Method for testing thickness of damaged layer of silicon single crystal

Through multiple tests and etching of the Rz value of the silicon wafer surface, combined with the flexible proportioning and low life requirements of acid or alkali liquid, the problems of small samples and large deviations in the existing technology are solved, and the silicon is achieved Accurate detection of the thickness of the sheet damaged layer and damage-free testing of large component materials ensure the integrity of the process and product quality.

CN118969661APending Publication Date: 2024-11-15SHANGHAI SHENHE THERMO MAGNETICS ELECTRONICS CO LTD
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202411037338.4
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-07-31
Publication Date
2024-11-15

AI Technical Summary

Technical Problem

In the prior art, the number of test samples for the damage layer thickness of the silicon wafer is small, and the test results are large, making it difficult to accurately detect the broken layer thickness of the material of large components.

Method used

By performing multiple tests and etchings on the Rz value of the silicon wafer surface to be tested, the initial and subsequent Rz values ​​are recorded, the thickness of the broken layer is determined by using the difference in Rz values, the number of samples is increased, the deviation of the test result is reduced, and the acid solution is used Or the flexible ratio and low life requirements of lye solution to avoid affecting the test results of the etching solution.

Benefits of technology

Improve the accuracy and reliability of the test results, and are suitable for damage-free testing of large-scale component materials, ensuring complete removal of mechanical damage layers in subsequent processes and ensuring final product quality.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118969661A_ABST
    Figure CN118969661A_ABST
Patent Text Reader

Abstract

The invention provides a method for testing the thickness of a damaged layer of a silicon single crystal, and belongs to the technical field of surface defect detection of the silicon single crystal, and the method comprises the following steps: S1, testing Rz of the surface of a tested silicon wafer, recording data as Rz-1, and enabling Rz to be the sum of microcosmic profile wave crests and wave troughs of the surface of the tested silicon wafer; s2, etching the tested silicon wafer by using acid liquor or alkali liquor; s3, cleaning is carried out after etching, Rz of the surface of the tested silicon wafer continues to be tested, data is recorded as Rz-2, and the testing method, path and position are the same as those of the step S1; s4, continuing to etch the tested silicon wafer tested in the step S3 in the same way as the step S2; s5, cleaning is carried out after etching, Rz of the surface of the tested silicon wafer is continuously tested, data is recorded as Rz-3, and the testing method, path and position are the same as those of the step S1; and S6, according to the Rz-1, the Rz-2 and the Rz-3, determining the thickness DOD of the broken layer of the tested silicon wafer. Through the Rz test method, the number of samples is increased, the deviation of test results is reduced, and the accuracy of the test results is improved.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the technical field of single crystal silicon surface defect detection, and in particular to a method for testing the thickness of a silicon single crystal damaged layer. Background Art

[0002] Silicon material is an important semiconductor material. Due to its excellent performance, it is widely used in industries such as high-power transistors, rectifiers, integrated circuits, and silicon component materials. From silicon material to product, it needs to go through slicing, grinding, etching, polishing and other processes. The machining process will cause a certain thickness of mechanical damage layer on the surface of the silicon wafer. Subsequent acid-base treatment, physical and chemical polishing and other processes need to completely remove the mechanical damage layer while processing the surface flatness of the silicon wafer. If the damage layer is not completely removed, due to the large number of unsaturated bonds in the damage layer, the surface potential energy is large, and it is easy to adsorb the surrounding metal and non-metal particles, resulting in the performance of the semiconductor device being affected. Therefore, it is necessary to know the DOD of the silicon wafer surface, that is, the thickness of the damage layer, to avoid the subsequent process from being unable to completely remove the damage layer and to avoid affecting the quality of the final product.

[0003] In the prior art, for example, the Chinese invention patent with application number 202311358939.0 discloses a method for detecting the damaged layer of a silicon wafer, specifically, chromic acid solution and hydrofluoric acid chromic acid solution with a volume ratio of 1 to 10:1 are mixed into a detection solution, and the single crystal silicon wafer is anisotropically corroded in the mixed solution. Due to the large rate difference between the complete lattice and the damaged layer, the complete lattice will appear as a protruding "hill" on the surface of the corroded silicon wafer after corrosion, and the damaged part will be corroded into a concave "pit", and then the height difference between the protrusion and the concave is measured using a microscope to test the DOD. This detection method requires sampling during the test and special treatment of the sample block. It is impossible to perform non-destructive testing on large component materials, and due to the magnification of the microscope, the rationality of the location of the points also needs to be considered. At the same time, the number of points taken is relatively small relative to the area of ​​the sample block. For example, the Chinese invention patent with application number 202210352909.8 discloses a test method for the thickness of the surface damage layer of a <100> crystal orientation silicon single crystal polishing wafer. This test method is to continuously corrode multiple silicon wafers of the same specification in an alkaline solution for several times; obtain the cumulative corrosion thickness and each corrosion rate of each silicon wafer under test after each corrosion, and use the turning point of the corrosion rate as the marking point of the DOD test to test the DOD of the sample. During the test process of this test method, the point measurement method is used for measuring the thickness, and the amount of thickness data collected is insufficient. In addition, the corrosion rate is the average value of the entire sample, and the position variability before and after the test is large, so the error volatility of the test is also relatively high. Summary of the invention

[0004] In view of this, the present invention provides a method for testing the thickness of a silicon single crystal damaged layer to solve the technical problems of a small number of existing DOD test samples and a large deviation in test results.

[0005] The technical solution adopted by the present invention to solve its technical problem is: A method for testing the thickness of a silicon single crystal damage layer comprises the following steps: S1. Test the Rz of the surface of the silicon wafer under test and record the data as Rz-1, where Rz is the sum of the peaks and valleys of the microscopic profile of the surface of the silicon wafer under test; S2, etching the silicon wafer to be tested using acid or alkali solution; S3, after etching, cleaning is performed and Rz of the surface of the silicon wafer under test is continuously tested, and the data is recorded as Rz-2, wherein the test method, path and position are the same as those in step S1; S4, continuing to etch the silicon wafer tested in step S3 in the same manner as step S2; S5, after etching, cleaning is performed and the Rz of the surface of the silicon wafer under test is continued to be tested, and the data is recorded as Rz-3, wherein the test method, path and position are the same as those in step S1; S6. Determine the broken layer thickness DOD of the silicon wafer under test according to Rz-1, Rz-2 and Rz-3.

[0006] Preferably, in step S6, the following steps are used to determine the thickness DOD of the broken layer of the silicon wafer under test according to Rz-1, Rz-2 and Rz-3: S61. Use Rz-2 and Rz-3 to perform linear analysis, and record the slope between Rz-2 and Rz-3 as K; when the slope K ≥ -0.01, DOD = (Rz-1) - (Rz-3) μm; S62. When the slope K is less than -0.01, continue etching the silicon wafer under test and test Rz until the slope K between the n-1th and nth times satisfies ≥-0.01, and DOD = (Rz-1) - (Rz-n) μm.

[0007] Preferably, in step S1, if the silicon wafer to be tested is a large-scale component material, Rz is tested on key characteristic parts of the large-scale component material respectively.

[0008] Preferably, in step S1, a roughness meter is used to test Rz, wherein the test length lr=5-20 mm.

[0009] Preferably, the distance between adjacent test lines is less than 2 mm.

[0010] Preferably, multiple tests are performed in a direction perpendicular to the test line and in a diagonal direction to obtain multiple groups of Rz, and the maximum and minimum values ​​are removed, and the Rz of the remaining groups are averaged to obtain Rz-1.

[0011] Preferably, in step S2, etching the silicon wafer to be tested with acid or alkali solution adopts the following steps: S21, converting the surface of the silicon wafer to be tested into silicon dioxide by an oxidant; S22. Hydrofluoric acid is used to react with silicon dioxide to produce an acid-base neutralization reaction to eliminate silicon dioxide, thereby achieving the effect of removing the damaged layer on the surface without causing any damage.

[0012] Preferably, the oxidant is any one of nitric acid, chromium oxide and dichromic acid.

[0013] Preferably, a weak acid or water is added to the acid solution as a buffer.

[0014] Preferably, in step S2, a strong base such as sodium hydroxide, potassium hydroxide, sodium hydroxide tetramethylamine or the like is used, and water is added to the strong base for dilution to obtain an alkaline solution.

[0015] Compared with the prior art, the present invention has the following beneficial effects: The present invention first tests the Rz of the surface of the silicon wafer to be tested, and records the initial Rz value, i.e., Rz-1, and then etches the silicon wafer to be tested with an acid solution or an alkali solution, and then cleans and continues to test the Rz of the surface of the silicon wafer to be tested to obtain Rz-2; then, the silicon wafer to be tested is repeatedly etched and tested for Rz to obtain Rz-3, and Rz-2 and Rz-3 are used to determine whether the damaged layer has been completely etched and removed. When the damaged layer is completely removed, the thickness of the damaged layer is obtained according to Rz-1 and the final Rz value. Among them, Rz is the sum of the microscopic contour peaks and valleys of the surface of the silicon wafer to be tested. Therefore, to test the Rz value, it is necessary to sample the surface of the silicon wafer to be tested multiple times to obtain the sum of the maximum contour peak height and the maximum contour valley depth of the silicon wafer surface, thereby increasing the number of samples through the Rz test method, reducing the deviation of the test results, and improving the accuracy of the test results. Furthermore, the testing method of the present invention is not limited to an acid or alkali solution of a certain specific ratio, and has a low requirement for the life of the acid or alkali solution, which can avoid the deviation of the test results caused by the reduction of the etching solution life, ensure the usable value of historical data, further improve the accuracy of the test results, and provide a basis for the formulation of subsequent acid-base and physical and chemical polishing processes, so that the mechanical damage layer can be completely removed while processing the surface flatness of the silicon wafer in subsequent acid-base treatment, physical and chemical polishing and other processes, thereby ensuring the quality of the final product. BRIEF DESCRIPTION OF THE DRAWINGS

[0016] Figure 1 The figure is a flow chart of the method for testing the thickness of the silicon single crystal damaged layer of the present invention.

[0017] Figure 2 This is the test path of the roughness meter of the present invention.

[0018] Figure 3It is the DOD test data tested by professional instruments. DETAILED DESCRIPTION

[0019] The technical solutions and technical effects of the embodiments of the present invention are further described in detail below in conjunction with the accompanying drawings of the present invention.

[0020] Rz (sum of micro-profile peaks and valleys): the height of the sum of the maximum profile peak height and the maximum profile valley depth within the sampling length lr.

[0021] DOD (damage layer thickness): After silicon single crystal and polycrystalline materials have been mechanically processed by wire cutting, machining and other processes, the complete lattice structure on the surface has been destroyed. From the processed layer to the inside, it can be divided into an amorphous area, a cracked area, an elastic area and a complete area. The sum of the thickness of the amorphous area and the cracked area is the thickness of the damage layer.

[0022] Please see Figure 1 , a method for testing the thickness of a silicon single crystal damage layer, comprising the following steps: S1. Test the Rz of the surface of the silicon wafer under test and record the data as Rz-1, where Rz is the sum of the peaks and valleys of the microscopic profile of the surface of the silicon wafer under test; S2, etching the silicon wafer to be tested using acid or alkali solution; S3, after etching, cleaning is performed and Rz of the surface of the silicon wafer under test is continuously tested, and the data is recorded as Rz-2, wherein the test method, path and position are the same as those in step S1; S4, continuing to etch the silicon wafer tested in step S3 in the same manner as step S2; S5, after etching, cleaning is performed and the Rz of the surface of the silicon wafer under test is continued to be tested, and the data is recorded as Rz-3, wherein the test method, path and position are the same as those in step S1; S6. Determine the broken layer thickness DOD of the silicon wafer under test according to Rz-1, Rz-2 and Rz-3.

[0023] The present invention first tests the Rz of the surface of the silicon wafer to be tested, and records the initial Rz value, i.e., Rz-1, and then etches the silicon wafer to be tested with an acid solution or an alkali solution, and then cleans and continues to test the Rz of the surface of the silicon wafer to be tested to obtain Rz-2; then, the silicon wafer to be tested is repeatedly etched and tested for Rz to obtain Rz-3, and Rz-2 and Rz-3 are used to determine whether the damaged layer has been completely etched and removed. When the damaged layer is completely removed, the thickness of the damaged layer is obtained according to Rz-1 and the final Rz value. Among them, Rz is the sum of the microscopic contour peaks and valleys of the surface of the silicon wafer to be tested. Therefore, to test the Rz value, it is necessary to sample the surface of the silicon wafer to be tested multiple times to obtain the sum of the maximum contour peak height and the maximum contour valley depth of the silicon wafer surface, thereby increasing the number of samples through the Rz test method, reducing the deviation of the test results, and improving the accuracy of the test results. Furthermore, the testing method of the present invention is not limited to an acid or alkali solution of a certain specific ratio, and has a low requirement for the life of the acid or alkali solution, which can avoid the deviation of the test results caused by the reduction of the etching solution life, ensure the usable value of historical data, further improve the accuracy of the test results, and provide a basis for the formulation of subsequent acid-base and physical and chemical polishing processes, so that the mechanical damage layer can be completely removed while processing the surface flatness of the silicon wafer in subsequent acid-base treatment, physical and chemical polishing and other processes, thereby ensuring the quality of the final product.

[0024] Furthermore, if the silicon wafer to be tested is a large-scale component material, the Rz of the key characteristic parts of the large-scale component material is tested separately. Among them, the silicon wafer to be tested in the present invention can be a sample material or a large-scale component material. The large-scale component material refers to silicon single crystal products, such as solar panels, semiconductor devices, optical devices, etc. For the sample material, the Rz of the sample material can be tested directly. For large-scale component materials, their size is larger, and the key characteristic parts can be tested. The key characteristic parts are the key parts on the material, such as positioning holes, screw holes, etc. The Rz of testing large-scale component materials can be regarded as the accumulation of multiple sample test data, that is, each key characteristic part of the large-scale component material is a sample material, and the interval range of the sample is 5×5mm. Rz is tested separately for each sample material, and finally the Rz of the large-scale component material is accumulated, so that the large-scale component material can be tested without damage.

[0025] In the specific implementation process, the test of Rz on the surface of the silicon wafer to be tested includes: using a roughness meter to test Rz, wherein the test length lr=5-20mm. The roughness meter includes an inductive sensor, and a diamond stylus is installed at one end of the sensor measuring rod, and the tip curvature radius of the stylus is very small. During the test, the stylus is placed on the surface of the silicon wafer to be tested, and is in vertical contact with the surface of the silicon wafer to be tested, and the sensor is dragged at a certain speed by the driver. Due to the ups and downs of the surface profile of the silicon wafer to be tested, when the stylus slides on the surface of the silicon wafer, the stylus will move up and down. This movement will cause the inductance of the inductive coil to change synchronously, and then generate a signal proportional to the displacement of the stylus. After this signal is amplified and processed by an electronic device, data representing the surface roughness can be obtained, that is, the Rz value. Among them, the test length lr=5-20mm is to limit and weaken the influence of surface waviness on the measurement results. During the roughness meter measurement process, the stylus will make multiple points on the surface of the silicon wafer, which is equivalent to multiple sampling on the surface of the silicon wafer. Among them, one test line contains more than 1,000 single-point test data. Compared with the patent in the background technology, the sample volume is expanded by more than 6,000 times, thereby improving the accuracy of the Rz value test.

[0026] Furthermore, the distance between adjacent test lines is less than 2 mm. Figure 2 As shown, adjacent and mutually parallel test lines are adjacent test lines, and the distance between adjacent test lines is less than 2 mm, so as to ensure that the samples taken during the test cover the entire surface of the silicon wafer under test and the number of samples is sufficient.

[0027] Furthermore, multiple tests are performed in the direction perpendicular to the test line and the diagonal direction to obtain multiple groups of Rz, and the maximum and minimum values ​​are removed. The Rz of the remaining groups are averaged to obtain Rz-1. Specifically, Figure 2 As shown, for the surface of the silicon wafer under test, a total of 6 tests are performed in a direction perpendicular to the test line in a grid-like path, and then 2 tests are performed in a diagonal direction, for a total of 8 times. The maximum and minimum Rz values ​​of these 8 times are removed, and the Rz values ​​of the remaining 6 times are averaged to obtain Rz-1, thereby fully sampling the surface of the silicon wafer under test and obtaining a larger number of samples to reduce the error of the Rz value test, improve the accuracy of the Rz value test, and further improve the accuracy of the obtained DOD value.

[0028] In the specific implementation process, the following steps are used to etch the silicon wafer to be tested using acid or alkali: S21, converting the surface of the silicon wafer to be tested into silicon dioxide by an oxidant; wherein the oxidant used is any one of nitric acid, chromium oxide, and dichromic acid, and utilizing the oxidizing effect of the oxidant to convert silicon into silicon dioxide; S22, using hydrofluoric acid to react with silicon dioxide to produce an acid-base neutralization reaction to eliminate silicon dioxide, thereby removing the damaged surface layer without damage. Among them, the HF concentration is 49%, the HNO3 concentration is 70%, and the HOAC concentration is 99.8%.

[0029] Furthermore, adding a weak acid or water as a buffer to the acid solution can not only adjust the pH value of the solution, but also maintain the stability of the solution. Selecting a suitable buffer can improve the reliability and accuracy of subsequent tests.

[0030] Furthermore, in step S2, a strong base such as sodium hydroxide, potassium hydroxide, sodium hydroxide tetramethylamine is used, and water is added to the strong base for dilution to obtain an alkaline solution. The alkaline solution is used to chemically react with impurities on the surface of the polycrystalline silicon to cause a removal reaction, thereby removing excess impurities, and the mechanical damage layer on the surface of the silicon wafer can be removed by the alkaline solution.

[0031] Existing conventional detection methods generally use acid or alkali etching processes, and the process formula implementation range is relatively small. For example, the Chinese invention patent with application number 202311358939.0 uses a detection solution made of chromic acid solution and hydrofluoric acid chromic acid solution with a volume ratio of 1 to 10:1 when detecting the damaged layer of silicon wafers. Therefore, the patent needs to be prepared strictly in accordance with the requirements during use. When the composition and ratio of the acid solution change, the test results will also change accordingly, but the patent does not explain this problem and propose corresponding improvement measures. Secondly, the acid or alkali solution has a service life. As the reaction time is delayed, its reaction ability will also decrease, resulting in a decrease in the reference value of previous historical data. The test method of the present invention has lower requirements for the ratio and life of the acid or alkali solution, which can avoid the deviation of the test results caused by the reduction of the etching solution life, and ensure the usable value of historical data.

[0032] In the specific implementation process, the following steps are used to determine the broken layer thickness DOD of the silicon wafer under test according to Rz-1, Rz-2, and Rz-3: S61. Use Rz-2 and Rz-3 to perform linear analysis, and record the slope between Rz-2 and Rz-3 as K; when the slope K ≥ -0.01, DOD = (Rz-1) - (Rz-3) μm; S62. When the slope K is less than -0.01, continue etching the silicon wafer under test and test Rz until the slope K between the n-1th and nth times satisfies ≥-0.01, and DOD = (Rz-1) - (Rz-n) μm.

[0033] Specifically, a linear analysis is performed on Rz-2 and Rz-3 to determine the linear relationship between Rz-2 and Rz-3, thereby obtaining the slope K between Rz-2 and Rz-3. When the slope K ≥ -0.01, it indicates that the surface of the silicon wafer has been etched to the elastic region, and the amorphous region and the crack region have been removed, that is, the damaged layer of the silicon wafer has been etched away, and the difference between the measured Rz value and Rz-1 at this time is the thickness DOD of the damaged layer. Example

[0034] The Rz value of the surface of the silicon wafer under test is tested by using a roughness meter, and Rz-1 is obtained as shown in No. 1 of Table 1, and Rz-1 is 0.4121; the silicon wafer under test is etched with acid or alkali solution, and after etching, it is cleaned and the Rz of the surface of the silicon wafer under test is continuously tested, and the data is recorded as Rz-2 as shown in No. 2 of Table 1, and Rz-2 is 0.3288, wherein the test method, path and position are the same as before; the silicon wafer under test is continuously etched after the test; after etching, it is cleaned and continued The Rz on the surface of the silicon wafer under test is tested, and the data recorded is Rz-3 as shown in No. 3 in Table 1. Rz-3 is 02492, wherein the test method, path and position are the same as the previous steps. Linear analysis is performed using Rz-2 and Rz-3, and the slope K between Rz-2 and Rz-3 is calculated, and K is obtained to be -0.0833. Since -0.0833<-0.01, the requirement is not met, and it is necessary to continue etching the silicon wafer under test and test Rz to obtain the Rz value and K value shown in Table 1.

[0035] Table 1

[0036] It can be seen from Table 1 that the linear slope of the two groups of data Rz-5 and Rz-6 is -0.0098>-0.01, which meets the requirements, so DOD=(Rz-1)-(Rz-6)=0.4121-0.1544=0.2577μm.

[0037] Comparative Example Use existing professional and authoritative instruments to test the DOD of silicon wafers. The test results are as follows: Figure 3 As shown, it can be seen that the DOD measured by the instrument is about 0.2533, and the DOD measured by the method of the present invention is 0.2577, and the two values ​​are not much different. It can be explained that the DOD data measured by the method of the present invention is close to the DOD data measured by the professional instrument. Therefore, although the test method of the present invention is simple, the test result has a small error and high accuracy.

[0038] What is disclosed above is only a preferred embodiment of the present invention, which certainly cannot be used to limit the scope of rights of the present invention. A person skilled in the art can understand that all or part of the processes of the above embodiments and equivalent changes made according to the claims of the present invention still fall within the scope of the invention.

Claims

1. A method for testing the thickness of a silicon single crystal damage layer, characterized in that: The following steps are involved: S1. Test the Rz of the surface of the silicon wafer under test and record the data as Rz-1, where Rz is the sum of the peaks and valleys of the microscopic profile of the surface of the silicon wafer under test; S2, etching the silicon wafer to be tested using acid or alkali solution; S3, after etching, cleaning is performed and Rz of the surface of the silicon wafer under test is continuously tested, and the data is recorded as Rz-2, wherein the test method, path and position are the same as those in step S1; S4, continuing to etch the silicon wafer tested in step S3 in the same manner as step S2; S5, after etching, cleaning is performed and the Rz of the surface of the silicon wafer under test is continued to be tested, and the data is recorded as Rz-3, wherein the test method, path and position are the same as those in step S1; S6. Determine the broken layer thickness DOD of the silicon wafer under test according to Rz-1, Rz-2 and Rz-3.

2. The method for testing the thickness of a silicon single crystal damaged layer according to claim 1, characterized in that: In step S6, the following steps are used to determine the thickness DOD of the broken layer of the silicon wafer under test according to Rz-1, Rz-2, and Rz-3: S61. Use Rz-2 and Rz-3 to perform linear analysis, and record the slope between Rz-2 and Rz-3 as K; when the slope K ≥ -0.01, DOD = (Rz-1) - (Rz-3) μm; S62. When the slope K is less than -0.01, continue etching the silicon wafer under test and test Rz until the slope K between the n-1th and nth times satisfies ≥-0.01, and DOD = (Rz-1) - (Rz-n) μm.

3. The method for testing the thickness of a silicon single crystal damaged layer according to claim 1, characterized in that: In step S1, if the silicon wafer to be tested is a large component material, Rz is tested on key characteristic parts of the large component material respectively.

4. The method for testing the thickness of a silicon single crystal damaged layer according to claim 1, characterized in that: In step S1, a roughness meter is used to test Rz, wherein the test length lr=5-20 mm.

5. The method for testing the thickness of a silicon single crystal damaged layer according to claim 4, characterized in that: The distance between adjacent test lines is less than 2mm.

6. The method for testing the thickness of a silicon single crystal damaged layer according to claim 5, characterized in that: Perform multiple tests in the direction perpendicular to the test line and in the diagonal direction to obtain multiple groups of Rz. Remove the maximum and minimum values, and take the average of the remaining groups' Rz to obtain Rz-1.

7. The method for testing the thickness of the silicon single crystal crushing layer according to claim 1, characterized in that: In step S2, etching the silicon wafer to be tested with acid or alkali solution is performed by the following steps: S21, converting the surface of the silicon wafer to be tested into silicon dioxide by an oxidant; S22. Hydrofluoric acid is used to react with silicon dioxide to produce an acid-base neutralization reaction to eliminate silicon dioxide, thereby achieving the effect of removing the damaged layer on the surface without causing any damage.

8. The method for testing the thickness of the silicon single crystal crushing layer according to claim 7, characterized in that: The oxidant is any one of nitric acid, chromium oxide and dichromic acid.

9. The method for testing the thickness of the silicon single crystal crushing layer according to claim 8, characterized in that: Add weak acid or water to the acid solution as a buffer.

10. The method for testing the thickness of the silicon single crystal crushing layer according to claim 1, characterized in that: In step S2, a strong base such as sodium hydroxide, potassium hydroxide, sodium hydroxide tetramethylamine or the like is used, and water is added to the strong base for dilution to obtain an alkaline solution.