Coating with low cost, high infrared emissivity and strong binding force and preparation method thereof
By using nanocarbon black, polyimide resin and p-toluenesulfonylhydrazide, combined with air spraying and heat treatment, low-cost, high infrared emissivity and strong binding force coatings were prepared, and the process in the prior art was solved The complex and cost-effective heat control effect is achieved.
Patent Information
- Application Number
- CN202411263499.5
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-09-10
- Publication Date
- 2024-11-15
AI Technical Summary
The existing high infrared emissivity coating preparation process is complex and costly, making it difficult to prepare high emissivity and strong binding force coatings with uniform pore distribution at low temperatures.
Nanocarbon black, thermoset polyimide resin and p-toluenesulfonylhydrazide are used as the main materials, and a microporous structure coating is formed through air spraying and heat treatment processes to optimize the pore structure and adhesion of the coating.
It realizes a low-cost, high infrared emissivity and strong binding force coating, improves the stability of the spraying process, and the emissivity can reach more than 0.94. The coating is resistant to high temperature and fatigue, and is suitable for large-scale industrial production.
Smart Images

Figure CN118956257A_ABST
Abstract
Description
Technical Field
[0001] The invention belongs to the technical field of infrared radiation coating materials, and relates to a low-cost, high-infrared emissivity and strong bonding coating and a preparation method thereof. Background Art
[0002] With the rapid development of high-power integrated circuits and high-power electronic components, greater requirements are placed on the thermal protection performance of the surfaces of metal materials and composite materials as key structural materials. However, most metal materials and composite materials have a high reflectivity to infrared radiation, so the infrared emissivity is low, and the surface radiation heat dissipation capacity is poor. The surface heat cannot be dissipated in time, which can easily lead to uneven distribution of thermal stress in the components and cause failure. Therefore, in order to further improve the thermal management and control capabilities of the material, preparing a high infrared emissivity coating on its surface can achieve a faster heat dissipation thermal management effect.
[0003] High-emissivity materials are mainly spinel, perovskite, cordierite ceramic materials, semiconductor materials and nanomaterials. At present, the high-infrared emissivity coatings studied by many scholars mostly use one or more of these materials as high-emissivity fillers, and then use plasma spraying, electroplating or pyrolytic carbon deposition to better combine the coating with the substrate. The preparation cost is high and the process is complicated, which is not suitable for large-scale preparation. Reference 1 "Xu M, Yuan J, Lu X, et al. Infrared radiation and thermal cyclic performance of a high-entropy rare-earth hexaaluminate coating prepared by atmospheric plasma spraying [J]. CERAMICS INTERNATIONAL, 2022 (18): 48." High-entropy RMgAl was prepared by atmospheric plasma spraying technology. 11 O 19(HE-RMA, R = La, Pr, Nd, Sm, Gd) coating, when annealed at 1100 ° C for 100h, still shows high infrared emissivity (0.932 at 1000 ° C). However, the cost of plasma spraying is high and the spraying efficiency is low, which is not suitable for large-scale preparation. Reference 2 "Vinetsky Y, Jambu J, Mandler D, et al. CNT-Based Solar Thermal Coatings: Absorptance vs. Emittance [J]. Coatings, 2020, 10 (11): 1101." Carbon nanotubes are dispersed in a solvent by air spraying and then sprayed on a substrate to obtain a high emissivity coating with a maximum emissivity of 0.9. Although the air spraying method is simple and low in cost, the price of carbon nanotube raw materials is relatively high. Reference 3 "Song, Guangping He, Shifeng He, Fei Yao, Yongtao Li, Jianjun Li, Mingwei He, Xiaodong. Effect of doping graphene oxide on the structure and properties of SiO2 based high emissivity coatings [J]. Journal of Applied Polymer Science, 2020, 137 (23a24)." Graphene oxide was doped into inorganic SiO2-based coatings in different proportions, and a high-emissivity coating was prepared on the surface of an iron-based alloy by spraying and heat treatment at 850°C. The emissivity was above 0.85, but this method requires high-temperature heat treatment, which is costly and has high requirements on the high-temperature resistance of the substrate, and has a small scope of application.
[0004] Therefore, optimizing the coating preparation process, reducing the cost of raw materials and equipment, and preparing high-emissivity and strong bonding coatings with uniform pore distribution at a lower temperature have become urgent issues to be solved in this field. Summary of the invention
[0005] The purpose of the present invention is to provide a low-cost, high-infrared emissivity and strong bonding coating and a preparation method thereof, so as to solve the problems of complex coating preparation process and high preparation cost in the prior art.
[0006] In order to achieve the above object, the present invention adopts the following technical solutions:
[0007] A low-cost, high-infrared emissivity and strong bonding coating comprises, by mass, 10-30 parts of nano carbon black, 40-100 parts of a binder, 1-4 parts of a foaming agent, 200-600 parts of NN dimethylacetamide and 1000-1500 parts of anhydrous ethanol.
[0008] Furthermore, the binder is a thermosetting polyimide resin;
[0009] The foaming agent is p-toluenesulfonyl hydrazide.
[0010] Furthermore, the particle size of the nano carbon black is 30 to 80 nm.
[0011] Furthermore, the thickness of the low-cost, high infrared emissivity and strong bonding coating is 50-100 μm.
[0012] A method for preparing the coating with low cost, high infrared emissivity and strong bonding strength comprises:
[0013] Dissolving polyimide resin powder in NN dimethylacetamide to obtain a polyimide solution;
[0014] Add nano carbon black to anhydrous ethanol in batches, and ultrasonically disperse each time until no obvious agglomerated particles are present. Add p-toluenesulfonyl hydrazide and ultrasonically disperse again. Add polyimide solution and ultrasonically disperse uniformly to obtain a coating slurry.
[0015] The coating slurry is evenly sprayed on the surface of the substrate by air spraying, and the sprayed substrate is heat treated under a protective atmosphere to obtain a low-cost, high infrared emissivity and strong bonding coating.
[0016] Furthermore, the mass ratio of the polyimide resin powder to NN dimethylacetamide is 1:4-8.
[0017] Furthermore, the mass fraction of the polyimide solution added to the coating slurry is 100 to 600 parts.
[0018] Furthermore, the air spraying method uses a spray gun with a caliber of 0.5 to 1.5 mm, a spraying pressure of 0.2 to 0.4 MPa, a distance between the nozzle of the spray gun and the substrate of 10 to 30 cm, and a spraying frequency of 3 to 5 times.
[0019] Furthermore, the protective atmosphere is argon.
[0020] Furthermore, the heat treatment process includes: slowly heating up to 100°C, keeping the temperature constant for 30 minutes, then heating up to 130-150°C, keeping the temperature constant for 40 minutes, and then heating up to 250-300°C, keeping the temperature constant for 1-2 hours.
[0021] Compared with the prior art, the present invention has the following beneficial effects:
[0022] The present invention provides a low-cost, high-infrared emissivity and strong bonding coating. By selecting low-priced commercial nano carbon black as the main high-emissivity filler and adding a thermosetting polyimide resin with good heat resistance and bonding properties as a binder, the problem of poor bonding after the coating is sprayed is solved. At the same time, p-toluenesulfonyl hydrazide is added to the coating slurry, and its pyrolysis and foaming characteristics are used to optimize the pore structure of the coating, thereby avoiding the complete film formation of the binder, and finally forming a microporous structure coating, solving the problem that it is difficult to obtain both high infrared emissivity and high bonding strength of the coating. The present invention selects low-priced commercial raw materials as the main materials of the coating, optimizes the composition of the coating, and prepares an infrared high-emissivity coating with good interface bonding, high temperature resistance and low cost through a simple preparation process.
[0023] Furthermore, after adding p-toluenesulfonyl hydrazide to the slurry, the coating is pyrolyzed and foamed, the distribution of nano carbon black and polyimide resin on the surface is adjusted, and a large number of network structures with nano-scale pores are formed on the surface of the coating, which is conducive to improving the surface infrared radiation capacity, avoiding the complete film formation of polyimide resin, increasing the contact area between carbon black particles, and improving the thermal conductivity of the coating. At the same time, it effectively solves the problem of large deviation of emissivity results caused by particle agglomeration during large-scale preparation, greatly improves the stability of the spraying process, and the average emissivity in the 1-22μm band can reach more than 0.94.
[0024] Furthermore, the polyimide resin in the coating has good high temperature resistance after curing and can be used for a long time below 380°C. It also has strong toughness, good fatigue resistance and excellent adhesion, making the coating highly durable and having a long service life.
[0025] The present invention also provides a method for preparing a coating with high infrared emissivity and strong binding force at low cost, which utilizes the characteristic of p-toluenesulfonyl hydrazide to generate N2 by heating and decomposing, and uses air spraying method and appropriate heat treatment process to make p-toluenesulfonyl hydrazide foam in the coating. The release of these gases can construct a uniform nano-network structure with polyimide resin as the skeleton and nano carbon black as the high emissivity filler on the coating surface, which maintains the stability of the performance while having high emissivity. The excellent adhesion and temperature resistance of polyimide after complete curing make it have excellent binding force. The preparation process of the present invention is simple, the cycle is short and the cost is low, and it can be used for large-scale industrial production, and the prepared microporous structure coating has the advantages of high emissivity, good binding force, controllable pores and low density, etc., which meets the heat dissipation requirements of most metals and composite materials. BRIEF DESCRIPTION OF THE DRAWINGS
[0026] In order to more clearly illustrate the technical solutions of the embodiments of the present invention, the drawings required for use in the embodiments are briefly introduced below. It should be understood that the following drawings only show certain embodiments of the present invention and therefore should not be regarded as limiting the scope. For ordinary technicians in this field, other related drawings can be obtained based on these drawings without creative work.
[0027] Figure 1 This is a macroscopic morphology of the coating with high infrared emissivity and strong bonding strength prepared in Example 1 of the present invention.
[0028] Figure 2 This is a surface microscopic morphology of the coating after spraying in Example 1 of the present invention.
[0029] Figure 3 This is a surface microscopic morphology of the coating after heat treatment and curing in Example 1 of the present invention.
[0030] Figure 4 This is a surface microscopic morphology of the coating when no blowing agent p-benzenesulfonylhydrazine is added in Comparative Example 1 of the present invention.
[0031] Figure 5 This is a surface microscopic morphology of the coating when no polyimide resin is added in Comparative Example 2 of the present invention. DETAILED DESCRIPTION
[0032] In order to enable those skilled in the art to understand the characteristics and effects of the present invention, the following is a general description and definition of the terms and expressions mentioned in the specification and claims. Unless otherwise specified, all technical and scientific terms used in the text are the common meanings understood by those skilled in the art for the present invention. In the event of a conflict, the definition in this specification shall prevail.
[0033] The theories or mechanisms described and disclosed herein, whether correct or incorrect, should not limit the scope of the present invention in any way, that is, the present invention can be implemented without being limited by any specific theory or mechanism.
[0034] Herein, all features such as values, quantities, contents and concentrations defined in the form of numerical ranges or percentage ranges are for simplicity and convenience only. Accordingly, the description of numerical ranges or percentage ranges should be considered to have included and specifically disclosed all possible secondary ranges and individual values within the range (including integers and fractions).
[0035] In this document, unless otherwise specified, “includes,” “including,” “contains,” “has,” or similar terms cover the meanings of “consisting of” and “mainly consisting of,” for example, “A includes a” covers the meanings of “A includes a and other” and “A only includes a.”
[0036] In this document, in order to make the description concise, not all possible combinations of various technical features in various embodiments or examples are described. Therefore, as long as there is no contradiction in the combination of these technical features, the various technical features in various embodiments or examples can be combined arbitrarily, and all possible combinations should be considered to be within the scope of this specification.
[0037] The present invention will be further described below in conjunction with specific embodiments. It should be understood that these embodiments are only used to illustrate the present invention and are not intended to limit the scope of the present invention. In addition, it should be understood that after reading the content taught by the present invention, those skilled in the art can make various changes or modifications to the present invention, and these equivalent forms fall within the scope limited by the appended claims of the application equally.
[0038] The following examples use conventional instruments and equipment in the art. The experimental methods in the following examples where specific conditions are not specified are usually carried out under conventional conditions or under conditions recommended by the manufacturer. The various raw materials used in the following examples are conventional commercial products unless otherwise specified, and their specifications are conventional specifications in the art. In the specification of the present invention and the following examples, unless otherwise specified, "%" means weight percentage, "part" means weight part, and ratio means weight ratio.
[0039] The present invention is further described in detail below in conjunction with the accompanying drawings:
[0040] The invention provides a low-cost, high-infrared emissivity and strong bonding coating, which comprises, by mass, 10-30 parts of nano carbon black, 40-100 parts of a binder, 1-4 parts of a foaming agent, 200-600 parts of NN dimethylacetamide and 1000-1500 parts of anhydrous ethanol.
[0041] The binder is a thermosetting polyimide resin, and the cured polyimide resin is used as a matrix to reinforce the coating, so that it has excellent bonding strength with the substrate.
[0042] The foaming agent is p-toluenesulfonyl hydrazide. The characteristic of p-toluenesulfonyl hydrazide that it decomposes upon heating to produce N2 is utilized. After being treated with a suitable spraying process and an appropriate heat treatment process, p-toluenesulfonyl hydrazide is foamed in the coating. The release of these gases can construct a uniform nano-network structure on the coating surface with a polyimide resin as the skeleton and nano-carbon black as a high-emissivity filler, thereby maintaining performance stability while having a high emissivity.
[0043] Preferably, the nano carbon black is a spherical particle with a diameter of 30 to 80 nm.
[0044] The present invention also provides a method for preparing a coating with low cost, high infrared emissivity and strong bonding strength, comprising the following steps:
[0045] S1. Weigh appropriate amounts of NN dimethylacetamide and polyimide resin powder in a weight ratio of 4 to 8:1 in a beaker, and stir evenly at room temperature to fully dissolve the polyimide to obtain a polyimide solution;
[0046] S2, adding 10 to 30 parts of nano carbon black into 1000 to 1500 parts of anhydrous ethanol twice, each time ultrasonically dispersing for 10 minutes, the obtained slurry should have no obvious agglomerated particles on the inner wall of the beaker when shaking, adding 1 to 4 parts of p-toluenesulfonyl hydrazide to the obtained dispersed slurry and then ultrasonically dispersing for 10 minutes, and finally adding 100 to 600 parts of polyimide solution and ultrasonically dispersing for 20 minutes to obtain a coating slurry;
[0047] S3. Pour the coating slurry into the spray gun and use an air compressor to evenly spray it on the surface of the sample. The spray gun caliber is 0.5-1.5 mm, the spraying pressure is 0.2-0.4 MPa, the distance between the spray gun nozzle and the substrate is 10-30 cm, spray 3-5 times, and the spraying thickness is 50-100 μm;
[0048] S4. Place the sprayed substrate in a heat treatment furnace, slowly heat it to 100°C in an argon protective atmosphere, keep the temperature constant for 30 minutes, remove the solvent, then heat it to 130-150°C, keep it warm for 40 minutes, so that the foaming agent p-toluenesulfonyl hydrazide can fully decompose and release N2, continue to heat it to 200-300°C, keep it warm for 1-2 hours, so that the polyimide is completely cured to obtain a low-cost, high infrared emissivity coating with excellent bonding strength.
[0049] The present invention will be further described below by means of specific embodiments:
[0050] Embodiment 1:
[0051] A method for preparing a coating with low cost, high infrared emissivity and strong bonding strength comprises the following steps:
[0052] S1. Weigh appropriate amounts of NN dimethylacetamide and polyimide resin powder in a weight ratio of 5:1 into a beaker, and stir evenly at room temperature to fully dissolve the polyimide to obtain a polyimide solution;
[0053] S2, adding 15 parts of nano carbon black to 1000 parts of anhydrous ethanol twice, each time ultrasonically dispersing for 10 minutes, the obtained slurry should have no obvious agglomerated particles on the inner wall of the beaker when shaking, adding 2 parts of p-toluenesulfonyl hydrazide to the obtained dispersed slurry and then ultrasonically dispersing for 10 minutes, and finally adding 360 parts of polyimide solution and ultrasonically dispersing for 20 minutes to obtain a coating slurry;
[0054] S3. Pour the coating slurry into the spray gun and use an air compressor to evenly spray it on the surface of the sample. The spray gun caliber is 1mm, the spraying pressure is 0.3MPa, the distance between the nozzle of the paint spray gun and the substrate is 10cm, spray 3 times, and the spraying thickness is 70μm;
[0055] S4. Place the sprayed substrate in a heat treatment furnace, slowly heat it to 100°C in an argon protective atmosphere, keep the temperature constant for 30 minutes, remove the solvent, then heat it to 140°C and keep it warm for 40 minutes to allow the foaming agent p-toluenesulfonyl hydrazide to fully decompose and release N2, then continue to heat it to 200°C and keep it warm for 1 hour to completely cure the polyimide to obtain a low-cost, high infrared emissivity coating with excellent bonding strength.
[0056] The low-cost, high infrared emissivity and strong bonding strength coating prepared in this embodiment has an average emissivity of 0.94 in the 1-22 μm band, a coating bonding strength of 6.2 MPa, and can be used for a long time below 400° C.
[0057] Embodiment 2:
[0058] A method for preparing a coating with low cost, high infrared emissivity and strong bonding strength comprises the following steps:
[0059] S1. Weigh appropriate amounts of NN dimethylacetamide and polyimide resin powder in a weight ratio of 5:1 into a beaker, and stir evenly at room temperature to fully dissolve the polyimide to obtain a polyimide solution;
[0060] S2, adding 15 parts of nano carbon black to 1000 parts of anhydrous ethanol twice, each time ultrasonically dispersing for 10 minutes, the obtained slurry should have no obvious agglomerated particles on the inner wall of the beaker when shaking, adding 2 parts of p-toluenesulfonyl hydrazide to the obtained dispersed slurry and then ultrasonically dispersing for 10 minutes, and finally adding 270 parts of polyimide solution and ultrasonically dispersing for 20 minutes to obtain a coating slurry;
[0061] S3. Pour the coating slurry into the spray gun and use an air compressor to evenly spray it on the surface of the sample. The spray gun caliber is 1mm, the spraying pressure is 0.3MPa, the distance between the nozzle of the paint spray gun and the substrate is 10cm, spray 3 times, and the spraying thickness is 60μm;
[0062] S4. Place the sprayed substrate in a heat treatment furnace, slowly heat it to 100°C in an argon protective atmosphere, keep the temperature constant for 30 minutes, remove the solvent, then heat it to 140°C and keep it warm for 40 minutes to allow the foaming agent p-toluenesulfonyl hydrazide to fully decompose and release N2, then continue to heat it to 200°C and keep it warm for 1 hour to completely cure the polyimide to obtain a low-cost, high infrared emissivity coating with excellent bonding strength.
[0063] The low-cost, high infrared emissivity and strong bonding strength coating prepared in this embodiment has an average emissivity of 0.95 in the 1-22 μm band, a coating bonding strength of 5.1 MPa, and can be used for a long time below 400° C.
[0064] Embodiment 3:
[0065] A method for preparing a coating with low cost, high infrared emissivity and strong bonding strength comprises the following steps:
[0066] S1. Weigh appropriate amounts of NN dimethylacetamide and polyimide resin powder in a weight ratio of 5:1 into a beaker, and stir evenly at room temperature to fully dissolve the polyimide to obtain a polyimide solution;
[0067] S2, adding 15 parts of nano carbon black to 1000 parts of anhydrous ethanol twice, each time ultrasonically dispersing for 10 minutes, the obtained slurry should have no obvious agglomerated particles on the inner wall of the beaker when shaking, adding 2 parts of p-toluenesulfonyl hydrazide to the obtained dispersed slurry and then ultrasonically dispersing for 10 minutes, and finally adding 180 parts of polyimide solution and ultrasonically dispersing for 20 minutes to obtain a coating slurry;
[0068] S3. Pour the coating slurry into the spray gun and use an air compressor to evenly spray it on the surface of the sample. The spray gun caliber is 1mm, the spraying pressure is 0.3MPa, the distance between the nozzle of the paint spray gun and the substrate is 10cm, spray 3 times, and the spraying thickness is 50μm;
[0069] S4. Place the sprayed substrate in a heat treatment furnace, slowly heat it to 100°C in an argon protective atmosphere, keep the temperature constant for 30 minutes, remove the solvent, then heat it to 140°C and keep it warm for 40 minutes to allow the foaming agent p-toluenesulfonyl hydrazide to fully decompose and release N2, then continue to heat it to 200°C and keep it warm for 1 hour to completely cure the polyimide to obtain a low-cost, high infrared emissivity coating with excellent bonding strength.
[0070] The low-cost, high-infrared emissivity and strong bonding coating prepared in this embodiment has an average emissivity of 0.96 in the 1-22 μm band, a coating bonding strength of 3.8 MPa, and can be used for a long time below 400°C.
[0071] Embodiment 4:
[0072] A method for preparing a coating with low cost, high infrared emissivity and strong bonding strength comprises the following steps:
[0073] S1. Weigh appropriate amounts of NN dimethylacetamide and polyimide resin powder in a weight ratio of 5:1 into a beaker, and stir evenly at room temperature to fully dissolve the polyimide to obtain a polyimide solution;
[0074] S2, adding 15 parts of nano carbon black to 1000 parts of anhydrous ethanol twice, each time ultrasonically dispersing for 10 minutes, the obtained slurry should have no obvious agglomerated particles on the inner wall of the beaker when shaking, adding 2 parts of p-toluenesulfonyl hydrazide to the obtained dispersed slurry and then ultrasonically dispersing for 10 minutes, and finally adding 450 parts of polyimide solution and ultrasonically dispersing for 20 minutes to obtain a coating slurry;
[0075] S3. Pour the coating slurry into the spray gun and use an air compressor to evenly spray it on the surface of the sample. The spray gun caliber is 1mm, the spraying pressure is 0.3MPa, the distance between the nozzle of the paint spray gun and the substrate is 10cm, spray 3 times, and the spraying thickness is 80μm;
[0076] S4. Place the sprayed substrate in a heat treatment furnace, slowly heat it to 100°C in an argon protective atmosphere, keep the temperature constant for 30 minutes, remove the solvent, then heat it to 140°C and keep it warm for 40 minutes to allow the foaming agent p-toluenesulfonyl hydrazide to fully decompose and release N2, then continue to heat it to 200°C and keep it warm for 1 hour to completely cure the polyimide to obtain a low-cost, high infrared emissivity coating with excellent bonding strength.
[0077] The low-cost, high infrared emissivity and strong bonding strength coating prepared in this embodiment has an average emissivity of 0.92 in the 1-22 μm band, a coating bonding strength of 7.8 MPa, and can be used for a long time below 400° C.
[0078] Embodiment 5:
[0079] A method for preparing a coating with low cost, high infrared emissivity and strong bonding strength comprises the following steps:
[0080] S1. Weigh appropriate amounts of N-N-dimethylacetamide and polyimide resin powder in a weight ratio of 4:1 into a beaker, and stir evenly at room temperature to fully dissolve the polyimide to obtain a polyimide solution;
[0081] S2, adding 30 parts of nano carbon black to 1500 parts of anhydrous ethanol twice, each time ultrasonically dispersing for 10 minutes, the obtained slurry should have no obvious agglomerated particles on the inner wall of the beaker when shaking, adding 4 parts of p-toluenesulfonyl hydrazide to the obtained dispersed slurry and then ultrasonically dispersing for 10 minutes, and finally adding 600 parts of polyimide solution and ultrasonically dispersing for 20 minutes to obtain a coating slurry;
[0082] S3. Pour the coating slurry into the spray gun and use an air compressor to evenly spray it on the surface of the sample. The spray gun caliber is 1.5 mm, the spraying pressure is 0.4 MPa, the distance between the nozzle of the paint spray gun and the substrate is 30 cm, spray 5 times, and the spraying thickness is 100 μm;
[0083] S4. Place the sprayed substrate in a heat treatment furnace, slowly heat it to 100°C in an argon protective atmosphere, keep the temperature constant for 30 minutes, remove the solvent, then heat it to 150°C and keep it warm for 40 minutes to allow the foaming agent p-toluenesulfonyl hydrazide to fully decompose and release N2, then continue to heat it to 300°C and keep it warm for 1 hour to completely cure the polyimide to obtain a low-cost, high infrared emissivity coating with excellent bonding strength.
[0084] The low-cost, high-infrared emissivity and strong bonding coating prepared in this embodiment has an average emissivity of 0.9 in the 1-22 μm band, a coating bonding strength of 7.1 MPa, and can be used for a long time below 400° C.
[0085] Embodiment 6:
[0086] A method for preparing a coating with low cost, high infrared emissivity and strong bonding strength comprises the following steps:
[0087] S1. Weigh appropriate amounts of NN dimethylacetamide and polyimide resin powder in a weight ratio of 8:1 into a beaker, and stir evenly at room temperature to fully dissolve the polyimide to obtain a polyimide solution;
[0088] S2, adding 10 parts of nano carbon black to 1000 parts of anhydrous ethanol twice, each time ultrasonically dispersing for 10 minutes, the obtained slurry should have no obvious agglomerated particles on the inner wall of the beaker when shaking, adding 1 part of p-toluenesulfonyl hydrazide to the obtained dispersed slurry and then ultrasonically dispersing for 10 minutes, and finally adding 100 parts of polyimide solution and ultrasonically dispersing for 20 minutes to obtain a coating slurry;
[0089] S3. Pour the coating slurry into the spray gun and use an air compressor to evenly spray it on the surface of the sample. The spray gun caliber is 0.8mm, the spraying pressure is 0.2MPa, the distance between the nozzle of the paint spray gun and the substrate is 10cm, spray 3 times, and the spraying thickness is 50μm;
[0090] S4. Place the sprayed substrate in a heat treatment furnace, slowly heat it to 100°C in an argon protective atmosphere, keep the temperature constant for 30 minutes, remove the solvent, then heat it to 130°C and keep it warm for 40 minutes to allow the foaming agent p-toluenesulfonyl hydrazide to fully decompose and release N2, then continue to heat it to 250°C and keep it warm for 2 hours to completely cure the polyimide to obtain a low-cost, high infrared emissivity coating with excellent bonding strength.
[0091] The low-cost, high-infrared emissivity and strong bonding coating prepared in this embodiment has an average emissivity of 0.9 in the 1-22 μm band, a coating bonding strength of 4.3 MPa, and can be used for a long time below 400° C.
[0092] Comparative Example 1
[0093] The difference between this comparative example and Example 1 is that p-toluenesulfonyl hydrazide is not added, and the comparative example is prepared by the following method:
[0094] S1. Weigh appropriate amounts of NN dimethylacetamide and polyimide resin powder in a weight ratio of 5:1 into a beaker, and stir evenly at room temperature to fully dissolve the polyimide to obtain a polyimide solution;
[0095] S2, adding 15 parts of nano carbon black to 1000 parts of anhydrous ethanol twice, each time ultrasonically dispersing for 10 minutes, the obtained slurry should have no obvious agglomerated particles on the inner wall of the beaker when shaking, adding 360 parts of polyimide solution to the obtained dispersed slurry and ultrasonically dispersing for 20 minutes to obtain a coating slurry;
[0096] S3. Pour the coating slurry into the spray gun and use an air compressor to evenly spray it on the surface of the sample. The spray gun caliber is 1mm, the spraying pressure is 0.3MPa, the distance between the nozzle of the paint spray gun and the substrate is 10cm, spray 3 times, and the spraying thickness is 70μm;
[0097] S4. Place the sprayed substrate in a heat treatment furnace, slowly heat it to 100°C in an argon protective atmosphere, keep the temperature constant for 30 minutes, remove the solvent, continue to heat it to 200°C, keep the temperature constant for 1 hour, so that the polyimide is completely cured to obtain a coating.
[0098] The coating prepared in this comparative example has an average emissivity of 0.90 in the 1-22 μm band, and a coating bonding strength of 5.8 MPa.
[0099] Comparative Example 2:
[0100] The difference between this comparative example and Example 1 is that no polyimide resin is added, and the comparative example is prepared by the following method:
[0101] S1. Add 15 parts of nano carbon black to 1000 parts of anhydrous ethanol twice, and ultrasonically disperse for 10 minutes each time. When the obtained slurry is shaken, there should be no obvious agglomerated particles on the inner wall of the beaker. Add 2 parts of p-toluenesulfonyl hydrazide to the obtained dispersed slurry and then ultrasonically disperse for 10 minutes to obtain a coating slurry;
[0102] S3. Pour the coating slurry into the spray gun and use an air compressor to evenly spray it on the surface of the sample. The spray gun caliber is 1mm, the spraying pressure is 0.3MPa, the distance between the nozzle of the paint spray gun and the substrate is 10cm, spray 3 times, and the spraying thickness is 60μm;
[0103] S4. Place the sprayed substrate in a heat treatment furnace, slowly heat it to 100°C in an argon protective atmosphere, keep the temperature constant for 30 minutes, remove the solvent, then heat it to 140°C and keep it constant for 40 minutes to allow the foaming agent p-toluenesulfonyl hydrazide to fully decompose and release N2 to obtain a coating.
[0104] The average emissivity of the coating prepared in this comparative example in the 1-22 μm band is 0.97, and the coating bonding force is 0.5 MPa.
[0105] In order to illustrate the relevant properties of the coating prepared by the present invention, the coating prepared in Example 1 is analyzed and explained in combination with Comparative Examples 1 and 2. Figures 1 to 5 shown.
[0106] like Figure 1 As shown, the macroscopic morphology of the low-cost, high infrared emissivity and strong bonding coating prepared on the carbon / carbon composite material substrate in Example 1 has a smooth, black surface and no obvious defects.
[0107] like Figure 2 As shown, it is a scanning electron microscope photograph of the coating after spraying but not heat-treated in Example 1. The surface is a microporous rough structure, the carbon black particles are relatively fluffy, there is no material bonding, and the coating bonding strength is poor.
[0108] like Figure 3 As shown in FIG. 1 , it is a scanning electron microscope photograph of the coating after heat treatment in Example 1. The carbon black particles are tightly bonded by the polyimide resin, and a rich pore structure remains after being foamed by p-toluenesulfonylhydrazine. Figure 4 The sealing phenomenon in the middle has been greatly improved.
[0109] like Figure 4 The following is a scanning electron microscope image of the coating after heat treatment when p-toluenesulfonyl hydrazide is not added in Comparative Example 1. Figure 4 It can be seen that when p-toluenesulfonyl hydrazide foaming agent is not added, the pore size and quantity of the coating surface are reduced, and the coating surface has strong heterogeneity.
[0110] like Figure 5 The following is a scanning electron microscope image of the coating after heat treatment when no polyimide resin is added in Comparative Example 2. Figure 5 It can be seen that when polyimide resin is not added, the contact area between the nanoparticles is small, and they are loosely stacked together and mechanically connected, with poor bonding strength.
[0111] The above are only preferred embodiments of the present invention and are not intended to limit the present invention. For those skilled in the art, the present invention may have various modifications and variations. Any modification, equivalent replacement, improvement, etc. made within the spirit and principle of the present invention shall be included in the protection scope of the present invention.
Claims
1. A low-cost, high infrared emissivity and strong bonding coating, characterized in that: Calculated by mass, it includes 10-30 parts of nano carbon black, 40-100 parts of binder, 1-4 parts of foaming agent, 200-600 parts of NN dimethylacetamide and 1000-1500 parts of anhydrous ethanol.
2. A low-cost, high infrared emissivity and strong bonding coating according to claim 1, characterized in that: The binder is a thermosetting polyimide resin; The foaming agent is p-toluenesulfonyl hydrazide.
3. A low-cost, high infrared emissivity and strong bonding coating according to claim 1, characterized in that: The particle size of the nano carbon black is 30 to 80 nm.
4. A low-cost, high infrared emissivity and strong bonding coating according to claim 1, characterized in that: The thickness of the low-cost, high-infrared emissivity and strong bonding coating is 50-100 μm.
5. A method for preparing a low-cost, high-infrared emissivity and strong bonding coating as claimed in any one of claims 1 to 4, characterized in that: include: Dissolving polyimide resin powder in NN dimethylacetamide to obtain a polyimide solution; Add nano carbon black to anhydrous ethanol in batches, and ultrasonically disperse each time until no obvious agglomerated particles are present. Add p-toluenesulfonyl hydrazide and ultrasonically disperse again. Add polyimide solution and ultrasonically disperse uniformly to obtain a coating slurry. The coating slurry is evenly sprayed on the surface of the substrate by air spraying, and the sprayed substrate is heat treated under a protective atmosphere to obtain a low-cost, high-infrared emissivity and strong bonding coating.
6. The method for preparing a coating with low cost, high infrared emissivity and strong bonding force according to claim 5, characterized in that: The mass ratio of the polyimide resin powder to NN dimethylacetamide is 1:(4-8).
7. The method for preparing a coating with low cost, high infrared emissivity and strong bonding force according to claim 5, characterized in that: The mass fraction of the polyimide solution added to the coating slurry is 100 to 600 parts.
8. The method for preparing a coating with low cost, high infrared emissivity and strong bonding strength according to claim 5, characterized in that: The air spraying method uses a spray gun with a caliber of 0.5 to 1.5 mm, a spray pressure of 0.2 to 0.4 MPa, a distance between the nozzle of the spray gun and the substrate of 10 to 30 cm, and a spraying frequency of 3 to 5 times.
9. The method for preparing a coating with low cost, high infrared emissivity and strong bonding force according to claim 5, characterized in that: The protective atmosphere is argon.
10. The method for preparing a coating with low cost, high infrared emissivity and strong bonding strength according to claim 5, characterized in that: The heat treatment process includes: slowly heating up to 100° C., keeping the temperature constant for 30 minutes, then heating up to 130-150° C., keeping the temperature constant for 40 minutes, and then heating up to 250-300° C., keeping the temperature constant for 1-2 hours.
Citation Information
Patent Citations
Coating with high infrared emissivity and strong binding force on surface of carbon / carbon composite material as well as preparation method and application of coating
CN117186728A
Polyimide / inorganic nano-composite insulating varnish and its preparation method
CN1718658A
Expanded coating, preparation method and use thereof, and permanent magnet comprising same
US20240101836A1