Back fine grid silver paste for TOPCon solar cell and preparation method of back fine grid silver paste
By combining silver paste with multi-size silver powder and specific resin, the problem of insufficient silver paste adhesion on the back of TOPCon batteries was solved, achieving efficient photoelectric conversion and improved wear resistance.
Patent Information
- Application Number
- CN202410973694.0
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-07-19
- Publication Date
- 2024-11-15
AI Technical Summary
The silver paste on the back of existing TOPCon batteries has problems such as insufficient adhesion, easy peeling, and grid breakage during the printing process, which makes it difficult to meet the requirements of high-efficiency photoelectric conversion and mechanical stress resistance.
A silver paste combination using a multi-particle-size silver powder system and a specific resin, with the addition of silane coupling agents and organic additives, improves adhesion and density and enhances conductivity through chemical bonding and cross-linking reactions.
It improves the adhesion and density of the silver layer, increases photoelectric conversion efficiency, and improves wear resistance and grid breakage during the printing process.
Smart Images

Figure BDA0004953941840000091 
Figure BDA0004953941840000101
Abstract
Description
Technical Field
[0001] The present invention relates to the technical field of photovoltaic electronic pastes, in particular to the field of IPCH01B1 / 22, and more specifically to a back-side fine grid silver paste for TOPCon solar cells and a preparation method thereof. Background Art
[0002] TOPCon cells are a new type of passivated contact solar cells. Through the synergistic effect of the tunneling oxide layer and the polysilicon layer, the surface recombination on the back of the silicon wafer can be significantly reduced, thereby increasing the open circuit voltage (Voc) and fill factor (FF) of the cell, thereby improving the overall efficiency of the cell and reducing losses. In recent years, TOPCon cells have been gradually adopted by the industry due to their obvious advantages such as high conversion efficiency, low attenuation performance, and high mass production cost performance. The silver paste must form a strong adhesion with the back passivation layer of the TOPCon cell to resist mechanical stress and environmental influences. At present, the N-type TOPCon cell uses an alkali polishing process to obtain a mirror-like back of the silicon wafer, which requires a higher adhesion of the silver paste on the silicon wafer. On the one hand, the silver paste needs to be able to dry quickly after printing to adapt to the rhythm of rapid production. On the other hand, it needs to have good adhesion after drying to ensure that there will be no problems such as silver fine grid falling off and broken grid during subsequent transmission and printing. Back fine grid silver paste printing is a crucial step in solar cell manufacturing. In order to reduce the shading area and improve the photoelectric conversion efficiency, the fine grid line should be as thin as possible while maintaining sufficient current carrying capacity. The silver paste is required to have strong mesh passing ability, good leveling and large aspect ratio. It is also required to avoid defects such as line breakage, holes, cracks, etc. that may occur during the printing process. These defects may affect the performance and reliability of the battery to a certain extent.
[0003] CN113979641A discloses a glass powder and a preparation method thereof, and a battery silver paste with a wide application window. It develops a suitable back silver paste for the polished surface of TOPCon solar cells, which can solve the problems of narrow contact window, EL fogging and even blackening on the back of TOPCon cells, but does not provide a detailed description of thin Si-poly structures. Summary of the invention
[0004] The first aspect of the present invention provides a back fine grid silver paste for TOPCon solar cells, which comprises, by weight, 75-90 parts of silver powder, 7-15 parts of organic carrier, 1.7-4 parts of glass powder, and 0.5-6 parts of organic additives.
[0005] The silver paste also includes a solvent.
[0006] The D50 particle size of the silver powder is 1-5 microns.
[0007] Preferably, the D50 particle size of the silver powder includes 1.4-1.6 microns and 1.6-2 microns.
[0008] Preferably, the weight ratio of the silver powder with a D50 particle size of 1.4-1.6 microns to that of the silver powder with a D50 particle size of 1.6-2 microns is (10-25):(60-75).
[0009] Preferably, the silver powder having a D50 particle size of 1.6-2 microns includes at least one of 1.6-1.8 microns and 1.9-2.0 microns.
[0010] The present application has found that the D50 particle size of the silver powder includes 1.4-1.6 microns and 1.6-2 microns, and the weight ratio of the silver powder with a D50 particle size of 1.4-1.6 microns and 1.6-2 microns is limited to (10-25): (60-75), which can increase the photoelectric conversion efficiency. It may be that the two particle size silver powders are compounded, which reduces the porosity, increases the tap density, and increases the bonding tightness between the particles. At the same time, the glass powder fully wets the silver powder during the melting process to form a good ohmic contact, so that the conductive film formed after printing and sintering is dense and uniform, the film has small pores, low porosity, and good conductivity.
[0011] Further research found that the resin includes acrylic resin, polyvinyl butyral resin, epoxy resin and ethyl cellulose, and the mass ratio of the acrylic resin, polyvinyl butyral resin, epoxy resin and ethyl cellulose is (4-6): (2-5): (0.5-1.5): (0.3-2). It can promote the close combination of the components, improve the adhesion of the silver layer, and enhance the compactness and conductivity. The resin is used as a bonding phase to provide adhesion, provide support for the slurry skeleton, and reduce the gap between the silver particles. At the same time, the resin does not undergo a cross-linking reaction during curing. The presence of epoxy resin can greatly improve the adhesion of the silver paste. The polar epoxy group can undergo a cross-linking reaction with the hydroxyl groups on other resins, which is beneficial to improve the rapid drying of the slurry, while promoting the close combination of the components, improving the adhesion of the silver layer, and enhancing the compactness and conductivity.
[0012] The organic carrier comprises resin, organic solvent and silane coupling agent.
[0013] Preferably, the resin comprises acrylic resin, polyvinyl butyral resin, epoxy resin and ethyl cellulose, and the mass ratio of the acrylic resin, polyvinyl butyral resin, epoxy resin and ethyl cellulose is (4-6): (2-5): (0.5-1.5): (0.3-2).
[0014] The organic solvent includes at least one of isophorone, terpineol, dimethyl phthalate, dimethyl terephthalate, diethylene glycol butyl ether, diethylene glycol butyl ether acetate, alcohol ester-12, alcohol ester-16, butyl carbiphenol, butyl carbiphenol acetate and ethylene glycol phenyl ether.
[0015] Preferably, the organic solvent includes diethylene glycol butyl ether, alcohol ester-16, and diethylene glycol butyl ether acetate, and the mass ratio of diethylene glycol butyl ether, alcohol ester-16, and diethylene glycol butyl ether acetate is (2-3): (1-4): (3-6).
[0016] The silane coupling agent includes at least one of a styrene-based silane coupling agent, a methylacryl-based silane coupling agent, an acryl-based silane coupling agent, and an amino-based silane coupling agent.
[0017] Preferably, the silane coupling agent includes an acryl silane coupling agent.
[0018] The organic additive includes at least one of a thixotropic agent, a leveling agent and a dispersant.
[0019] Preferably, the organic additives include a thixotropic agent, a leveling agent and a dispersant.
[0020] Further preferably, the weight ratio of the thixotropic agent, the leveling agent and the dispersant is (0.5-1):(1-1.5):(1-2).
[0021] The thixotropic agent includes at least one of hydrogenated castor oil, polyamide wax, polyvinyl alcohol and hydroxypropyl methylcellulose.
[0022] Preferably, the thixotropic agent comprises polyamide wax.
[0023] The leveling agent includes at least one of polyurethane, silicone oil and polysiloxane.
[0024] The dispersant includes at least one of polyvinyl alcohol and polyvinyl chloride alcohol.
[0025] Preferably, the acrylic resin is selected from one or a combination of JS-10 and JS-30 of Polysheng Chemical, BR-115, BR-116, and LR-7609 of Mitsubishi Liyang Chemical of Japan, and AC-510, AC162, and B32 of Shanghai Qizhan New Materials.
[0026] The polyvinyl butyral resin is selected from one or a combination of Yamade Butvar-76, Japan Sekisui BL-2, Kuraray Mowital B30H, Mowital B45M, Mowital B45H, and Mowital B60T.
[0027] The epoxy resin is selected from one or a combination of Nan Ya NPES-903, NPEF-903H, NPEF-902, and Dow DER series.
[0028] The ethyl cellulose is selected from one or a combination of Dow ethyl cellulose STD-4, STD-10, STD-45, Ashland Natrosol Plus 330, 250HBR, 250HHBR.
[0029] The styrene resin is selected from one or a combination of the following: POLYSCOPES Z25010 from the Netherlands, TORAY 450YX10 from Japan, and Clayville SMA-3000P.
[0030] Acrylic silane coupling agent: Momentive A-174, A-178, Dow Corning silane coupling agent Z-6030, Z-6033, one or more combinations of jessicachem KH series.
[0031] Silver powder with a D50 particle size of 1.4-1.6 microns: one or a combination of dowaAG-3-1F, Yinrui YRS-S180-3C, Xilong S815C.
[0032] Silver powder with a particle size of 1.6-1.8 microns at D50: one or a combination of Smet S354, Jianbang E30QP20, and Tianfu TFGP-02.
[0033] D50 silver powder with a particle size of 1.9-2 microns: one or a combination of Dongguan Dazhou DSP-90, Jianbang 152-20, dowa4-8F.
[0034] Polyamide wax: one or more combinations of THIXATRO LPM8056, PLUS, P600 and HLAQ series.
[0035] A second aspect of the present invention provides a method for preparing a back fine grid silver paste for a TOPCon solar cell, comprising the following steps:
[0036] S1, resin dissolution: weigh the resin and the organic solvent, pour them into a three-necked flask, and stir at 50-80°C for 30-120 minutes to obtain a resin solution; after the resin solution is cooled, add a silane coupling agent, stir for 30-60 minutes, and obtain an organic carrier;
[0037] S2, silver paste preparation: mix the organic carrier with silver powder, glass powder and organic additives, add them into a planetary mixer, stir evenly at a stirring speed of 200-600rpm for 0.5h, and then roll through a three-roll mill for 3-5 times until the slurry fineness meets the requirements.
[0038] Beneficial effects:
[0039] 1. The conductive silver powder used in the present invention is a multi-silver powder system, including a combination of silver powders of various particle sizes, which can improve the compactness of the silver layer and thus increase the photoelectric conversion efficiency.
[0040] 2. The present invention adds a variety of resins to the silver paste for compounding, which can meet the high-speed printing requirements while narrowing the linear type. The presence of epoxy resin in the carrier can greatly improve the adhesion of the silver paste. The polar epoxy group can undergo a cross-linking reaction with the hydroxyl groups on other resins, which is beneficial to improving the rapid drying of the paste, while promoting close bonding between the components, improving the adhesion of the silver layer, and enhancing the density and conductivity.
[0041] 3. Add silane coupling agent to the silver paste, which combines with the hydroxyl group and hydrogen on the surface of the inorganic material to form a chemical bond, thereby improving the adhesion of the silver paste to the silicon wafer surface. In addition, the silane coupling agent, with its polar group, can form a hydrogen bond with the hydroxyl group on the resin, effectively improving the compatibility of the resin, and facilitating the wettability and coating of the organic carrier on the silver powder.
[0042] 4. By compounding specific organic solvents, the wear resistance can be improved and the grid breaking condition of the battery cell can be improved. DETAILED DESCRIPTION
[0043] Example 1
[0044] A back fine grid silver paste for TOPCon solar cells comprises, by weight, 85 parts of silver powder, 7.5 parts of organic carrier, 3.5 parts of glass powder, 3 parts of organic additives and 1 part of cosolvent.
[0045] The organic carrier is a resin, an organic solvent and a silane coupling agent; the resin is 30g of acrylic resin, 10g of polyvinyl butyral resin, 5g of epoxy resin and 5g of ethyl cellulose; the organic solvent is 15g of diethylene glycol butyl ether, 15g of alcohol ester-16 and 20g of diethylene glycol butyl ether acetate; the silane coupling agent is 5g of acryl silane coupling agent.
[0046] The silver powder includes 25 parts of silver powder with a D50 particle size of 1.4-1.6 microns and 60 parts of silver powder with a D50 particle size of 1.6-1.8 microns.
[0047] The organic additives are thixotropic agent, leveling agent and dispersant, the thixotropic agent is polyamide wax, the leveling agent is silicone oil, and the dispersant is polyvinyl chloride alcohol, including 0.5 parts of polyamide wax, 1 part of silicone oil, and 1.5 parts of polyvinyl chloride alcohol.
[0048] The cosolvent is diethylene glycol butyl ether.
[0049] A method for preparing a back fine grid silver paste for a TOPCon solar cell comprises the following steps:
[0050] S1, resin dissolution: weigh the resin and the organic solvent, pour them into a three-necked flask, and stir them at 80°C and 1000 rpm for 60 min to obtain a resin solution; after the resin solution is cooled, add the silane coupling agent, stir it in a high-speed disperser for 30 min at a speed of 1000 rpm to obtain an organic carrier (all used in step S2);
[0051] S2, silver paste preparation: the organic carrier is mixed with silver powder, glass powder and organic additives, added into a planetary mixer, stirred evenly at a stirring speed of 200 rpm for 0.5 h, and then rolled 4 times by a three-roll mill until the slurry fineness is qualified.
[0052] Example 2
[0053] A back fine grid silver paste for TOPCon solar cells comprises, by weight, 85 parts of silver powder, 8 parts of organic carrier, 3 parts of glass powder, 3 parts of organic additives and 1 part of cosolvent.
[0054] The organic carrier is a resin, an organic solvent and a silane coupling agent;
[0055] The resin is 25g of acrylic resin, 10g of polyvinyl butyral resin, 7g of epoxy resin, and 6g of ethyl cellulose; the organic solvent is 15g of diethylene glycol butyl ether, 15g of alcohol ester-16, and 20g of diethylene glycol butyl ether acetate; and the silane coupling agent is 5g of acryl silane coupling agent.
[0056] The silver powder includes 25 parts of silver powder with a D50 particle size of 1.4-1.6 microns and 60 parts of silver powder with a D50 particle size of 1.9-2 microns.
[0057] The organic additives are thixotropic agent, leveling agent and dispersant, the thixotropic agent is polyamide wax, the leveling agent is silicone oil, and the dispersant is polyvinyl chloride alcohol, including 0.5 parts of polyamide wax, 1 part of silicone oil, and 1.5 parts of polyvinyl chloride alcohol.
[0058] The cosolvent is diethylene glycol butyl ether acetate.
[0059] A method for preparing back fine grid silver paste for TOPCon solar cells, same as that of Example 1.
[0060] Example 3
[0061] A back fine grid silver paste for TOPCon solar cells comprises, by weight, 85 parts of silver powder, 7.5 parts of organic carrier, 2.5 parts of glass powder, 3 parts of organic additives and 2 parts of cosolvent.
[0062] The organic carrier is a resin, an organic solvent and a silane coupling agent;
[0063] The resin is 30g of acrylic resin, 15g of polyvinyl butyral resin, 5g of epoxy resin, and 6g of ethyl cellulose; the organic solvent is 10g of diethylene glycol butyl ether, 9g of alcohol ester-16, and 25g of diethylene glycol butyl ether acetate; and the silane coupling agent is 7g of acryl silane coupling agent.
[0064] The silver powder includes 20 parts of silver powder with a D50 particle size of 1.4-1.6 microns and 60 parts of silver powder with a D50 particle size of 1.6-1.8 microns.
[0065] The organic additives are thixotropic agent, leveling agent and dispersant, the thixotropic agent is polyamide wax, the leveling agent is silicone oil, and the dispersant is polyvinyl chloride alcohol, including 0.5 parts of polyamide wax, 1 part of silicone oil, and 1.5 parts of polyvinyl chloride alcohol.
[0066] The cosolvent is alcohol ester-16.
[0067] A method for preparing back fine grid silver paste for TOPCon solar cells, same as that of Example 1.
[0068] Example 4
[0069] A back fine grid silver paste for TOPCon solar cells comprises, by weight, 85 parts of silver powder, 8 parts of organic carrier, 2.5 parts of glass powder, 3.5 parts of organic additives and 1 part of cosolvent.
[0070] The organic carrier is a resin, an organic solvent and a silane coupling agent;
[0071] The resin is 30g of acrylic resin, 15g of polyvinyl butyral resin, 6g of epoxy resin, and 5g of ethyl cellulose; the organic solvent is 10g of diethylene glycol butyl ether, 9g of alcohol ester-16, and 25g of diethylene glycol butyl ether acetate; and the silane coupling agent is 6g of acryl silane coupling agent.
[0072] The silver powder includes 10 parts of silver powder with a D50 particle size of 1.4-1.6 microns and 75 parts of silver powder with a D50 particle size of 1.9-2 microns.
[0073] The organic additives are thixotropic agent, leveling agent and dispersant, the thixotropic agent is polyamide wax, the leveling agent is silicone oil, and the dispersant is polyvinyl chloride alcohol, including 1 part of polyamide wax, 1 part of silicone oil, and 1.5 parts of polyvinyl chloride alcohol.
[0074] The cosolvent is diethylene glycol butyl ether acetate.
[0075] A method for preparing back fine grid silver paste for TOPCon solar cells, same as that of Example 1.
[0076] Comparative Example 1
[0077] A back fine grid silver paste for TOPCon solar cells comprises, by weight, 85 parts of silver powder, 7.5 parts of organic carrier, 3.5 parts of glass powder, 3 parts of organic additives and 1 part of cosolvent.
[0078] The organic carrier is a resin, an organic solvent and a silane coupling agent;
[0079] The resin is 30g of acrylic resin, 10g of polyvinyl butyral resin, 5g of epoxy resin, and 5g of ethyl cellulose; the organic solvent is 15g of diethylene glycol butyl ether, 15g of alcohol ester-16, and 20g of diethylene glycol butyl ether acetate; and the silane coupling agent is 5g of acryl silane coupling agent.
[0080] The silver powder is 85 parts of silver powder with a D50 particle size of 1.6-1.8 microns.
[0081] The organic additives are thixotropic agent, leveling agent and dispersant, the thixotropic agent is polyamide wax, the leveling agent is silicone oil, and the dispersant is polyvinyl chloride alcohol, including 0.5 parts of polyamide wax, 1 part of silicone oil, and 1.5 parts of polyvinyl chloride alcohol.
[0082] The cosolvent is diethylene glycol butyl ether.
[0083] A method for preparing back fine grid silver paste for TOPCon solar cells, same as that of Example 1.
[0084] Comparative Example 2
[0085] A back fine grid silver paste for TOPCon solar cells comprises, by weight, 85 parts of silver powder, 8 parts of organic carrier, 3 parts of glass powder, 3 parts of organic additives and 1 part of cosolvent.
[0086] The organic carrier is a resin or an organic solvent;
[0087] The resin is 25g of acrylic resin, 10g of polyvinyl butyral resin, 7g of epoxy resin, and 6g of ethyl cellulose; the organic solvent is 15g of diethylene glycol butyl ether, 15g of alcohol ester-16, and 20g of diethylene glycol butyl ether acetate.
[0088] The silver powder includes 25 parts of silver powder with a D50 particle size of 1.4-1.6 microns and 60 parts of silver powder with a D50 particle size of 1.9-2 microns.
[0089] The organic additives are thixotropic agent, leveling agent and dispersant, the thixotropic agent is polyamide wax, the leveling agent is silicone oil, and the dispersant is polyvinyl chloride alcohol, including 0.5 parts of polyamide wax, 1 part of silicone oil, and 1.5 parts of polyvinyl chloride alcohol.
[0090] The cosolvent is diethylene glycol butyl ether acetate.
[0091] A method for preparing back fine grid silver paste for TOPCon solar cells, same as that of Example 1.
[0092] Comparative Example 3
[0093] A back fine grid silver paste for TOPCon solar cells comprises, by weight, 85 parts of silver powder, 7.5 parts of organic carrier, 2.5 parts of glass powder, 3 parts of organic additives and 2 parts of cosolvent.
[0094] The organic carrier is a resin, an organic solvent and a silane coupling agent;
[0095] The resin is 32g of acrylic resin, 17g of polyvinyl butyral resin, and 7g of ethyl cellulose; the organic solvent is 10g of diethylene glycol butyl ether, 9g of alcohol ester-16, and 25g of diethylene glycol butyl ether acetate; and the silane coupling agent is 7g of acryl silane coupling agent.
[0096] The silver powder includes 20 parts of silver powder with a D50 particle size of 1.4-1.6 microns and 65 parts of silver powder with a D50 particle size of 1.6-1.8 microns.
[0097] The organic additives are thixotropic agent, leveling agent and dispersant, the thixotropic agent is polyamide wax, the leveling agent is silicone oil, and the dispersant is polyvinyl chloride alcohol, including 0.5 parts of polyamide wax, 1 part of silicone oil, and 1.5 parts of polyvinyl chloride alcohol.
[0098] The cosolvent is alcohol ester-16.
[0099] A method for preparing back fine grid silver paste for TOPCon solar cells, same as that of Example 1.
[0100] Comparative Example 4
[0101] A back fine grid silver paste for TOPCon solar cells comprises, by weight, 85 parts of silver powder, 8 parts of organic carrier, 2.5 parts of glass powder, 3.5 parts of organic additives and 1 part of cosolvent.
[0102] The organic carrier is a resin, an organic solvent and a silane coupling agent;
[0103] The resin is 30g of acrylic resin, 20g of styrene resin, and 6g of ethyl cellulose; the organic solvent is 10g of diethylene glycol butyl ether, 9g of alcohol ester-16, and 25g of diethylene glycol butyl ether acetate; and the silane coupling agent is 6g of acryl silane coupling agent.
[0104] The silver powder includes 10 parts of silver powder with a D50 particle size of 1.4-1.6 microns and 75 parts of silver powder with a D50 particle size of 1.6-1.8 microns.
[0105] The organic additives are thixotropic agent, leveling agent and dispersant, the thixotropic agent is polyamide wax, the leveling agent is silicone oil, and the dispersant is polyvinyl chloride alcohol, including 1 part of polyamide wax, 1 part of silicone oil, and 1.5 parts of polyvinyl chloride alcohol.
[0106] The cosolvent is alcohol ester-16.
[0107] A method for preparing back fine grid silver paste for TOPCon solar cells, same as that of Example 1.
[0108] The raw materials used in the above examples and comparative examples all come from the following manufacturers:
[0109] The acrylic resin is selected from JS-10 produced by Polysheng Chemical.
[0110] The polyvinyl butyral resin is selected from Yamed Butvar-76.
[0111] The epoxy resin is selected from Nan Ya NPES-903.
[0112] The ethyl cellulose is selected from Dow ethyl cellulose STD-4.
[0113] The styrene resin is selected from POLYSCOPES Z25010 from the Netherlands.
[0114] Acrylic silane coupling agent: Momentive A-174.
[0115] Silver powder with a D50 particle size of 1.4-1.6 microns: dowaAG-3-1F.
[0116] Silver powder with a D50 particle size of 1.6-1.8 microns: Smet S354.
[0117] Silver powder with a particle size of 1.9-2 microns at D50: Dongguan Dazhou DSP-90.
[0118] Polyamide wax: THIXATROLPM8056.
[0119] Silicone oil: Shin-Etsu dimethyl silicone oil KF96L.
[0120] Polyvinyl chloride alcohol: Japan Kuraray 17-94PVA.
[0121] Glass powder: Na2O.
[0122] Performance Testing Methods
[0123] The performance tests were carried out in the embodiments and comparative examples, and the test data are listed in Table 1.
[0124] Halm's IV tester was used to test the photoelectric conversion efficiency of the cell and the influence of the carrier formula on the photoelectric conversion efficiency of the TOPCon cell.
[0125] An EL tester is used to detect the broken grid of the battery cell and compare the adhesion of different carriers.
[0126] Use 3M tape to tear off the battery cell and compare the wear resistance. Stick the tape on the surface of the battery cell and tear it off quickly to compare the shedding situation. If 20-30% of the area is peeled off and there is obvious silver powder adhesion, it is considered to have fair wear resistance; if 10-20% of the area is peeled off and there is a small amount of silver powder adhesion, it is considered to have good wear resistance; if less than 10% of the area is peeled off and there is no silver powder adhesion, it is considered to have good wear resistance.
[0127] Performance test data
[0128] Table 1
[0129]
[0130]
Claims
1. A back-side fine grid silver paste for TOPCon solar cells, It is characterized in that In parts by weight, the components include: 75-90 parts of silver powder, 7-15 parts of organic carrier, 1.7-4 parts of glass powder, and 0.5-6 parts of organic additives.
2. The back fine grid silver paste for TOPCon solar cells according to claim 1, It is characterized in that The D50 particle size of the silver powder is 1-5 microns.
3. The back fine grid silver paste for TOPCon solar cells according to claim 2, It is characterized in that The organic carrier comprises resin, organic solvent and silane coupling agent.
4. The back fine grid silver paste for TOPCon solar cells according to claim 3, It is characterized in that The resin comprises acrylic resin, polyvinyl butyral resin, epoxy resin and ethyl cellulose, and the mass ratio of the acrylic resin, polyvinyl butyral resin, epoxy resin and ethyl cellulose is (4-6): (2-5): (0.5-1.5): (0.3-2).
5. The back fine grid silver paste for TOPCon solar cells according to claim 2 or 4, It is characterized in that The organic solvent includes at least one of isophorone, terpineol, dimethyl phthalate, dimethyl terephthalate, diethylene glycol butyl ether, diethylene glycol butyl ether acetate, alcohol ester-12, alcohol ester-16, butyl carbiphenol, butyl carbiphenol acetate and ethylene glycol phenyl ether.
6. The back fine grid silver paste for TOPCon solar cells according to claim 5, It is characterized in that The silane coupling agent includes at least one of a styrene-based silane coupling agent, a methylacryl-based silane coupling agent, an acryl-based silane coupling agent, and an amino-based silane coupling agent.
7. The back fine grid silver paste for TOPCon solar cells according to claim 6, It is characterized in that The organic additive includes at least one of a thixotropic agent, a leveling agent and a dispersant.
8. The back fine grid silver paste for TOPCon solar cells according to claim 7, It is characterized in that The thixotropic agent includes at least one of hydrogenated castor oil, polyamide wax, polyvinyl alcohol and hydroxypropyl methylcellulose.
9. The back fine grid silver paste for TOPCon solar cells according to claim 8, It is characterized in that The leveling agent includes at least one of polyurethane, silicone oil and polysiloxane.
10. A method for preparing a back side fine grid silver paste for TOPCon solar cells according to any one of claims 3 to 9, It is characterized in that The following steps are involved: S1, resin dissolution: weigh the resin and the organic solvent, pour them into a three-necked flask, and stir at 50-80°C for 30-120 minutes to obtain a resin solution; after the resin solution is cooled, add a silane coupling agent, stir for 30-60 minutes, and obtain an organic carrier; S2, silver paste preparation: mix the organic carrier with silver powder, glass powder and organic additives, add them into a planetary mixer, stir evenly at a stirring speed of 200-600rpm for 0.5-2h, and then roll through a three-roll mill for 3-5 times until the slurry fineness meets the requirements.
Citation Information
Patent Citations
Glass powder and preparation method thereof and battery silver paste with wide application window
CN113979641A
Cited By
Silver paste, preparation method thereof and photovoltaic cell
CN119626628A
Back fine grid silver paste for TOPCon solar cell and preparation method of back fine grid silver paste
CN120511100A