Method for recovering valuable metal in welding rod after aerobic pyrolysis of waste crystalline silicon photovoltaic module

By employing a high-temperature chlorination reaction and a three-stage cooling crystallization process, the problem of recovering valuable metals from waste crystalline silicon photovoltaic module welding electrodes has been solved. This process achieves efficient separation and purification of copper, lead, and tin, provides high-purity copper raw materials, and improves the recovery efficiency of valuable metals.

CN118957275APending Publication Date: 2024-11-15SUZHOU XIRE ENERGY SAVING ENVIRONMENTAL PROTECTION TECH CO LTD
View PDF 0 Cites 3 Cited by

Patent Information

Application Number
CN202411250455.9
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-09-06
Publication Date
2024-11-15

AI Technical Summary

Technical Problem

Valuable metals in the welding rods of waste crystalline silicon photovoltaic modules are difficult to effectively recycle after aerobic pyrolysis, mainly because the welding rods are oxidized during high-temperature pyrolysis, resulting in complex composition, which is difficult to effectively separate and recycle with existing technologies.

Method used

A high-temperature chlorination reaction combined with a three-stage cooling crystallization process is adopted. After crushing the welding rod, copper chloride powder is added to carry out a high-temperature chlorination reaction. By utilizing the difference in volatilization temperature of metal chlorides, copper, lead and tin can be separated in a precise manner, thereby reducing the lead and tin content in copper.

Benefits of technology

It achieves efficient separation and purification of copper, lead, and tin in welding electrodes, reducing the lead and tin content in copper products to below 0.5%, providing high-quality copper raw materials, laying the foundation for subsequent deep processing, and improving the recycling value of valuable metals.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118957275A_ABST
    Figure CN118957275A_ABST
Patent Text Reader

Abstract

The invention discloses a method for recovering valuable metals in welding rods after aerobic pyrolysis of waste crystalline silicon photovoltaic modules, which belongs to the technical field of resource utilization of waste photovoltaic modules and comprises the following steps: (1) physically refining the welding rods; (2) adding copper chloride mixed materials; (3) performing pressure-controlled high-temperature chlorination treatment; (4) carrying out three-section step-by-step cooling separation on volatile flue gas; and (5) naturally cooling and recovering copper metal. Aiming at the characteristics of complex composition and various components of the welding rod under the aerobic pyrolysis condition, according to the physicochemical characteristics of copper, lead and tin metal chlorides, the high-temperature chlorination and step-by-step cooling processes are adopted, so that the precise and deep separation of valuable metal substances in the flue gas is realized, the purification of copper metal is also realized, and the production efficiency is improved. And the contents of lead and tin impurities in the final copper product can be respectively reduced to below 0.5%. The problem that aerobic pyrolysis welding rods are difficult to separate, purify and recycle is solved, and cyclic utilization of copper, lead and tin metal is achieved.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention belongs to the technical field of resource utilization of waste photovoltaic modules, and specifically relates to a method for recovering valuable metals in welding rods after aerobic pyrolysis of waste crystalline silicon photovoltaic modules. Background Art

[0002] With the rapid development of the photovoltaic industry, the use of crystalline silicon photovoltaic panels has increased rapidly. The service life of crystalline silicon photovoltaic cells is about 25 years. Waste photovoltaic modules contain glass, aluminum metal frames, silicon, silver, copper, lead, tin, etc. How to recycle valuable resources in waste crystalline silicon photovoltaic modules has become an important research direction.

[0003] The recycling of waste photovoltaic modules requires the disassembly of each module. Currently, the aluminum metal frame can be automatically disassembled and recycled, and the technology is relatively mature; the remaining part is mainly a laminate composed of glass, battery cells, backplanes, EVA films, solder strips, etc. The separation of this part is a very critical step in module recycling technology. At present, the main methods for separating and recycling the laminate are physical sorting, high-temperature pyrolysis, and chemical dissolution. Among them, the high-temperature pyrolysis method has the advantages of simple operation, no use of chemical agents, no waste liquid generation, and easy scale-up. Some companies have completed pilot experiments and are expected to be industrialized in the future.

[0004] After high-temperature pyrolysis of photovoltaic modules in an air atmosphere, the film decomposes and loses its adhesiveness, and each component can be separated after physical sorting. In photovoltaic modules, welding rods are mainly based on copper, and the copper content is generally higher than 80% (wt%). The surface is coated with low-melting-point lead and tin metals, located on the surface of the battery cell, and used for connecting between battery cells, playing an important role in conducting electricity. However, during the high-temperature pyrolysis process, the welding rod is prone to oxidation due to the influence of oxygen. Therefore, after aerobic pyrolysis, the composition of the welding rod becomes complex, consisting of metal oxides (copper oxide, lead oxide, tin oxide, stannous oxide) and metal elements (copper, lead, tin), which undoubtedly increases the difficulty of recycling the welding rod. Therefore, in view of the complex composition of pyrolysis welding rods, it is urgent to develop targeted and efficient recycling methods. Summary of the invention

[0005] In order to overcome the shortcomings of the above-mentioned prior art, the purpose of the present invention is to provide a method for recovering valuable metals in welding rods after aerobic pyrolysis of waste crystalline silicon photovoltaic modules, so as to solve the technical problem that valuable metals in welding rods after air pyrolysis of waste crystalline silicon photovoltaic modules are difficult to recycle.

[0006] In order to achieve the above object, the present invention adopts the following technical solutions:

[0007] The invention discloses a method for recovering valuable metals in welding rods after aerobic pyrolysis of waste crystalline silicon photovoltaic modules, comprising: crushing the welding rods after aerobic pyrolysis of waste crystalline silicon photovoltaic modules, then adding copper chloride powder, fully mixing, carrying out chlorination reaction, and obtaining copper with low lead and tin content after three-stage cooling and crystallization.

[0008] Preferably, the particle size of the pulverized welding rod is 0.1-30 mm; and the particle size of the copper chloride powder is less than 100 μm.

[0009] Preferably, the amount of cupric chloride powder added is 3%-15% of the mass of the welding rod; and the mixing time is 10-90 minutes.

[0010] Preferably, the temperature of the chlorination reaction is 1000-1200°C.

[0011] Preferably, the chlorination reaction time is 1-10 h.

[0012] Preferably, the protective atmosphere of the chlorination reaction is chlorine gas with a pressure of 0.1-0.5 atm.

[0013] Preferably, in the three-stage cooling crystallization, the temperature of the first stage cooling is 680-880° C.; after the first stage cooling, a mixture of copper chloride and lead chloride is obtained, and the copper chloride and lead chloride are separated by water leaching.

[0014] Preferably, in the three-stage cooling crystallization, the second stage cooling temperature is 200-400° C.; after the second stage cooling, solid tin dichloride is obtained.

[0015] Preferably, in the three-stage cooling crystallization, the temperature of the third stage cooling is 20-60° C.; after the third stage cooling, tin tetrachloride liquid is obtained, and the excess chlorine is returned to the chlorination reaction for recycling.

[0016] Preferably, in the copper with low lead-tin content, the mass percentage of lead is reduced to below 0.5%, and the mass percentage of tin is reduced to below 0.5%.

[0017] Compared with the prior art, the present invention has the following beneficial effects:

[0018] The present invention discloses a method for recovering valuable metals in welding rods after aerobic pyrolysis of waste crystalline silicon photovoltaic modules. Aiming at the problem that the welding rods of waste crystalline silicon photovoltaic modules under aerobic pyrolysis conditions have complex structures and various components, and valuable metals in welding rods are difficult to recycle after air pyrolysis, an innovative method for separating impurities with high efficiency is proposed. After the aerobic pyrolysis welding rods are crushed and treated with high-temperature chlorination reaction, the basic idea of ​​high-temperature chlorination-three-stage cooling is proposed according to the physical and chemical properties of each metal chloride therein, and the lead and tin metals in the welding rods are separated according to the difference in the volatilization temperature of the chlorides, realizing the deep separation of copper, lead and tin substances in the flue gas, reducing the lead and tin content in copper, and also realizing the purification of metallic copper. The lead and tin content in the obtained copper can be reduced to less than 0.5%, respectively, providing high-quality materials for the subsequent deep processing of copper, and realizing the comprehensive utilization of valuable metals in welding rods. A new method is provided to improve the resource utilization of valuable metals in welding rods after aerobic pyrolysis of waste photovoltaic modules. BRIEF DESCRIPTION OF THE DRAWINGS

[0019] Figure 1 The present invention discloses a process flow chart for recovering valuable metals in welding rods after aerobic pyrolysis of waste crystalline silicon photovoltaic modules. DETAILED DESCRIPTION

[0020] In order to enable those skilled in the art to better understand the scheme of the present invention, the technical scheme in the embodiments of the present invention will be clearly and completely described below in conjunction with the drawings in the embodiments of the present invention. Obviously, the described embodiments are only part of the embodiments of the present invention, not all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work should fall within the scope of protection of the present invention.

[0021] In order to enable those skilled in the art to understand the characteristics and effects of the present invention, the following is a general description and definition of the terms and expressions mentioned in the specification and claims. Unless otherwise specified, all technical and scientific terms used in the text are the common meanings understood by those skilled in the art for the present invention. In the event of a conflict, the definition in this specification shall prevail.

[0022] It should be noted that the terms "first", "second", etc. in the specification and claims of the present invention and the above-mentioned drawings are used to distinguish similar objects, and are not necessarily used to describe a specific order or sequence. It should be understood that the data used in this way can be interchanged where appropriate, so that the embodiments of the present invention described herein can be implemented in an order other than those illustrated or described herein. In addition, the terms "including" and "having" and any variations thereof are intended to cover non-exclusive inclusions, for example, a process, method, system, product or device that includes a series of steps or units is not necessarily limited to those steps or units that are clearly listed, but may include other steps or units that are not clearly listed or inherent to these processes, methods, products or devices.

[0023] The theories or mechanisms described and disclosed herein, whether correct or incorrect, should not limit the scope of the present invention in any way, that is, the present invention can be implemented without being limited by any specific theory or mechanism.

[0024] Herein, all features such as values, quantities, contents and concentrations defined in the form of numerical ranges or percentage ranges are for simplicity and convenience only. Accordingly, the description of numerical ranges or percentage ranges should be considered to have included and specifically disclosed all possible secondary ranges and individual values ​​within the range (including integers and fractions).

[0025] In this document, unless otherwise specified, “includes,” “including,” “contains,” “has,” or similar terms cover the meanings of “consisting of” and “mainly consisting of,” for example, “A includes a” covers the meanings of “A includes a and other” and “A only includes a.”

[0026] In this document, in order to make the description concise, not all possible combinations of various technical features in various embodiments or examples are described. Therefore, as long as there is no contradiction in the combination of these technical features, the various technical features in various embodiments or examples can be combined arbitrarily, and all possible combinations should be considered to be within the scope of this specification.

[0027] The present invention will be further described below in conjunction with specific embodiments. It should be understood that these embodiments are only used to illustrate the present invention and are not intended to limit the scope of the present invention. In addition, it should be understood that after reading the content taught by the present invention, those skilled in the art can make various changes or modifications to the present invention, and these equivalent forms fall within the scope limited by the appended claims of the application equally.

[0028] The following examples use conventional instruments and equipment in the art. The experimental methods in the following examples where specific conditions are not specified are usually carried out under conventional conditions or under conditions recommended by the manufacturer. The various raw materials used in the following examples are conventional commercial products unless otherwise specified, and their specifications are conventional specifications in the art. In the specification of the present invention and the following examples, unless otherwise specified, "%" means weight percentage, "part" means weight part, and ratio means weight ratio.

[0029] The present invention is further described in detail below in conjunction with the accompanying drawings:

[0030] See also Figure 1 The present invention discloses a process flow chart for recovering valuable metals in welding rods after aerobic pyrolysis of waste crystalline silicon photovoltaic modules. As can be seen from the figure, the method for recovering valuable metals in welding rods after aerobic pyrolysis of waste crystalline silicon photovoltaic modules includes the following steps: (1) physically refining welding rods; (2) adding copper chloride to the mixture; (3) high-temperature chlorination treatment under controlled pressure; (4) three-stage step-by-step cooling to separate volatile flue gas; (5) natural cooling to recover copper metal. In view of the complex structure and various components of welding rods under aerobic pyrolysis conditions, the present invention adopts high-temperature chlorination and step-by-step cooling processes according to the physical and chemical properties of copper, lead and tin metal chlorides, thereby achieving a sophisticated separation of valuable metal substances in flue gas and purification of copper metal. The content of lead and tin impurities in the final copper product can be reduced to less than 0.5%, respectively. This solves the problem that aerobic pyrolysis welding rods are difficult to separate, purify and recycle, and is conducive to the recycling of copper, lead and tin metals.

[0031] The present invention discloses a method for recovering valuable metals in welding rods after pyrolysis of waste crystalline silicon photovoltaic modules, and the specific steps are as follows:

[0032] (1) The pyrolysis welding rod is crushed to a particle size of less than 30 mm; the specific surface area of ​​the welding rod is effectively increased, providing better conditions for the subsequent high-temperature chlorination reaction, making the chlorination reaction more complete, and improving the extraction efficiency of valuable metals.

[0033] (2) adding cupric chloride powder to the pulverized welding rod in step (1) and mixing them thoroughly; the addition of cupric chloride not only promotes the chlorination reaction of copper in the welding rod, but also utilizes the catalytic effect of cupric chloride to enhance the chlorination effect of other valuable metals such as lead and tin, thus laying a foundation for subsequent separation and purification.

[0034] (3) subjecting the mixed raw materials obtained in step (2) to a high-temperature chlorination reaction in a pressure-controlled reactor under a chlorine atmosphere; the chlorination treatment under high temperature and controlled pressure conditions effectively promotes the chlorination reaction of various metal elements in the welding rod, allowing the valuable metals to enter the gas phase in the form of chlorides, which is convenient for subsequent separation and recovery.

[0035] (4) During the high-temperature reaction, lead-tin-containing substances are converted into volatile chlorides and enter the flue gas. After three stages of cooling and crystallization, the volatile substances in the flue gas can be obtained as copper chloride, lead chloride, tin dichloride and tin tetrachloride, respectively. The excess chlorine can be recycled after recovery. After the high-temperature reaction, copper with a low lead-tin content can be obtained after cooling, which can be used as a raw material for producing pure copper or copper alloys. By precisely controlling the cooling temperature and time and utilizing the difference in the volatilization temperature of different metal chlorides, the effective separation of metal chlorides such as copper, lead and tin is achieved, greatly improving the recovery purity and efficiency of valuable metals. After the first three steps of treatment, high-purity copper metal can be obtained by natural cooling, in which the lead and tin impurity content is significantly reduced to less than 0.5%, providing high-quality raw materials for subsequent deep processing of copper.

[0036] As a preferred technical solution of the present invention, the particle size of the welding rod in step (1) is 0.1-30 mm. Strict control of the particle size of the welding rod ensures the uniformity and high efficiency of the chlorination reaction and increases the reaction contact area.

[0037] Furthermore, in step (2), the size of the cupric chloride powder is less than 100 μm, the amount added is 3%-15% of the mass of the welding rod, and the mixing time is 10-90 min. The fine particle size of the cupric chloride powder improves its contact efficiency with the metal in the welding rod, promotes the chlorination reaction, and thus improves the extraction rate of valuable metals. The appropriate amount of cupric chloride powder added ensures that the chlorination reaction is fully carried out, and neither wastes resources nor affects the reaction effect due to excessive addition. The control of the mixing time ensures that the cupric chloride powder is fully in contact with the metal in the welding rod, laying a good foundation for the subsequent chlorination reaction.

[0038] Furthermore, the chlorination reaction temperature in step (3) is 1000-1200°C, the treatment time is 1-10h, chlorine is used as a protective atmosphere, and the pressure under air pressure conditions is 0.1-0.5atm. High temperature conditions are conducive to the chlorination reaction, which improves the reaction rate and the extraction efficiency of valuable metals. At the same time, the interference of other non-target components in the welding rod can be avoided within this temperature range, ensuring the high-purity extraction of valuable metals. The appropriate chlorination reaction time ensures the full progress of the reaction, and neither incomplete reaction due to too short a time nor waste of energy and time due to too long a time. Chlorine as a protective atmosphere can effectively prevent the valuable metals from being oxidized or reacting with other impurities during the chlorination process, ensuring the high-purity extraction of valuable metals. Appropriate pressure conditions are conducive to the chlorination reaction and the volatilization of valuable metals.

[0039] Furthermore, step (4) comprises three cooling stages, wherein the first stage cooling temperature is 680-880° C., and a mixture of copper chloride and lead chloride can be obtained after cooling, and copper chloride and lead chloride can be separated by subsequent water leaching. Control of the first stage cooling temperature enables copper chloride and lead chloride to form a mixture and be easily separated by water leaching, thereby achieving effective separation and purification of copper and lead.

[0040] Furthermore, the second stage cooling temperature is 200-400° C., and solid tin dichloride can be obtained after cooling. Control of the second stage cooling temperature enables tin dichloride to precipitate in the form of solid, which is convenient for subsequent collection and purification, and realizes effective separation and recovery of tin.

[0041] Furthermore, the third stage cooling temperature is 20-60°C, and a tin tetrachloride liquid can be obtained after cooling, and the excess chlorine is recycled by returning to the chlorination reaction. The control of the third stage cooling temperature allows the tin tetrachloride to precipitate in the form of a liquid, which is convenient for subsequent collection and purification. At the same time, the excess chlorine is recycled by returning to the chlorination reaction, thereby improving resource utilization and environmental protection.

[0042] Through the recovery method of the present invention, the content of lead and tin in the copper product finally obtained is significantly reduced, the purity and quality of copper are improved, and high-quality raw materials are provided for the subsequent deep processing of copper. At the same time, this also realizes the effective separation and recovery of lead and tin, and improves the recovery value and utilization rate of the overall valuable metals. The method of the present invention not only solves the problem that valuable metals in welding rods are difficult to recycle under aerobic pyrolysis conditions, but also realizes the efficient separation and purification of metals such as copper, lead, and tin through the innovative application of high-temperature chlorination and step-by-step cooling processes, significantly improving the recovery value and utilization rate of valuable metals, opening up a new way for the resource utilization of waste crystalline silicon photovoltaic modules, and is of great significance to promoting circular economy and sustainable development.

[0043] The numerical range described in the present invention not only includes the point values ​​listed above, but also includes any point values ​​between the above numerical ranges that are not listed. For the sake of simplicity, the present invention no longer exhaustively lists the specific point values ​​included in the range.

[0044] The present invention aims to solve the problem that the welding rods of waste crystalline silicon photovoltaic modules under aerobic pyrolysis conditions have complex structures, numerous components, and are difficult to recycle, and innovatively proposes a method for efficiently separating impurities. After the aerobic pyrolysis welding rods are crushed and treated with a high-temperature chlorination reaction, a three-stage flue gas cooling crystallization method is proposed based on the physical and chemical properties of each metal chloride therein, thereby achieving a sophisticated separation of copper, lead, and tin substances in the flue gas, and also achieving the purification of metallic copper, and the lead and tin contents in the obtained copper can be reduced to less than 0.5%, respectively. Among them, the lead content is reduced to 0.21%-0.42%; the tin content is reduced to 0.18%-0.28%. This provides a new method for improving the resource utilization of valuable metals in welding rods after aerobic pyrolysis of waste photovoltaic modules.

[0045] The present invention will be further described below in conjunction with specific embodiments:

[0046] Example 1

[0047] A method for recovering valuable metals in welding rods after pyrolysis of waste crystalline silicon photovoltaic modules, comprising the following steps:

[0048] First, the aerobic pyrolysis welding rod is crushed to a particle size of less than 30mm. Then take 100g of the crushed welding rod, add 8% cupric chloride powder, and mix thoroughly for 30 minutes. After mixing, put it into a tube, evacuate it, and then introduce chlorine gas to a pressure of 0.3atm. React at a high temperature of 1100℃ for 1h. During this process, the first cooling temperature of the volatile flue gas is 800℃, the second cooling temperature is 300℃, and the third cooling temperature is 30℃, which can achieve the separation of metal chlorides in the flue gas. Finally, after natural cooling, the lead and tin contents in the obtained copper sample are 0.41% and 0.24% (mass percentage), respectively.

[0049] Example 2

[0050] A method for recovering valuable metals in welding rods after pyrolysis of waste crystalline silicon photovoltaic modules, comprising the following steps:

[0051] First, the aerobic pyrolysis welding rod is crushed to a particle size of less than 30mm. Then take 100g of the crushed welding rod, add 10% cupric chloride powder, and mix thoroughly for 40min. After mixing, put it into a tube, evacuate it, and then introduce chlorine gas to a pressure of 0.1atm. React at a high temperature of 1100℃ for 2h. During this process, the first cooling temperature of the volatile flue gas is 750℃, the second cooling temperature is 250℃, and the third cooling temperature is 50℃, which can realize the separation of metal chlorides in the flue gas. Finally, after natural cooling, the lead and tin contents in the obtained copper sample are 0.35% and 0.27% (mass percentage), respectively.

[0052] Example 3

[0053] A method for recovering valuable metals in welding rods after pyrolysis of waste crystalline silicon photovoltaic modules, comprising the following steps:

[0054] First, the aerobic pyrolysis welding rod is crushed to a particle size of less than 30mm. Then take 100g of the crushed welding rod, add 10% cupric chloride powder, and mix thoroughly for 40min. After mixing, place it in a tube, evacuate it, and then introduce chlorine gas to a pressure of 0.3atm. React at a high temperature of 1150℃ for 2h. During this process, the first cooling temperature of the volatile flue gas is 800℃, the second cooling temperature is 250℃, and the third cooling temperature is 30℃, which can realize the separation of metal chlorides in the flue gas. Finally, after natural cooling, the lead and tin contents in the obtained copper sample are 0.28% and 0.21% (mass percentage), respectively.

[0055] Example 4

[0056] A method for recovering valuable metals in welding rods after pyrolysis of waste crystalline silicon photovoltaic modules, comprising the following steps:

[0057] First, the aerobic pyrolysis welding rod is crushed to a particle size of 0.1mm. Then take 100g of the crushed welding rod, add 30% cupric chloride powder, and mix thoroughly for 10 minutes. After mixing, put it into a tube, evacuate it, and then introduce chlorine gas to a pressure of 0.2atm. React at a high temperature of 1000℃ for 10h. During this process, the first cooling temperature of the volatile flue gas is 700℃, the second cooling temperature is 200℃, and the third cooling temperature is 20℃, which can achieve the separation of metal chlorides in the flue gas. Finally, after natural cooling, the lead and tin contents in the obtained copper sample are 0.42% and 0.28% (mass percentage), respectively.

[0058] Example 5

[0059] A method for recovering valuable metals in welding rods after pyrolysis of waste crystalline silicon photovoltaic modules, comprising the following steps:

[0060] First, the aerobic pyrolysis welding rod is crushed to a particle size of 10mm. Then take 100g of the crushed welding rod, add 12% cupric chloride powder, and mix thoroughly for 80min. After mixing, put it into a tube, evacuate it, and then introduce chlorine gas to a pressure of 0.4atm. React at a high temperature of 1200℃ for 8h. During this process, the first cooling temperature of the volatile flue gas is 850℃, the second cooling temperature is 400℃, and the third cooling temperature is 60℃, which can realize the separation of metal chlorides in the flue gas. Finally, after natural cooling, the lead and tin contents in the obtained copper sample are 0.26% and 0.2% (mass percentage), respectively.

[0061] Example 6

[0062] A method for recovering valuable metals in welding rods after pyrolysis of waste crystalline silicon photovoltaic modules, comprising the following steps:

[0063] First, the aerobic pyrolysis welding rod is crushed to a particle size of 20mm. Then take 100g of the crushed welding rod, add 15% cupric chloride powder, and mix thoroughly for 90min. After mixing, put it into a tube, evacuate it, and then introduce chlorine gas to a pressure of 0.5atm. React at a high temperature of 1200℃ for 4h. During this process, the first cooling temperature of the volatile flue gas is 880℃, the second cooling temperature is 350℃, and the third cooling temperature is 40℃, which can realize the separation of metal chlorides in the flue gas. Finally, after natural cooling, the lead and tin contents in the obtained copper sample are 0.34% and 0.28% (mass percentage), respectively.

[0064] The present invention aims to solve the problem that the welding rods of waste crystalline silicon photovoltaic modules under aerobic pyrolysis conditions are complex in structure, have many components, and are difficult to recycle, and innovatively proposes a method for efficiently separating impurities. After the aerobic pyrolysis welding rods are crushed and treated with a high-temperature chlorination reaction, a three-stage flue gas cooling crystallization method is proposed based on the physical and chemical properties of each metal chloride therein, which achieves the precise separation of copper, lead, and tin substances in the flue gas, and also achieves the purification of metallic copper. The lead and tin contents in the obtained copper can be reduced to less than 0.5%, respectively. This provides a new method for improving the resource utilization of valuable metals in welding rods after aerobic pyrolysis of waste photovoltaic modules.

[0065] The above contents are only for explaining the technical idea of ​​the present invention and cannot be used to limit the protection scope of the present invention. Any changes made on the basis of the technical solution in accordance with the technical idea proposed by the present invention shall fall within the protection scope of the claims of the present invention.

Claims

1. A method for recovering valuable metals in welding rods after aerobic pyrolysis of waste crystalline silicon photovoltaic modules, characterized in that: include: The welding rods after aerobic pyrolysis of waste crystalline silicon photovoltaic modules are crushed, and then copper chloride powder is added, mixed thoroughly, and a chlorination reaction is carried out. After three stages of cooling and crystallization, copper with a low lead-tin content is obtained.

2. The method for recovering valuable metals in welding rods after aerobic pyrolysis of waste crystalline silicon photovoltaic modules according to claim 1, characterized in that: The particle size of the pulverized welding rod is 0.1-30 mm; the particle size of the cupric chloride powder is less than 100 μm.

3. The method for recovering valuable metals in welding rods after aerobic pyrolysis of waste crystalline silicon photovoltaic modules according to claim 1, characterized in that: The added amount of the cupric chloride powder is 3%-15% of the mass of the welding rod; and the mixing time is 10-90 minutes.

4. The method for recovering valuable metals in welding rods after aerobic pyrolysis of waste crystalline silicon photovoltaic modules according to claim 1, characterized in that: The temperature of the chlorination reaction is 1000-1200°C.

5. The method for recovering valuable metals in welding rods after aerobic pyrolysis of waste crystalline silicon photovoltaic modules according to claim 1, characterized in that: The chlorination reaction time is 1-10h.

6. The method for recovering valuable metals in welding rods after aerobic pyrolysis of waste crystalline silicon photovoltaic modules according to claim 1, characterized in that: The protective atmosphere of the chlorination reaction is chlorine gas, and the pressure is 0.1-0.5atm.

7. The method for recovering valuable metals in welding rods after aerobic pyrolysis of waste crystalline silicon photovoltaic modules according to claim 1, characterized in that: In the three-stage cooling crystallization, the temperature of the first stage cooling is 680-880° C. After the first stage cooling, a mixture of copper chloride and lead chloride is obtained, and the copper chloride and lead chloride are separated by water leaching.

8. The method for recovering valuable metals in welding rods after aerobic pyrolysis of waste crystalline silicon photovoltaic modules according to claim 1, characterized in that: In the three-stage cooling crystallization, the second stage cooling temperature is 200-400° C.; after the second stage cooling, solid tin dichloride is obtained.

9. The method for recovering valuable metals in welding rods after aerobic pyrolysis of waste crystalline silicon photovoltaic modules according to claim 1, characterized in that: In the three-stage cooling crystallization, the third stage cooling temperature is 20-60° C. After the third stage cooling, tin tetrachloride liquid is obtained, and the excess chlorine is returned to the chlorination reaction for recycling.

10. The recovery of valuable metals in welding rods after aerobic pyrolysis of waste crystalline silicon photovoltaic modules according to claim 1 The collecting method is characterized in that In the copper with low lead-tin content, the lead mass percentage is reduced to below 0.5%, The tin mass percentage dropped to below 0.5%.

Citation Information

Cited By

  • Separation and recovery method for valuable metal in retired photovoltaic module solder strip

    CN119710236A

  • Method for recovering copper and tin from waste photovoltaic panel

    CN121915252A

  • Method for recovering copper and tin from waste photovoltaic panels

    CN121915252B