Heat-resistant steel and casting method suitable for turbocharger shell
By using low-carbon steel to prepare heat-resistant steel in the turbocharger housing, combining alloy element additives and deoxygenation treatment technology, the problems of high material costs and high consumption of rare metals are solved, and the dual optimization of high temperature performance and cost are achieved. Suitable for casting of turbocharger housings.
Patent Information
- Application Number
- CN202411092701.2
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Priority Date
- 2023-08-10
- Filing Date
- 2024-08-09
- Publication Date
- 2024-11-15
AI Technical Summary
The existing turbocharger housing materials are high and consumes high resources for rare metals, making it difficult to reduce costs while ensuring high-temperature performance.
Using low carbon steel as the substrate, heat-resistant steel is prepared through specific chemical composition and process treatment, including alloy element additives, deoxygenation treatment and fully automatic casting technology, controlling the smelting and casting temperatures, and optimizing the casting process to reduce costs and improve performance.
It realizes the reduction of the material cost of the turbocharger housing without reducing the high temperature performance, and improves the high temperature performance and casting accuracy of the material, reduces the use of rare metals, and meets the working conditions of the turbocharger housing. need.
Smart Images

Figure CN118957452A_ABST
Abstract
Description
Technical Field
[0001] The invention belongs to the technical field of heat-resistant steel and turbocharger casting, and particularly relates to a heat-resistant steel and a casting method thereof suitable for a turbocharger housing. Background Art
[0002] Heat-resistant steel refers to alloy steel with high strength and good chemical stability at high temperatures. It mainly includes two types: oxidation-resistant steel and heat-resistant steel. Oxidation-resistant steel mainly requires good chemical stability, while heat-resistant steel requires high high-temperature strength and corresponding oxidation resistance. Heat-resistant steel is often used to manufacture parts that work at high temperatures in boilers, steam turbines, power machinery, industrial furnaces, and aviation, petrochemical and other industrial sectors. In addition to requiring high-temperature strength and resistance to high-temperature oxidation corrosion, these parts must also have sufficient toughness, good machinability and weldability, as well as a certain degree of organizational stability.
[0003] In recent years, the turbocharging technology in the automotive industry has developed rapidly. As the core component of the turbocharger, the turbocharger housing directly determines the performance and life of the turbocharger. With the rapid development of turbocharging technology in the automotive industry, the material requirements for the turbocharger housing are getting higher and higher. The turbocharger housing needs to work under harsh conditions such as high temperature, high pressure, and high-speed rotation. Therefore, the material is required to have excellent high-temperature strength, oxidation resistance, fatigue resistance, and corrosion resistance.
[0004] At present, most new turbocharger housings on the market are cast with NI-based heat-resistant steel, but the content of precious alloys, such as nickel alloys, is high and the cost is high. Therefore, is it possible to choose a heat-resistant steel and a casting method suitable for turbocharger housings that can meet the working conditions of turbochargers in terms of material, while reducing the use of non-renewable alloy resources, thereby saving energy and reducing costs. Summary of the invention
[0005] In view of the above technical problems, the present invention discloses a heat-resistant steel and a casting method thereof suitable for a turbocharger housing, which can reduce the use of non-renewable alloy resources, thereby saving energy and reducing costs.
[0006] In order to solve the above technical problems, the technical solution adopted by the present invention is: A heat-resistant steel: its raw material is mainly low-carbon steel, and is composed of the following chemical composition mass percentages of various alloy elements: carbon 0.35%-0.45%, silicon 0.5%-1.5%, manganese 0.5-2.0%, phosphorus ≤0.04%, sulfur ≤0.04%, chromium 23.0-24.0%, nickel 8.5-10%, niobium 0.8-0.9%, nitrogen 0.2%-0.28%; The smelting method of the heat-resistant steel comprises the following steps: Choose low carbon steel as the base material; Prepare corresponding alloy element additives according to mass percentage, wherein the alloy element additives include carburizer, ferrosilicon, ferromanganese, ferrophosphorus, ferrosulfur, ferrochrome, ferronickel, ferroniobium, ferromanganese, and ferrochromium nitride; placing the base material and alloying element additives into a furnace for smelting; The furnace temperature is controlled at 1650-1700° C., and within this temperature range, the molten steel in the furnace is sampled and analyzed, and the mass fraction of each chemical component is detected by a spectrometer, and the composition is adjusted according to the detection data until the composition meets the requirements; After smelting, sprinkle deslagging agent into the furnace and use a slag-skimming rod to remove the slag; Deoxidation treatment is carried out to reduce the oxygen content in the molten steel and improve the quality of the molten steel.
[0007] Preferably, the recarburizer includes recarburized pig iron, electrode powder, petroleum coke powder, charcoal powder or coke powder.
[0008] Optimized, the specific steps of the deoxidation treatment include: Prepare the deoxidizer. When the surface of the molten steel is calm and the slag layer is cleaned, and the furnace temperature is 1670℃, add the deoxidizer evenly and quickly into the molten steel. Stir the molten steel to allow the deoxidizer to quickly disperse in the molten steel and fully contact and react with the oxygen in the molten steel; During the stirring process, observe the reaction of the molten steel. When the oxygen in the molten steel reacts with the deoxidizer, a large number of bubbles will be generated and float to the surface of the molten steel. As the reaction proceeds, the oxygen content in the molten steel will gradually decrease. After the deoxidation reaction, a large amount of oxide inclusions will be generated in the molten steel. Skimming is used to remove these inclusions from the molten steel to ensure the purity of the molten steel.
[0009] Preferably, the deoxidizer comprises aluminum powder or quicklime.
[0010] Preferably, the melting furnace includes an induction heating furnace, a medium frequency induction melting furnace, a vacuum induction melting furnace, an electroslag remelting furnace or a plasma melting furnace.
[0011] A method for casting a heat-resistant steel suitable for a turbocharger housing comprises the following steps: Step 1, heat-resistant steel smelting; Step 2: Molding the core, using a fully automatic molding machine to mold the sand core and then place it into the mold cavity; Step three, box assembly and pouring; Step 4: Sand removal. 45 minutes after pouring, the boxes are unpacked and the casting blanks are neatly stacked in order.
[0012] Optimally, the steps of the box-closing and pouring are: Fully automatic box closing machine closes the boxes and sends them to be poured; The molten steel in the furnace is transferred into the ladle. The furnace temperature is controlled at 1650℃~1680℃ in this process. The temperature drop rate of the molten steel in the ladle after it comes out of the furnace is 8-12℃ / minute. A temperature gun is used to measure the temperature of the molten steel in the ladle before pouring. When the temperature drops to 1580~1620℃, pouring begins. At the end of pouring, the temperature in the ladle is measured again, and the temperature is not lower than 1560℃.
[0013] Optimally, in step three, the furnace temperature is controlled at 1660°C.
[0014] The beneficial effects of the present invention are: The heat-resistant steel used in the present invention is aimed at the special needs of heat-resistant steel, thereby improving the material performance based on low-carbon steel. On the basis of reducing the cost of precious alloys, the high temperature resistance of the turbocharger housing itself can be maintained. The high temperature resistance of the turbocharger housing can reach 1020°C, which has good high temperature performance and can effectively reduce costs.
[0015] The room temperature mechanical properties of the turbocharger housing structure prepared by the present invention are as follows: Yield strength ≥350MPa, tensile strength ≥500MPa, elongation ≥5%, Brinell hardness 200-270HBW, maximum operating temperature 1000℃, and room temperature mechanical properties are superior to those of existing nickel-based heat-resistant steel materials.
[0016] In response to the differentiated requirements of turbocharger housings for material properties, on the basis of meeting the requirements of high temperature resistance and ease of smelting and pouring, a substitution method is adopted to reduce the use and consumption of rare metal materials and optimize performance surplus. A heat-resistant steel smelting and casting method specifically for turbocharger housings is designed.
[0017] Control the pouring temperature and cooling rate, optimize the relative temperature of heat-resistant steel at different stages of the smelting process, ensure sufficient mixing and reaction of raw materials and controllable temperature during pouring, so as to obtain good organizational structure and performance, and improve the quality and performance of castings.
[0018] Set up a deoxidation treatment operation. As the molten steel solidifies, the solubility of oxygen will decrease significantly with the decrease in temperature, causing the precipitated oxygen to react with elements such as carbon in the molten steel to produce bubbles such as CO. If these bubbles remain in the steel, they will form pores, which will seriously affect the quality of the casting. The high oxygen content of the molten steel will also increase the tendency of cast steel to crack. Deoxidation treatment after slag removal can ensure that the deoxidation reaction is carried out in the purest molten steel possible, thereby improving the deoxidation efficiency and molten steel quality.
[0019] High degree of automation. The application of fully automatic molding machines has greatly improved the degree of automation in the casting process. Compared with traditional manual or semi-automatic casting methods, fully automatic molding machines can more accurately control casting parameters, reduce errors caused by human factors, improve casting accuracy and consistency, and are suitable for factory batch manufacturing.
[0020] The pouring temperature and pouring speed of the combination box pouring step are controlled to avoid casting defects. BRIEF DESCRIPTION OF THE DRAWINGS
[0021] Figure 1 It is a schematic diagram of the casting process of the present invention. DETAILED DESCRIPTION
[0022] In order to better understand the present invention, the content of the present invention is further clearly described below in conjunction with the embodiments and the accompanying drawings, but the protection content of the present invention is not limited to the following embodiments. In the following description, a large number of specific details are provided to provide a more thorough understanding of the present invention. However, it is obvious to those skilled in the art that the present invention can be implemented without one or more of these details.
[0023] like Figure 1 As shown, the present invention discloses a heat-resistant steel and a casting method thereof suitable for a turbocharger housing. Among them, a heat-resistant steel, whose raw material is mainly low-carbon steel, is composed of the following chemical composition mass percentages of various alloy elements: carbon 0.35%-0.45%, silicon 0.5%-1.5%, manganese 0.5-2.0%, phosphorus ≤0.04%, sulfur ≤0.04%, chromium 23.0-24.0%, nickel 8.5-10%, niobium 0.8-0.9%, nitrogen 0.2%-0.28%.
[0024] The smelting method of heat-resistant steel comprises the following steps: Choose low carbon steel as the base material; Prepare corresponding alloy element additives according to mass percentage, wherein the alloy element additives include carburizer, ferrosilicon, ferromanganese, ferrophosphorus, ferrosulfur, ferrochrome, ferronickel, ferroniobium, ferromanganese and ferrochrome nitride, and the carburizer includes carburized pig iron, electrode powder, petroleum coke powder, charcoal powder or coke powder; The base material and alloy element additives are placed in a melting furnace for melting. The melting furnace may be an induction heating furnace, a medium frequency induction melting furnace, a vacuum induction melting furnace, an electroslag remelting furnace or a plasma melting furnace; The furnace temperature is controlled at 1650-1700° C., and within this temperature range, the molten steel in the furnace is sampled and analyzed, and the chemical composition mass fraction of each alloy element is detected by a spectrometer, and the composition is adjusted according to the detection data until the composition meets the requirements; After smelting, sprinkle deslagging agent into the furnace and use a slag-skimming rod to remove the slag; Deoxidation treatment is carried out to reduce the oxygen content in the molten steel and improve the quality of the molten steel.
[0025] The specific steps of deoxidation treatment include: Prepare the deoxidizer. When the surface of the molten steel is calm and the slag layer is cleaned, and the furnace temperature is 1670℃, add the deoxidizer evenly and quickly into the molten steel. During this process, be careful to avoid the deoxidizer directly impacting the furnace wall or the bottom of the ladle to avoid introducing new impurities. Stir the molten steel to allow the deoxidizer to quickly disperse in the molten steel and fully contact and react with the oxygen in the molten steel; During the stirring process, observe the reaction of the molten steel. When the oxygen in the molten steel reacts with the deoxidizer, a large number of bubbles will be generated and float to the surface of the molten steel. As the reaction proceeds, the oxygen content in the molten steel will gradually decrease. After the deoxidation reaction, a large amount of oxide inclusions will be generated in the molten steel. Skimming is used to remove these inclusions from the molten steel to ensure the purity of the molten steel.
[0026] In the above arrangement, the deoxidizer can be aluminum powder or quicklime. Because the molten steel already contains a variety of alloy elements such as carburizer, ferrosilicon, ferromanganese, ferrophosphorus, ferrosulfur, ferrochrome, ferronickel, ferroniobium, etc., when deoxidizing the molten steel, this embodiment gives priority to using aluminum powder, a deoxidizer with high affinity for oxygen and capable of effectively reducing the oxygen content in the molten steel. When aluminum powder is used, aluminum is a strong deoxidizer and reacts with oxygen to form aluminum oxide, which has a low density and is easy to float and be removed, and then the product can be discharged by a slag skimming method.
[0027] The invention also discloses a casting method of heat-resistant steel suitable for a turbocharger housing, which comprises the following steps.
[0028] Step 1: Melting of heat-resistant steel.
[0029] Step 2: Molding the core. After molding with a fully automatic molding machine, place the sand core into the mold cavity. During this process, the sand core cannot collide with the molding sand and lose sand. After being placed flat in the mold cavity, the sand core cannot swing.
[0030] Step 3: Combine the box and pour. The steps of combining the box and pouring are as follows: Fully automatic box closing machine closes the boxes and sends them to be poured; The molten steel in the furnace is transferred into the ladle. The furnace temperature is controlled at 1650℃~1680℃ in this process. The temperature drop rate of the molten steel in the ladle after it comes out of the furnace is 8-12℃ / minute. A temperature gun is used to measure the temperature of the molten steel in the ladle before pouring. When the temperature drops to 1580~1620℃, pouring begins. At the end of pouring, the temperature in the ladle is measured again, and the temperature is not lower than 1560℃.
[0031] Step 4: Sand removal. 45 minutes after pouring, the sand is removed and the box is opened. The casting blanks are neatly stacked in order.
[0032] In step three, the outlet temperature of the molten steel in the furnace transferred into the ladle is controlled at 1660°C.
[0033] This embodiment optimizes the composition alloy elements of heat-resistant steel on the basis of Embodiment 1. The raw material is mainly low-carbon steel, which is composed of the following chemical composition mass percentages of various alloy elements: carbon 0.40%, silicon 1.3%, manganese 1.8%, phosphorus 0.035%, sulfur 0.035%, chromium 23.5%, nickel 9.3%, niobium 0.85%, and nitrogen 0.26%.
[0034] Finally, it should be noted that the above embodiments are only used to illustrate the technical solution of the present invention rather than to limit it. Other modifications or equivalent substitutions made to the technical solution of the present invention by ordinary technicians in the field should be included in the scope of the claims of the present invention as long as they do not depart from the spirit and scope of the technical solution of the present invention.
Claims
1. A heat-resistant steel, characterized in that: Its raw material is mainly low-carbon steel, which is composed of the following chemical composition mass percentages of various alloy elements: carbon 0.35%-0.45%, silicon 0.5%-1.5%, manganese 0.5-2.0%, phosphorus ≤0.04%, sulfur ≤0.04%, chromium 23.0-24.0%, nickel 8.5-10%, niobium 0.8-0.9%, nitrogen 0.2%-0.28%; The smelting method of the heat-resistant steel comprises the following steps: Choose low carbon steel as the base material; Prepare corresponding alloy element additives according to mass percentage, wherein the alloy element additives include carburizer, ferrosilicon, ferromanganese, ferrophosphorus, ferrosulfur, ferrochrome, ferronickel, ferroniobium, ferromanganese and ferrochrome nitride; placing the base material and alloying element additives into a furnace for smelting; The furnace temperature is controlled at 1650-1700° C., and within this temperature range, the molten steel in the furnace is sampled and analyzed, and the mass fraction of each chemical component is detected by a spectrometer, and the composition is adjusted according to the detection data until the composition meets the requirements; After smelting, sprinkle deslagging agent into the furnace and use a slag-skimming rod to remove the slag; Deoxidation treatment is carried out to reduce the oxygen content in the molten steel and improve the quality of the molten steel.
2. A heat-resistant steel according to claim 1, characterized in that: The recarburizer includes recarburized pig iron, electrode powder, petroleum coke powder, charcoal powder or coke powder.
3. A heat-resistant steel according to claim 2, characterized in that: The specific steps of the deoxidation treatment include: Prepare the deoxidizer. When the surface of the molten steel is calm and the slag layer is cleaned, and the furnace temperature is 1670℃, add the deoxidizer evenly and quickly into the molten steel. Stir the molten steel to allow the deoxidizer to quickly disperse in the molten steel and fully contact and react with the oxygen in the molten steel; During the stirring process, observe the reaction of the molten steel. When the oxygen in the molten steel reacts with the deoxidizer, a large number of bubbles will be generated and float to the surface of the molten steel. As the reaction proceeds, the oxygen content in the molten steel will gradually decrease. After the deoxidation reaction, a large amount of oxide inclusions will be generated in the molten steel. Skimming is used to remove these inclusions from the molten steel to ensure the purity of the molten steel.
4. A heat-resistant steel according to claim 3, characterized in that: The deoxidizer includes aluminum powder or quicklime.
5. A heat-resistant steel according to claim 4, characterized in that: The melting furnace includes an induction heating furnace, a medium frequency induction melting furnace, a vacuum induction melting furnace, an electroslag remelting furnace or a plasma melting furnace.
6. A method for casting a heat-resistant steel suitable for a turbocharger housing according to any one of claims 1 to 5, characterized in that: The following steps are involved: Step 1, heat-resistant steel smelting; Step 2: Molding the core, using a fully automatic molding machine to mold the sand core and then place it into the mold cavity; Step three, box assembly and pouring; Step 4: Sand removal. 45 minutes after pouring, the sand is removed and the box is opened. The casting blanks are neatly stacked in order.
7. A casting method for a heat-resistant steel suitable for a turbocharger housing according to claim 6, characterized in that: The steps of the box-closing pouring are: Fully automatic box closing machine closes the boxes and sends them to be poured; The molten steel in the furnace is transferred into the ladle. The temperature out of the furnace is controlled at 1650℃~1680℃ in this process. The temperature drop rate of the molten steel in the ladle after it comes out of the furnace is 8-12℃ / minute. Before pouring, a temperature gun is used to measure the temperature of the molten steel in the ladle. When the temperature drops to 1580~1620℃, pouring begins. At the end of pouring, the temperature in the ladle is measured again, and the temperature is not lower than 1560℃.
8. A casting method for a heat-resistant steel suitable for a turbocharger housing according to claim 7, characterized in that: In step three, the furnace temperature is controlled at 1660°C.