Method for chlorine-free removal of antimony and tellurium in anode slime through multi-section pressurization

Through the multi-stage pressurized chlorine-free removal method, the antimony and tellurium in the anode mud are deeply removed under alkaline conditions by using the thiourea and vulcanization reaction, which solves the equipment corrosion and environmental pollution problems of the chlorination removal process in the prior art. , realizes chlorine-free and environmentally friendly metal recycling and tail fluid treatment.

CN118957264AActive Publication Date: 2024-11-15JIANGXI COPPER GRP (GUIXI) SMELTING NEW TECH CO LTD
View PDF 5 Cites 0 Cited by

Patent Information

Application Number
CN202411026689.5
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-07-30
Publication Date
2024-11-15
Estimated Expiration
2044-07-30

AI Technical Summary

Technical Problem

In the existing anode mud treatment methods, the process of acidic chlorination to remove antimony tellurium produces high-corrosive waste liquid with high corrosion, and it is difficult to deal with harmful substances, affecting the environment.

Method used

Multi-stage pressurized chlorine-free removal method, including one-stage pressurized thiourea transformation depth decopper and two-stage pressurized chlorine-free decompressed antimony and tellurium, using alkaline media, through precipitation, filtration and catalytic treatment, the tail liquid is removed. by-products and heavy metal ions are converted into harmless substances.

Benefits of technology

It reduces equipment corrosion damage, realizes effective treatment of harmful substances, and meets emission standards, reducing environmental pollution.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118957264A_ABST
    Figure CN118957264A_ABST
Patent Text Reader

Abstract

The invention relates to the technical field of anode slime treatment, and discloses a method for removing antimony and tellurium in anode slime in a multi-section pressurization chlorine-free mode, which comprises the following steps: S1, anode slime pretreatment, S2, multi-section pressurization type treatment, S3, separation of antimony and tellurium from anode slime, S4, preparation of sodium antimonate, S5, tail gas treatment, S6, waste liquid treatment, and S7, post-treatment. Through the process design of first-stage pressurization thiourea transformation deep copper removal and second-stage pressurization vulcanization chlorine-free antimony and tellurium removal, chlorine-containing substances do not participate in the whole process flow, alkaline medium pressurization leaching is adopted, substances with high corrosivity are not generated, and damage to equipment is reduced; in the process of removing antimony and tellurium metal, waste gas and waste liquid treatment can be carried out on harmful substances generated in the reaction process, by-products, precipitates, heavy metal ions which are not completely removed, micropollutants and the like in tail liquid are removed, or the tail liquid is converted into harmless substances, so that the tail liquid reaches the emission standard, and the pollution of tail liquid emission to the environment is reduced.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the technical field of anode mud treatment, in particular to a multi-stage pressurized chlorine-free method for removing antimony and tellurium from anode mud. Background Art

[0002] Anode mud is the muddy fine-grained material that falls to the bottom of the electrolytic cell during electrolytic refining. It is mainly composed of impurities in the anode crude metal that are insoluble in the electrolyte and the metal to be refined. It often contains precious and valuable metals and can be recycled as a raw material for refining precious metals such as gold and silver.

[0003] After searching, the patent with application number CN201410221865.0 discloses a fully wet pretreatment method for copper anode mud. The present invention firstly performs hot acid leaching on the copper anode mud, and leaches metals such as copper, selenium, silver, and barium into the liquid, and leaves gold, tellurium, tin, platinum and platinum group metals in the leached slag; the hot acid leaching slag is leached and enriched in the liquid by alkaline leaching, and the obtained tellurium separation slag is then subjected to chlorination gold separation, and gold, platinum and platinum group metals are enriched in the liquid, and tin and antimony are enriched in the slag; the hot acid leaching liquid is diluted with water, copper and selenium are enriched in the diluted liquid, and the obtained precipitate is then dissolved by nitric acid, and filtered to obtain barium sulfate slag and silver nitrate solution. The invention eliminates the high energy consumption and pollution-intensive sulfuric acid roasting process in the traditional copper anode mud treatment method, and removes barium before extracting gold and silver through hot acid leaching and open circuit recovery, thereby reducing the amount of copper anode mud to be treated and improving the recovery rate of gold and silver.

[0004] Among the current methods for removing rare and precious metals from anode mud, acid chlorination is mostly used to remove antimony. The high-chloride salt waste liquid generated during the reaction is highly corrosive to the equipment, and after removing precious metals such as antimony and tellurium, it is not convenient to harmlessly treat the harmful substances (waste gas and waste liquid) generated during the reaction or treatment process. If they are discharged directly, they will affect the environment. Therefore, we need to propose a multi-stage pressurized chlorine-free method for removing antimony and tellurium from anode mud. Summary of the invention

[0005] The object of the present invention is to provide a method for removing antimony and tellurium from anode mud by multi-stage pressurization without chlorine. The method adopts a process design of one-stage pressurized thiourea transformation for deep copper removal and two-stage pressurized sulfidation for chlorine-free antimony and tellurium removal. The whole process is free of chlorine-containing substances, and alkaline medium is used for pressurized leaching, so that no highly corrosive substances are produced, thereby reducing damage to equipment. In the process of removing antimony and tellurium metals, the harmful substances produced during the reaction can be treated for waste gas and waste liquid, and by-products, precipitates, heavy metal ions that are not completely removed, trace pollutants, etc. in the tail liquid can be removed, or converted into harmless substances, so that the tail liquid meets the discharge standard, and the pollution of the tail liquid discharge to the environment is reduced, so as to solve the problems raised in the above-mentioned background technology.

[0006] To achieve the above object, the present invention provides the following technical solution: a multi-stage pressurized chlorine-free method for removing antimony and tellurium from anode mud, comprising the following steps:

[0007] S1. Anode mud pretreatment: remove impurities and moisture in anode mud by drying, crushing and screening to facilitate subsequent processing;

[0008] S2, multi-stage pressurized treatment: one stage of pressurized thiourea transformation for deep copper removal, and two stage of pressurized sulfidation without chlorine for antimony and tellurium removal;

[0009] S3, using separation technology to separate antimony and tellurium from anode mud and recover other valuable metal components;

[0010] S4, after leaching antimony and tellurium and reducing tellurium, sodium antimonate is prepared from the tail liquid formed, and the remaining solution is waste liquid;

[0011] S5. Tail gas treatment: In the process of the above chemical reaction and material treatment, unreacted gas, volatile organic matter, and acidic or alkaline gas will be generated. The above gas will be collected and then introduced into the exhaust gas treatment device for purification;

[0012] S6. Waste liquid treatment: In chemical reactions and material processing, incompletely reacted raw materials, reaction by-products, dissolved metal ions and impurities are treated to remove trace pollutants in the waste liquid;

[0013] S7. The separated antimony, tellurium and other metals are further post-processed to achieve the required purity and form of antimony and tellurium.

[0014] Preferably, in step S1, the anode mud is crushed into small particles or powder, which can increase the surface area of ​​the anode mud, make the chemical reaction and physical reaction in the subsequent treatment more efficient, and expose the impurities and metal elements inside the anode mud, which is convenient for subsequent extraction and separation;

[0015] The anode mud is then screened according to its particle size to ensure the particle size range of the anode mud and improve the uniformity and consistency of subsequent processing steps.

[0016] Preferably, in step S2, the process of one-stage pressurized thiourea transformation deep copper removal is: using a copper electrolyte supplemented with 30,000ths by weight of thiourea auxiliary agent, performing one-stage pressurized transformation leaching on the thickener copper-nickel anode mud, selectively removing copper and removing part of tellurium, separating tellurium from the leachate after the one-stage pressurized transformation leaching and entering the copper electrolysis production system, and sending the slag after the one-stage pressurized transformation leaching to the two-stage pressurized sulfidation leaching;

[0017] The process of two-stage pressure sulfidation chlorine-free removal of antimony and tellurium is as follows: the slag after the first-stage pressure transformation leaching is subjected to sulfidation leaching under alkaline conditions to selectively leach antimony and tellurium; the slag after the second-stage pressure sulfidation leaching is used as high-quality raw material for extracting rare and precious metals; the leachate after the second-stage pressure sulfidation leaching is selectively reduced to crude tellurium powder through acidic gas sulfur dioxide flue gas, and the tail liquid after reduction is used to prepare sodium antimonate.

[0018] Preferably, in step S3, antimony and tellurium are separated by precipitation and filtration, by adding a precipitant to the leaching solution and controlling the pH value and temperature conditions of the leaching solution, so that antimony and tellurium are precipitated from the solution in the form of a precipitate, and then the precipitate of antimony and tellurium is separated from the leaching solution by a filter press or a vacuum filter, and the filtration operation is repeated multiple times to fully filter out antimony and tellurium;

[0019] For the recovery of other valuable metal components: the leachate after filtering out antimony and tellurium is treated by distillation to separate the volatile metal components, and then the leachate is heated to convert the volatile metal components into steam, which is then collected by condensation to achieve the separation of the metal components.

[0020] Preferably, in step S4, sodium nitrate is added to the tail liquid purified in step S3, and the sodium nitrate reacts with the antimony ions in the tail liquid to generate insoluble antimonate. After the antimonate is completely precipitated, the antimonate is collected by filtering, and the collected antimonate is washed to remove impurities attached to the surface, and then dried. Finally, the dried antimonate is reacted with a sodium hydroxide solution or a sodium carbonate solution to generate sodium antimonate, and the sodium antimonate is separated from the solution by filtering.

[0021] Preferably, in step S5, the tail gas treatment method may be any one of chemical adsorption, physical adsorption or catalytic conversion, wherein:

[0022] Chemical adsorption: The harmful substances in the exhaust gas react chemically with the absorbent and are converted into harmless gas;

[0023] Physical adsorption: using adsorbents to adsorb harmful substances in the tail gas and separate them from the tail gas;

[0024] Catalytic conversion: Harmful substances in exhaust gas undergo chemical reactions at low temperatures through the use of catalysts and are converted into harmless substances.

[0025] Preferably, in step S6, the treatment of the tail liquid after the preparation of sodium antimonate includes the following process:

[0026] Pretreatment: Remove suspended matter, by-products and precipitated matter from the tail liquid through a screen;

[0027] Main treatment: using activated carbon or ion exchange resin to absorb the antimony and tellurium heavy metal ions in the waste liquid;

[0028] Advanced treatment: Use oxidation or biological treatment to further remove trace pollutants in wastewater.

[0029] Preferably, in step S7, the post-processing process includes:

[0030] Purification: The separated antimony, tellurium and other metals are purified by electrolysis or refining to remove residual impurities and improve the purity of the metals;

[0031] Form adjustment: converting the purified metal into powder, granules or blocks;

[0032] Quality control: Accurately determine the purity and composition of metals through chemical analysis and spectral analysis.

[0033] Compared with the prior art, the present invention has the following beneficial effects:

[0034] The present invention adopts a process design of one-stage pressurized thiourea transformation for deep copper removal and two-stage pressurized sulfidation for chlorine-free antimony and tellurium removal. The whole process is free of chlorine-containing substances, and alkaline medium pressure leaching is adopted, so that no highly corrosive substances are generated, thereby reducing damage to equipment. In addition, in the process of removing antimony and tellurium metals, waste gas and waste liquid treatment can be performed on harmful substances generated during the reaction, and by-products, precipitates, heavy metal ions that are not completely removed, trace pollutants, etc. in the tail liquid can be removed or converted into harmless substances, so that the tail liquid meets the emission standards and the pollution of the tail liquid emission to the environment is reduced. BRIEF DESCRIPTION OF THE DRAWINGS

[0035] Figure 1 It is a flowchart of the present invention;

[0036] Figure 2 It is a flow chart of the present invention. DETAILED DESCRIPTION

[0037] The following will be combined with the drawings in the embodiments of the present invention to clearly and completely describe the technical solutions in the embodiments of the present invention. Obviously, the described embodiments are only part of the embodiments of the present invention, not all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.

[0038] Example 1

[0039] See also Figure 1-2 The present invention provides a technical solution: a multi-stage pressurized chlorine-free method for removing antimony and tellurium from anode mud, comprising the following steps:

[0040] S1. Anode mud pretreatment: remove impurities and moisture in anode mud by drying, crushing and screening to facilitate subsequent processing;

[0041] In step S1, the anode mud is crushed into small particles or powders, which can increase the surface area of ​​the anode mud, making the chemical reaction and physical reaction in the subsequent treatment more efficient, and can also destroy the anode mud agglomerates, and expose the impurities and metal elements inside the anode mud, which is convenient for subsequent extraction and separation;

[0042] Then the anode mud is screened according to the particle size to ensure the particle size range of the anode mud and improve the uniformity and consistency of the subsequent processing steps. Screening can also preliminarily separate the impurities and metal elements in the anode mud according to the particle size, laying the foundation for subsequent finer separation.

[0043] S2, multi-stage pressurized treatment: one stage of pressurized thiourea transformation for deep copper removal, and two stage of pressurized sulfidation without chlorine for antimony and tellurium removal;

[0044] In step S2, the process of one-stage pressurized thiourea transformation deep copper removal is as follows: using a copper electrolyte supplemented with 30,000ths by weight of thiourea auxiliary agent, a one-stage pressurized transformation leaching is performed on the thickener copper-nickel anode mud to selectively remove copper and part of tellurium, and the leachate after the one-stage pressurized transformation leaching is separated from tellurium and enters the copper electrolysis production system, and the slag after the one-stage pressurized transformation leaching is sent to the two-stage pressurized sulfidation leaching;

[0045] In the process of deep copper removal by pressurized thiourea transformation, the optimal leaching parameters are: temperature 60°C, reaction time 60 minutes, and thiourea weight ratio 3 / 10,000.

[0046] At this stage, copper electrolyte was used and supplemented with 3 parts by weight of thiourea as an auxiliary agent. The addition of thiourea helps to promote copper leaching and assists in the removal of some tellurium. The thickener copper-nickel anode mud was subjected to pressure leaching in this electrolyte to achieve selective removal of copper and some tellurium.

[0047] The process of two-stage pressure sulfidation chlorine-free removal of antimony and tellurium is as follows: the slag after the first-stage pressure transformation leaching is subjected to sulfidation leaching under alkaline conditions to selectively leach antimony and tellurium; the slag after the second-stage pressure sulfidation leaching (i.e., sulfided slag, rich in rare and precious metals) is used as high-quality raw material for extracting rare and precious metals; the leachate after the second-stage pressure sulfidation leaching is selectively reduced to crude tellurium powder through acidic gas sulfur dioxide flue gas, and the tail liquid after reduction is used to prepare sodium antimonate.

[0048] In the two-stage pressure sulfidation chlorine-free removal of antimony and tellurium process, the optimal leaching parameters are: temperature 60°C, reaction time 30 minutes, the amount of sulfiding agent used is 1.1 times the amount of antimony and tellurium leaching, and the liquid-to-solid ratio is 3:1.

[0049] As an effective chelating agent, thiourea can react with copper ions under pressurized conditions. Thiourea combines with copper ions to form a stable complex, which reduces the solubility of copper in anode mud and thus achieves copper separation.

[0050] The goal of the two-stage pressure sulfidation chlorine-free removal of antimony and tellurium is to remove antimony and tellurium from anode mud. Sulfidation reaction is selected as the chlorine-free removal method to avoid the generation of harmful chloride emissions.

[0051] Under pressure, the sulfiding agent is introduced to react with the antimony and tellurium in the anode mud to form corresponding sulfides. No chlorine-containing compounds are used in the whole process, thus avoiding the generation and emission of chlorides, which meets environmental protection requirements.

[0052] Table 1 Composition of anode mud in one-stage pressure decoppering (%)

[0053]

[0054] Table 2 Composition of anode mud in the second stage of pressure decoppering (%)

[0055]

[0056] In step S2, the first-stage pressurized copper removal rate is greater than 98.1%; the second-stage pressurized antimony removal rate is greater than 96.3%; the second-stage pressurized tellurium removal rate is greater than 91.2%, the tellurium reduction rate is greater than 99.0%, and the crude tellurium powder grade is greater than 98.5%; the entire process can achieve the goal of not introducing chloride ions, high sulfidation pressurized leaching rate, thorough separation, and high crude tellurium grade, which is beneficial to the next step of refining.

[0057] S3, using separation technology to separate antimony and tellurium from anode mud and recover other valuable metal components;

[0058] In step S3, antimony and tellurium are separated by precipitation and filtration. A precipitant is added to the leaching solution, and the pH value and temperature of the leaching solution are controlled so that antimony and tellurium are precipitated from the solution in the form of a precipitate. The precipitate of antimony and tellurium is then separated from the leaching solution by a filter press or a vacuum filter. The filtration operation is repeated multiple times to fully filter out antimony and tellurium, thereby improving the purity of antimony and tellurium.

[0059] For the recovery of other valuable metal components: the leachate after filtering out antimony and tellurium is treated by distillation to separate the volatile metal components, and then the leachate is heated to convert the volatile metal components into steam, which is then collected by condensation to achieve the separation of the metal components.

[0060] The resulting antimony and tellurium compounds require further refining to remove remaining impurities.

[0061] S4, after leaching antimony and tellurium and reducing tellurium, sodium antimonate is prepared from the tail liquid formed, and the remaining solution is waste liquid;

[0062] In step S4, sodium nitrate is added to the tail liquid purified in step S3, and the sodium nitrate reacts with the antimony ions in the tail liquid to generate insoluble antimonate. After the antimonate is completely precipitated, the antimonate is collected by filtering, and the collected antimonate is washed to remove impurities attached to the surface, and then dried. Finally, the dried antimonate is reacted with a sodium hydroxide solution or a sodium carbonate solution to generate sodium antimonate, and the sodium antimonate is separated from the solution by filtering.

[0063] In the process of the reaction of sodium nitrate with antimony ions, and the reaction of antimonate with sodium hydroxide solution or sodium carbonate solution, sufficient stirring is required to promote the rapid generation of antimonate by sodium nitrate and antimony ions, and to promote the rapid generation of sodium antimonate by antimonate and alkali solution.

[0064] S5. Tail gas treatment: In the process of the above chemical reaction and material treatment, unreacted gas, volatile organic matter, and acidic or alkaline gas will be generated. The above gas will be collected and then introduced into the exhaust gas treatment device for purification;

[0065] In step S5, the tail gas treatment method may be any one of chemical adsorption, physical adsorption or catalytic conversion, wherein:

[0066] Chemical adsorption: The harmful substances in the exhaust gas react chemically with the absorbent and are converted into harmless gas;

[0067] Physical adsorption: using adsorbents to adsorb harmful substances in the tail gas and separate them from the tail gas;

[0068] Catalytic conversion: Harmful substances in exhaust gas undergo chemical reactions at low temperatures through the use of catalysts and are converted into harmless substances.

[0069] S6. Waste liquid treatment: In chemical reactions and material processing, incompletely reacted raw materials, reaction by-products, dissolved metal ions and impurities are treated to remove trace pollutants in the waste liquid;

[0070] In step S6, the tail liquid treatment after the preparation of sodium antimonate includes the following process:

[0071] Pretreatment: Remove suspended matter, by-products and precipitated matter from the tail liquid through a screen;

[0072] Main treatment: using activated carbon or ion exchange resin to absorb the antimony and tellurium heavy metal ions in the waste liquid;

[0073] Advanced treatment: Use oxidation or biological treatment to further remove trace pollutants in wastewater.

[0074] S7. The separated antimony, tellurium and other metals are further post-processed to achieve the required purity and form of antimony and tellurium.

[0075] In step S7, the post-processing process includes:

[0076] Purification: The separated antimony, tellurium and other metals are purified by electrolysis or refining to remove residual impurities and improve the purity of the metals;

[0077] Form adjustment: converting the purified metal into powder, granules or blocks;

[0078] Quality control: Accurately determine the purity and composition of metals through chemical analysis and spectral analysis.

[0079] Example 2

[0080] The same as Example 1 is not repeated here, except that

[0081] S2, multi-stage pressurized treatment: one stage of pressurized thiourea transformation for deep copper removal, and two stage of pressurized sulfidation without chlorine for antimony and tellurium removal;

[0082] In step S2, the process of one-stage pressurized thiourea transformation deep copper removal is as follows: using a copper electrolyte supplemented with 30,000ths by weight of thiourea auxiliary agent, a one-stage pressurized transformation leaching is performed on the thickener copper-nickel anode mud to selectively remove copper and part of tellurium, and the leachate after the one-stage pressurized transformation leaching is separated from tellurium and enters the copper electrolysis production system, and the slag after the one-stage pressurized transformation leaching is sent to the two-stage pressurized sulfidation leaching;

[0083] In the process of deep copper removal by pressurized thiourea transformation, the optimal leaching parameters are: temperature 90°C, reaction time 90 minutes, and thiourea weight ratio 3 / 10,000.

[0084] At this stage, copper electrolyte was used and supplemented with 3 parts by weight of thiourea as an auxiliary agent. The addition of thiourea helps to promote copper leaching and assists in the removal of some tellurium. The thickener copper-nickel anode mud was subjected to pressure leaching in this electrolyte to achieve selective removal of copper and some tellurium.

[0085] The process of two-stage pressure sulfidation chlorine-free removal of antimony and tellurium is as follows: the slag after the first-stage pressure transformation leaching is subjected to sulfidation leaching under alkaline conditions to selectively leach antimony and tellurium; the slag after the second-stage pressure sulfidation leaching (i.e., sulfided slag, rich in rare and precious metals) is used as high-quality raw material for extracting rare and precious metals; the leachate after the second-stage pressure sulfidation leaching is selectively reduced to crude tellurium powder through acidic gas sulfur dioxide flue gas, and the tail liquid after reduction is used to prepare sodium antimonate.

[0086] In the two-stage pressure sulfidation chlorine-free removal of antimony and tellurium process, the optimal leaching parameters are: temperature 90°C, reaction time 75 minutes, the amount of sulfiding agent used is 1.2 times the amount of antimony and tellurium leaching, and the liquid-to-solid ratio is 4:1.

[0087] As an effective chelating agent, thiourea can react with copper ions under pressurized conditions. Thiourea combines with copper ions to form a stable complex, which reduces the solubility of copper in anode mud and thus achieves copper separation.

[0088] The goal of the two-stage pressure sulfidation chlorine-free removal of antimony and tellurium is to remove antimony and tellurium from anode mud. Sulfidation reaction is selected as the chlorine-free removal method to avoid the generation of harmful chloride emissions.

[0089] Under pressure, the sulfiding agent is introduced to react with the antimony and tellurium in the anode mud to form corresponding sulfides. No chlorine-containing compounds are used in the whole process, thus avoiding the generation and emission of chlorides, which meets environmental protection requirements.

[0090] Table 3 Composition of anode mud in one-stage pressure decoppering (%)

[0091]

[0092] Table 4 Composition of anode mud in the second stage of pressure decoppering (%)

[0093]

[0094] In step S2, the first-stage pressurized copper removal rate is greater than 98.3%; the second-stage pressurized antimony removal rate is greater than 96.5%; the second-stage pressurized tellurium removal rate is greater than 91.4%, the tellurium reduction rate is greater than 99.3%, and the crude tellurium powder grade is greater than 98.7%; the entire process can achieve no introduction of chloride ions, high sulfidation pressure leaching rate, thorough separation, and high crude tellurium grade, which is conducive to the next step of refining.

[0095] Example 3

[0096] The same points as in Example 1 and Example 2 are not repeated here, except that

[0097] S2, multi-stage pressurized treatment: one stage of pressurized thiourea transformation for deep copper removal, and two stage of pressurized sulfidation without chlorine for antimony and tellurium removal;

[0098] In step S2, the process of one-stage pressurized thiourea transformation deep copper removal is as follows: using a copper electrolyte supplemented with 30,000ths by weight of thiourea auxiliary agent, a one-stage pressurized transformation leaching is performed on the thickener copper-nickel anode mud to selectively remove copper and part of tellurium, and the leachate after the one-stage pressurized transformation leaching is separated from tellurium and enters the copper electrolysis production system, and the slag after the one-stage pressurized transformation leaching is sent to the two-stage pressurized sulfidation leaching;

[0099] In the process of deep copper removal by pressurized thiourea transformation, the optimal leaching parameters are: temperature 120°C, reaction time 120 minutes, and thiourea weight ratio 3 / 10,000.

[0100] At this stage, copper electrolyte was used and supplemented with 3 parts by weight of thiourea as an auxiliary agent. The addition of thiourea helps to promote copper leaching and assists in the removal of some tellurium. The thickener copper-nickel anode mud was subjected to pressure leaching in this electrolyte to achieve selective removal of copper and some tellurium.

[0101] The process of two-stage pressure sulfidation chlorine-free removal of antimony and tellurium is as follows: the slag after the first-stage pressure transformation leaching is subjected to sulfidation leaching under alkaline conditions to selectively leach antimony and tellurium; the slag after the second-stage pressure sulfidation leaching (i.e., sulfided slag, rich in rare and precious metals) is used as high-quality raw material for extracting rare and precious metals; the leachate after the second-stage pressure sulfidation leaching is selectively reduced to crude tellurium powder through acidic gas sulfur dioxide flue gas, and the tail liquid after reduction is used to prepare sodium antimonate.

[0102] In the two-stage pressure sulfidation chlorine-free removal of antimony and tellurium process, the optimal leaching parameters are: temperature 120°C, reaction time 120 minutes, the amount of sulfiding agent used is 1.3 times the amount of antimony and tellurium leaching, and the liquid-to-solid ratio is 5:1.

[0103] As an effective chelating agent, thiourea can react with copper ions under pressurized conditions. Thiourea combines with copper ions to form a stable complex, which reduces the solubility of copper in anode mud and thus achieves copper separation.

[0104] The goal of the two-stage pressure sulfidation chlorine-free removal of antimony and tellurium is to remove antimony and tellurium from anode mud. Sulfidation reaction is selected as the chlorine-free removal method to avoid the generation of harmful chloride emissions.

[0105] Under pressure, the sulfiding agent is introduced to react with the antimony and tellurium in the anode mud to form corresponding sulfides. No chlorine-containing compounds are used in the whole process, thus avoiding the generation and emission of chlorides, which meets environmental protection requirements.

[0106] Table 5 Composition of anode mud in one-stage pressure decoppering (%)

[0107]

[0108]

[0109] Table 6 Composition of anode mud in the second stage of pressure decoppering (%)

[0110]

[0111] In step S2, the first-stage pressurized copper removal rate is greater than 98.4%; the second-stage pressurized antimony removal rate is greater than 96.7%; the second-stage pressurized tellurium removal rate is greater than 91.5%, the tellurium reduction rate is greater than 99.4%, and the crude tellurium powder grade is greater than 98.8%; the entire process can achieve no introduction of chloride ions, high sulfidation pressure leaching rate, thorough separation, and high crude tellurium grade, which is conducive to the next step of refining.

[0112] Although embodiments of the present invention have been shown and described, it will be appreciated by those skilled in the art that various changes, modifications, substitutions and variations may be made to the embodiments without departing from the principles and spirit of the present invention, and that the scope of the present invention is defined by the appended claims and their equivalents.

Claims

1. A multi-stage pressurized chlorine-free method for removing antimony and tellurium from anode mud, characterized by: The following steps are involved: S1. Anode mud pretreatment: Drying, crushing and screening are used to remove impurities and moisture from the anode mud to facilitate subsequent processing; S2, multi-stage pressurized treatment: using a first stage of pressurized thiourea transformation to remove copper deeply, and a second stage of pressurized sulfidation without chlorine to remove antimony and tellurium; S3. Use separation technology to separate antimony and tellurium from anode mud and recover other valuable metal components; S4. After leaching antimony and tellurium and reducing tellurium, sodium antimonate is prepared from the resulting tail liquid, and the remaining solution is waste liquid; S5. Tail gas treatment: In the process of the above chemical reaction and material treatment, unreacted gases, volatile organic compounds, and acidic or alkaline gases are generated. These gases are collected and then introduced into the exhaust gas treatment device for purification; S6. Waste liquid treatment: In chemical reactions and material processing, incompletely reacted raw materials, reaction by-products, dissolved metal ions and impurities are treated to remove trace pollutants in the waste liquid; S7. The separated antimony, tellurium and other metals are further post-processed to achieve the required purity and form of antimony and tellurium.

2. The method for removing antimony and tellurium from anode mud by multi-stage pressurization and chlorine-free method according to claim 1, characterized in that: In step S1, the anode mud is crushed into small particles or powder, which can increase the surface area of ​​the anode mud, making the chemical and physical reactions in subsequent processing more efficient, and exposing the impurities and metal elements inside the anode mud, facilitating subsequent extraction and separation; The anode mud is then screened according to its particle size to ensure the particle size range of the anode mud and improve the uniformity and consistency of subsequent processing steps.

3. The multi-stage pressurized chlorine-free removal method for antimony and tellurium in anode mud according to claim 1, characterized in that: In step S2, the process of the one-stage pressurized thiourea transition deep copper removal is as follows: using a copper electrolyte supplemented with 0.03% by weight of thiourea as an auxiliary agent, the thickener copper-de-nickel anode mud is subjected to a one-stage pressurized transition leaching to selectively remove copper and partially remove tellurium. After the tellurium is separated from the leachate after the one-stage pressurized transition leaching, the leachate enters the copper electrolysis production system. The residue after the one-stage pressurized transition leaching is sent to the second-stage pressurized sulfidation leaching. The process of two-stage pressure sulfidation chlorine-free removal of antimony and tellurium is as follows: the residue after the first-stage pressure transformation leaching is subjected to sulfidation leaching under alkaline conditions to selectively leach antimony and tellurium. The residue after the second-stage pressure sulfidation leaching is used as high-quality raw material for extracting rare and precious metals. The leachate after the second-stage pressure sulfidation leaching is selectively reduced to crude tellurium powder through acidic gas sulfur dioxide flue gas, and the tail liquid after reduction is used to prepare sodium antimonate.

4. The multi-stage pressurized chlorine-free removal method for antimony and tellurium in anode mud according to claim 1, characterized in that: In step S3, antimony and tellurium are separated by precipitation and filtration. A precipitant is added to the leachate, and the pH and temperature of the leachate are controlled to allow antimony and tellurium to precipitate from the solution. The precipitate of antimony and tellurium is then separated from the leachate by a filter press or a vacuum filter. The filtration operation is repeated multiple times to fully filter out the antimony and tellurium. For the recovery of other valuable metal components: the leachate after filtering out antimony and tellurium is treated by distillation to separate the volatile metal components, and then the leachate is heated to convert the volatile metal components into steam, which is then collected by condensation to achieve the separation of the metal components.

5. The multi-stage pressurized chlorine-free removal method for antimony and tellurium in anode mud according to claim 1, characterized in that: In step S4, sodium nitrate is added to the tail liquid purified in step S3. The sodium nitrate reacts with the antimony ions in the tail liquid to generate insoluble antimonate. After the antimonate is completely precipitated, the antimonate is collected by filtration, and the collected antimonate is washed to remove impurities attached to the surface. The antimonate is then dried, and finally the dried antimonate is reacted with a sodium hydroxide solution or a sodium carbonate solution to generate sodium antimonate, which is then separated from the solution by filtration.

6. The multi-stage pressurized chlorine-free removal method for antimony and tellurium in anode mud according to claim 1, characterized in that: In step S5, the tail gas treatment method can be any one of chemical adsorption, physical adsorption or catalytic conversion, wherein: Chemical adsorption: The harmful substances in the exhaust gas react chemically with the absorbent and are converted into harmless gases; Physical adsorption: using adsorbents to adsorb harmful substances in the tail gas and separate them from the tail gas; Catalytic conversion: Harmful substances in exhaust gas undergo chemical reactions at low temperatures through catalysts and are converted into harmless substances.

7. The multi-stage pressurized chlorine-free removal method for antimony and tellurium from anode mud according to claim 1, characterized in that: In step S6, the tail liquid treatment after the preparation of sodium antimonate includes the following process: Pretreatment: Remove suspended matter, by-products and sediment in the tail liquid through a screen; Main treatment: using activated carbon or ion exchange resin to absorb antimony and tellurium heavy metal ions in wastewater; Advanced treatment: Oxidation or biological treatment is used to further remove trace pollutants in wastewater.

8. The multi-stage pressurized chlorine-free method for removing antimony and tellurium from anode mud according to claim 1, characterized in that: In step S7, the post-processing process includes: Purification: The separated antimony, tellurium and other metals are purified by electrolysis or refining to remove residual impurities and improve the purity of the metals; Form adjustment: converting the purified metal into powder, granules or blocks; Quality control: Accurately determine the purity and composition of metals through chemical analysis and spectral analysis.

Citation Information

Patent Citations

  • Method for selectively extracting gold and silver from copper anode slime

    CN103320624A

  • Comprehensive utilization method of copper electrolyte purification resources

    CN110669932A

  • Method for comprehensively recovering tellurium slag

    CN117107061A

  • Electrorefining method of low-grade copper anode, and electrolytic solution used therefor

    JP2019052329A

  • Hydrometallurgical process for the recovery of tellurium from high lead bearing copper refinery anode slime

    US20150053572A1