0045] (5) adding a silicon-containing chain extender to a chloroform solvent, stirring and dispersing, and continuing to add vinyl trichlorosilane, wherein the mass ratio of the silicon-containing chain extender to vinyl trichlorosilane is 2.0:1, heating to 100° C., reacting for 10.5 hours, filtering, distilling the filtrate under reduced pressure, washing with deionized water, and drying to obtain olefinated silane;
[0046] (6) adding alkenyl silane to N,N-dimethylformamide solvent, stirring evenly, and then adding aqueous hydrogen peroxide solution thereto, wherein the mass ratio of alkenyl silane to aqueous hydrogen peroxide solution is 1:3.4, stirring and reacting at 35° C. for 5 h. After the reaction is completed, distilling under reduced pressure, filtering and drying to obtain epoxy silane;
[0047] (7) 17.5 parts by weight of maleic anhydride grafted polyvinyl chloride, 80 parts by weight of polyvinyl chloride resin, 3 parts by weight of calcium carbonate, 2 parts by weight of stearic acid, 11 parts by weight of silicon-modified polyurethane, and 5.5 parts by weight of epoxy silane were added to a double-roller plasticator, plasticized at 177° C. for 12.5 min, and then molded in a flat plate vulcanizer at 180° C. and 10 MPa for 7.5 min to obtain a PVC composite material for a yoga mat.
[0048] Example 4
[0049] (1) adding allyl glycidyl ether, tetrahydrofuran solvent and chloroplatinic acid into a reactor, activating at 40° C. for 35 minutes, then dropping 1,1,3,3-tetramethyldisiloxane, wherein the mass ratio of allyl glycidyl ether, chloroplatinic acid and 1,1,3,3-tetramethyldisiloxane is 1:0.02:1.2, the dropping time is 50 minutes, and the reaction is continued at 50° C. for 4 hours. After the reaction is completed, it is cooled to room temperature, an activated carbon adsorbent is added, ultrasonically shaken for 30 minutes, the catalyst chloroplatinic acid is removed, filtered, and rotary evaporated to obtain an intermediate 1;
[0050] (2) adding sulfaguanidine and phenylphosphonic acid dichloride to N,N-dimethylformamide solvent, wherein the mass ratio of sulfaguanidine to phenylphosphonic acid dichloride is 1.3:1, stirring to dissolve, reacting at 16° C. for 6 h, and after the reaction, removing the solvent by rotary evaporation, filtering, washing and drying to obtain intermediate 2;
[0051] (3) adding intermediate 2 to N,N-dimethylformamide solvent, heating in a water bath at 80° C., and then adding intermediate 1 under constant pressure, wherein the mass ratio of intermediate 2 to intermediate 1 is 1:1.3, and continuing the reaction for 14 hours. After the reaction, distilling under reduced pressure, washing and drying are performed to obtain a silicon-containing chain extender;
[0052] (4) adding hexamethylene diisocyanate and polyether polyol into a reaction kettle, adding dibutyltin dilaurate catalyst, and prepolymerizing under a nitrogen atmosphere at a temperature of 90° C. for 6 hours, and then adding a silicon-containing chain extender, wherein the mass ratio of hexamethylene diisocyanate, polyether polyol, dibutyltin dilaurate catalyst, and silicon-containing chain extender is 1.5:1:0.02:1.2. After the reaction is completed, cooling to room temperature to obtain silicon-modified polyurethane;
[0053] (5) adding a silicon-containing chain extender to a chloroform solvent, stirring and dispersing, and continuing to add vinyl trichlorosilane, wherein the mass ratio of the silicon-containing chain extender to vinyl trichlorosilane is 2.0:1, heating to 100° C., reacting for 10.5 hours, filtering, distilling the filtrate under reduced pressure, washing with deionized water, and drying to obtain olefinated silane;
[0054] (6) adding alkenyl silane to N,N-dimethylformamide solvent, stirring evenly, and then adding aqueous hydrogen peroxide solution thereto, wherein the mass ratio of alkenyl silane to aqueous hydrogen peroxide solution is 1:3.4, stirring and reacting at 35° C. for 5 h. After the reaction is completed, distilling under reduced pressure, filtering and drying to obtain epoxy silane;
[0055] (7) 17.5 parts by weight of maleic anhydride grafted polyvinyl chloride, 80 parts by weight of polyvinyl chloride resin, 3 parts by weight of calcium carbonate, 2 parts by weight of stearic acid, 11 parts by weight of silicon-modified polyurethane, and 5.5 parts by weight of epoxy silane were added to a double-roller plasticator, plasticized at 177° C. for 12.5 min, and then molded in a flat plate vulcanizer at 180° C. and 10 MPa for 7.5 min to obtain a PVC composite material for a yoga mat.
[0056] Comparative Example 1
[0057] The difference between this comparative example and Example 4 is that no silicon-modified polyurethane is added.
[0058] Comparative Example 2
[0059] The difference between this comparative example and Example 4 is that no epoxy silane is added.
[0060] Use an oxygen index meter to test the limiting oxygen index of the material, and use a horizontal and vertical combustion instrument to test the combustion level of the material.
[0061] Table 1: Flame retardancy tests.
[0062] project Limiting oxygen index (%) Combustion level Example 1 31 V-0 Example 2 33 V-0 Example 3 32 V-0 Example 4 33 V-0 Comparative Example 1 20 V-1 Comparative Example 2 21 V-1
[0063] It can be seen from Table 1 that Examples 1-4 of the present invention have better flame retardant effects than Comparative Examples 1-2.
[0064] Tensile properties: Tensile strength and elongation at break were measured according to JIS K6251. The test results are shown in Table 2.
[0065] Table 2: Mechanical properties tests.
[0066] project Tensile strength(Mpa) Elongation at break (%) Example 1 12 125 Example 2 14 128 Example 3 13 127 Example 4 13 126 Comparative Example 1 9.2 115 Comparative Example 2 8.8 116
[0067] It can be seen from Table 2 that Examples 1-4 of the present invention have better mechanical properties than Comparative Examples 1-2.
[0068] The preferred embodiments of the present invention disclosed above are only used to help illustrate the present invention. The preferred embodiments do not describe all the details in detail, nor do they limit the invention to the specific implementation methods described. Obviously, many modifications and changes can be made according to the content of this specification. This specification selects and specifically describes these embodiments in order to better explain the principles and practical applications of the present invention, so that those skilled in the art can understand and use the present invention well. The present invention is limited only by the claims and their full scope and equivalents.
Claims
1. A method for preparing a PVC composite material for a yoga mat, characterized in that: The preparation method of the PVC composite material for yoga mat is as follows: (1) adding allyl glycidyl ether, tetrahydrofuran solvent and chloroplatinic acid to a reactor, activating at 40-55° C. for 35-40 min, then dropping 1,1,3,3-tetramethyldisiloxane for 50-60 min, continuing the reaction at 50-60° C. for 4-7 h, cooling to room temperature after completion, adding activated carbon adsorbent, ultrasonically shaking for 30-40 min, removing the catalyst chloroplatinic acid, filtering, and rotary evaporation to obtain intermediate 1; (2) adding sulfaguanidine and phenylphosphonic acid dichloride to N,N-dimethylformamide solvent, stirring to dissolve, reacting at 16-24° C. for 6-8 hours, and after the reaction, removing the solvent by rotary evaporation, filtering, washing and drying to obtain intermediate 2; (3) adding intermediate 2 to N,N-dimethylformamide solvent, heating in a water bath at 70-80° C., then adding intermediate 1 under constant pressure, continuing the reaction for 8-14 hours, distilling under reduced pressure after the reaction, washing and drying to obtain a silicon-containing chain extender; (4) adding hexamethylene diisocyanate and polyether polyol into a reaction kettle, adding dibutyltin dilaurate as a catalyst, and performing prepolymerization under a nitrogen atmosphere at a temperature of 70-90° C. for 4-6 hours, and then adding a silicon-containing chain extender. After the reaction is completed, cooling to room temperature to obtain a silicon-modified polyurethane; (5) adding the silicon-containing chain extender to the chloroform solvent, stirring and dispersing, continuing to add vinyl trichlorosilane, heating to 90-110° C., reacting for 9-12 hours, filtering, distilling the filtrate under reduced pressure, washing with deionized water, and drying to obtain olefinated silane; (6) adding the olefinated silane to the N,N-dimethylformamide solvent, stirring evenly, and then adding the hydrogen peroxide aqueous solution thereto, stirring and reacting at 30-40° C. for 4-6 hours. After the reaction is completed, distilling under reduced pressure, filtering and drying to obtain epoxy silane; (7) 15-20 parts by weight of maleic anhydride grafted polyvinyl chloride, 60-100 parts by weight of polyvinyl chloride resin, 2-4 parts by weight of calcium carbonate, 1-3 parts by weight of stearic acid, 8-14 parts by weight of silicon-modified polyurethane, and 4-7 parts by weight of epoxy silane are added to a double-roller plasticator, plasticized at 170-185° C. for 10-15 min, and then molded in a flat vulcanizer at 175-190° C. and 8-12 MPa for 5-10 min to obtain a PVC composite material for a yoga mat.
2. The method for preparing a PVC composite material for a yoga mat according to claim 1, characterized in that: The mass ratio of allyl glycidyl ether, chloroplatinic acid and 1,1,3,3-tetramethyldisiloxane in (1) is 1:0.02-0.04:1.2-1.
3.
3. The method for preparing a PVC composite material for a yoga mat according to claim 1, characterized in that: The mass ratio of sulfaguanidine to phenylphosphonic acid dichloride in (2) is 1.3-1.5:
1.
4. The method for preparing a PVC composite material for a yoga mat according to claim 1, characterized in that: The mass ratio of intermediate 2 to intermediate 1 in (3) is 1:0.8-1.
3.
5. The method for preparing a PVC composite material for a yoga mat according to claim 1, characterized in that: The mass ratio of hexamethylene diisocyanate, polyether polyol, dibutyltin dilaurate catalyst and silicon-containing chain extender in (4) is 1.2-1.5:1:0.01-0.02:0.6-1.
2.
6. The method for preparing a PVC composite material for a yoga mat according to claim 1, characterized in that: The mass ratio of the silicon-containing chain extender to vinyl trichlorosilane in (5) is 1.6-2.4:
1.
7. The method for preparing a PVC composite material for a yoga mat according to claim 1, characterized in that: The mass ratio of alkenyl silane to aqueous hydrogen peroxide solution in (6) is 1:3.2-3.6.
Citation Information
Cited By
Flame-retardant cable and preparation method thereof
CN119192712A