Writing feeling improving film with protective film
By controlling the relationship between the linear expansion coefficients of the writing feel improvement film and the protective film, the curling problem caused by temperature changes was solved, ensuring the quality and performance of the writing feel improvement film.
Patent Information
- Application Number
- CN202280094534.8
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Priority Date
- 2022-03-31
- Filing Date
- 2022-12-02
- Publication Date
- 2024-11-15
AI Technical Summary
During the manufacturing, storage, handling, and processing of the writing feel improvement film, curling issues caused by temperature changes affect the quality of the film.
By controlling the writing feel, the relationship between the linear expansion coefficients of the film and the protective film is improved, so that they satisfy the relationship within a specific range (-6.5 < (α-β) < 6.5), in order to suppress curling caused by temperature changes.
It effectively suppresses curling caused by temperature changes, maintains the writing feel, and improves the quality and performance of the film.
Smart Images

Figure CN118973815A_ABST
Abstract
Description
Technical Field
[0001] The present invention relates to a writing feel improving film with a protective film obtained by laminating a protective film on a writing feel improving film used to improve the writing feel of a stylus pen in a touch panel or the like. Background Art
[0002] In recent years, image display devices (touch panels) with a position detection function that serve as both a display device and an input unit are often used in various electronic devices.
[0003] For such a touch panel, it has been studied to attach a film for improving the writing feeling of a stylus pen (hereinafter referred to as a “writing feeling improving film”) to the outermost surface of the touch panel.
[0004] Regarding the writing feel improving film, for example, disclosed are: a writing feel improving film having a writing feel improving layer having a specific friction force (Patent Document 1); an anti-glare hard coating film for a touch panel that specifies the pen tip resistance and the oleic acid contact angle of a stylus pen (Patent Document 2); a transparent film having a specific total light transmittance and a specific maximum height of a rolling waviness curve (Patent Document 3); a tactile film comprising linear protrusions forming a mesh structure (Patent Document 4); a transparent laminated film having a surface shape having a specific maximum height of a rolling waviness curve and an arithmetic mean roughness (Patent Document 5), etc.
[0005] However, these documents do not describe a laminated body in which a protective film is laminated on a writing feel improving film.
[0006] Prior art literature
[0007] Patent Literature
[0008] Patent document 1: WO2020 / 122172 (US2022 / 0033600A1)
[0009] Patent Document 2: Japanese Patent Application Publication No. 2014-232276
[0010] Patent Document 3: Japanese Patent Application Publication No. 2014-97649 (US 2015 / 0291828A1)
[0011] Patent Document 4: Japanese Patent Application Publication No. 2015-54417
[0012] Patent Document 5: Japanese Patent Application Publication No. 2016-196113 (US2018 / 0030229A1) Summary of the invention
[0013] Problems to be solved by the invention
[0014] After the writing feel improving film is manufactured, it is stored, transported, processed, etc. Therefore, for the purpose of protecting the surface of the writing feel improving film until the writing feel improving film is used for a touch panel, a protective film is sometimes pre-pasted (laminated) on the surface of the film. In addition, the writing feel improving film with a protective film laminated on the surface (hereinafter referred to as "the writing feel improving film with a protective film") is sometimes also exposed to a high temperature state (40 to 60°C) for a long time during storage and transportation, or is processed at a high temperature state (50 to 90°C) during processing. Due to the application of such temperature changes, the film curls, thereby causing a problem of reduced quality of the writing feel improving film.
[0015] The present invention has been made in view of such actual conditions, and an object of the present invention is to provide a writing feel improving film with a protective film in which the occurrence of curling due to temperature change is suppressed.
[0016] Means used to solve problems
[0017] In order to solve the above problems, the inventors of the present invention have conducted intensive research on a writing feel improving film with a protective film. As a result, they found that by increasing the linear expansion coefficient α (×10 -5 / K) and the linear expansion coefficient of the protective film β(×10 -5 / K) have a specific relationship, so that the problem can be solved, thereby completing the present invention.
[0018] Therefore, according to the present invention, the writing feel improving film with a protective film as described below [1] to [6] can be provided.
[0019] [1] A writing feel improving film with a protective film, wherein a protective film is laminated on at least one side of a writing feel improving film having a writing feel improving film substrate layer and a writing feel improving layer, wherein:
[0020] The linear expansion coefficient of the writing feel improving film is α(×10 -5 / K), the linear expansion coefficient of the protective film is set to β(×10 -5 / K), the formula is satisfied: -6.5<(α-β)<6.5.
[0021] [2] The writing feel improving film with a protective film according to [1], wherein the protective film is laminated on the writing feel improving layer side of the writing feel improving film.
[0022] [3] A writing feel improving film with a protective film according to [1] or [2], wherein the protective film has an adhesive layer and a protective film substrate layer, and the writing feel improving film with a protective film is laminated in such a way that at least one side of the writing feel improving film is in contact with the adhesive layer of the protective film.
[0023] [4] The writing feel improving film with a protective film according to [1] or [2], wherein the linear expansion coefficient of the writing feel improving film is set to α (×10 -5 / K), the linear expansion coefficient of the protective film is set to β(×10 -5 / K), the formula is satisfied: -1.0<(α-β)<1.0.
[0024] [5] The writing feel improving film with a protective film according to [1] or [2], wherein the linear expansion coefficient of the writing feel improving film is α (×10 -5 / K) is 1.5 or more and 8.0 or less (×10 -5 / K).
[0025] [6] The writing feel improving film with a protective film according to [1] or [2], wherein the interlayer peeling force between the writing feel improving film and the protective film is 800 mN / 25 mm or less.
[0026] Effects of the Invention
[0027] According to the writing feel-improving film with a protective film of the present invention, the occurrence of curling due to temperature changes during storage, transportation, processing, etc. can be suppressed, and therefore, the quality of the writing feel-improving film can be maintained. BRIEF DESCRIPTION OF THE DRAWINGS
[0028] Figure 1 This is a schematic diagram showing an example of the layer structure of the writing feel improving film with a protective film of the present invention.
[0029] Figure 2 is a diagram illustrating the maximum height of curl. DETAILED DESCRIPTION
[0030] The writing feel improving film with a protective film of the present invention is a writing feel improving film with a protective film laminated on at least one side of a writing feel improving film having a writing feel improving film substrate layer and a writing feel improving layer, and is characterized in that:
[0031] The linear expansion coefficient of the writing feel improving film is α(×10 -5 / K), the linear expansion coefficient of the protective film is set to β(×10 -5 / K), the formula is satisfied: -6.5<(α-β)<6.5.
[0032] Hereinafter, the writing feel improving film with a protective film of the present invention will be described in detail.
[0033] 1) Film for improving writing feel
[0034] The writing feel-improving film according to the present embodiment includes a writing feel-improving film base material layer and a writing feel-improving layer.
[0035] (1) Writing feel improvement film substrate layer
[0036] The writing feel improving film base material layer according to this embodiment has a function of supporting the writing feel improving layer.
[0037] As the material of the writing feel improving film substrate layer, a transparent material can be appropriately selected from conventionally known materials for optical substrates and used.
[0038] Examples thereof include polyester films such as polyethylene terephthalate films, polybutylene terephthalate films, and polyethylene naphthalate films; polyolefin films such as polyethylene films and polypropylene films; cellulose diacetate films, cellulose triacetate films, cellulose acetate butyrate films, polyvinyl chloride films, polyvinylidene chloride films, polyvinyl alcohol films, ethylene-vinyl acetate copolymer films, polystyrene films, polycarbonate films, polymethylpentene films, polysulfone films, polyetheretherketone films, polyethersulfone films, polyetherimide films, polyimide films, fluororesin films, polyamide films, acrylic resin films, polyurethane resin films, norbornene-based polymer films, cyclic olefin-based polymer films, cyclic conjugated diene-based polymer films, vinyl alicyclic hydrocarbon polymer films, polyphenylene sulfide films, and liquid crystal polymer films; cellophane; glass; and laminated films thereof.
[0039] Among them, in combination with the writing feel improving layer, from the viewpoint of being able to well maintain the writing feel of the stylus pen, preferred are polyethylene terephthalate films, polycarbonate films, acrylic resin films, norbornene-based polymer films, and particularly preferred are polyethylene terephthalate films, polycarbonate films, polymethyl methacrylate films, and composite substrates thereof.
[0040] The writing feel improving film substrate layer may be subjected to surface treatment by oxidation, embossing, or the like, primer treatment, or the like on one or both sides as desired in order to improve adhesion with layers (writing feel improving layer, adhesive layer, etc.) provided on the surface thereof.
[0041] Examples of the oxidation method include corona discharge treatment, plasma discharge treatment, chromating treatment (wet method), flame treatment, hot air treatment, and ozone / ultraviolet treatment.
[0042] Examples of the roughening method include a sandblasting method and a solvent treatment method.
[0043] The primer treatment can be performed by a known method such as coating an adhesive resin material on the surface of the writing feel improving film substrate layer.
[0044] These surface treatments and the like may be appropriately selected according to the material of the base material layer and the like.
[0045] From the perspective of appropriately supporting the writing feel improving layer, processability, protection of the touch panel, and durability against writing with a stylus pen, the thickness of the writing feel improving film substrate layer is preferably 30 to 300 μm, more preferably 90 to 250 μm, particularly preferably 120 to 220 μm, and further preferably 150 to 200 μm.
[0046] (2) Writing feel improvement layer
[0047] The writing feel improving layer described in this embodiment has a function of improving the writing feel of the stylus pen.
[0048] Here, "improving the writing feel of the stylus pen" means that when writing on the writing feel improvement layer with the stylus pen, the vibration feeling (vibration feeling) when writing on paper with a ballpoint pen can be reproduced, and the resistance feeling (degree of friction) when writing on paper with a ballpoint pen can be reproduced (resistance feeling).
[0049] The writing feel-improving layer can be formed using a composition for forming a writing feel-improving layer.
[0050] The writing feel improving layer-forming composition can be prepared by, for example, mixing a curable component, fine particles, a surface conditioner, and the like.
[0051] (2-1) Curable Component
[0052] The composition for forming a writing feel improving layer according to the present embodiment preferably contains a curable component as a main component.
[0053] The curable component is a component that is cured by active energy rays such as visible light, ultraviolet rays, electron beams, heat, etc. Examples thereof include active energy ray-curable components and thermosetting components.
[0054] Among them, active energy ray-curable components are preferably used from the viewpoints of the hardness of the formed writing feel improving layer, the heat resistance of the writing feel improving film substrate layer, and the effect of reducing the linear expansion coefficient α of the writing feel improving film. The writing feel improving film provided with such a writing feel improving layer is easy to exhibit an excellent anti-curling effect by combining it with a protective film.
[0055] As active energy ray-curable components, multifunctional (meth)acrylate monomers, (meth)acrylate prepolymers, active energy ray-curable polymers, etc. can be cited. Among them, from the perspective of having a specified hardness and being able to improve the writing feel of the stylus pen, multifunctional (meth)acrylate monomers and / or (meth)acrylate prepolymers are preferred, and multifunctional (meth)acrylate monomers are more preferred. By using a writing feel improvement layer made of such a material in combination with a protective film, an excellent anti-curling effect can be easily exerted.
[0056] The polyfunctional (meth)acrylate monomer and the (meth)acrylate prepolymer may be used alone or in combination.
[0057] It should be noted that, in this specification, (meth)acrylate refers to acrylate and / or methacrylate. The same applies to other similar terms.
[0058] Examples of the multifunctional (meth)acrylate monomer include 1,4-butanediol di(meth)acrylate, 1,6-hexanediol di(meth)acrylate, neopentyl glycol di(meth)acrylate, polyethylene glycol di(meth)acrylate, hydroxypivalate neopentyl glycol di(meth)acrylate, dicyclopentyl di(meth)acrylate, caprolactone-modified dicyclopentenyl di(meth)acrylate, ethylene oxide-modified phosphoric acid di(meth)acrylate, allylated cyclohexyl di(meth)acrylate, isocyanurate di(meth)acrylate, trimethylolpropane tri(meth)acrylate, and polyisocyanurate. Polyfunctional (meth)acrylates include polyfunctional (meth)acrylates such as propionic acid-modified dipentaerythritol tri(meth)acrylate, pentaerythritol tri(meth)acrylate, propionic acid-modified dipentaerythritol tri(meth)acrylate, pentaerythritol tri(meth)acrylate, propylene oxide-modified trimethylolpropane tri(meth)acrylate, tri(acryloyloxyethyl)isocyanurate, pentaerythritol tetra(meth)acrylate, propionic acid-modified dipentaerythritol penta(meth)acrylate, dipentaerythritol hexa(meth)acrylate, ethylene oxide-modified dipentaerythritol hexa(meth)acrylate, and caprolactone-modified dipentaerythritol hexa(meth)acrylate.
[0059] These can be used alone or in combination of two or more.
[0060] Examples of the (meth)acrylate prepolymer include polyester acrylate-based, epoxy acrylate-based, urethane acrylate-based, and polyol acrylate-based prepolymers.
[0061] The polyester acrylate prepolymer can be obtained by esterifying the hydroxyl groups of a polyester oligomer having hydroxyl groups at both ends obtained by condensation of a polycarboxylic acid and a polyol with (meth)acrylic acid, or by esterifying the terminal hydroxyl groups of an oligomer obtained by adding an alkylene oxide to a polycarboxylic acid with (meth)acrylic acid.
[0062] The epoxy acrylate prepolymer can be obtained by reacting (meth)acrylic acid with the oxirane ring of a bisphenol epoxy resin or a novolac epoxy resin having a relatively low molecular weight to form an ester.
[0063] The urethane acrylate prepolymer can be obtained by esterifying a polyurethane oligomer obtained by a reaction of a polyether polyol or a polyester polyol with a polyisocyanate with (meth)acrylic acid.
[0064] The polyol acrylate prepolymer can be obtained by esterifying the hydroxyl group of polyether polyol with (meth)acrylic acid.
[0065] These prepolymers may be used alone or in combination of two or more.
[0066] (2-2) Microparticles
[0067] The composition for forming the writing feel improvement layer described in this embodiment preferably contains microparticles. By containing microparticles, the surface of the writing feel improvement layer formed is appropriately roughened, and the average value, maximum value, minimum value, and standard deviation of the friction force described later are easily adjusted to the desired range. As a result, the obtained writing feel improvement film can show a moderate sense of friction and vibration when writing on the writing feel improvement layer with a stylus pen, and can well reproduce the writing feel when writing on paper with a ballpoint pen. In addition, by easily reducing the linear expansion coefficient α of the writing feel improvement film, especially in combination with a protective film, it is easy to exert an excellent anti-curling effect.
[0068] The above-mentioned microparticles refer to particles having an average particle size larger than the silica nanoparticles described later. For example, the average particle size of the microparticles is preferably 1 to 20 μm, more preferably 3 to 18 μm, particularly preferably 6 to 16 μm, further preferably 8 to 14 μm, and further preferably 10 to 12 μm. By using microparticles having an average particle size in the above-mentioned range, it is easy to adjust the average value, maximum value, minimum value, and standard deviation of the friction force described later to the desired range, and give the writing feel improvement layer a moderate sense of friction and vibration, so as to reproduce the writing feel when writing on paper with a ballpoint pen. In addition, it is easy to reduce the linear expansion coefficient α of the writing feel improvement film, especially by combining it with a protective film, so that it is easy to exert an excellent anti-curling effect.
[0069] The average particle size of the fine particles is a value measured using a laser diffraction scattering particle size distribution analyzer using a few drops of a 5 mass % dispersion prepared using methyl ethyl ketone as a dispersion medium as a sample.
[0070] The microparticles may be inorganic microparticles or organic microparticles, or may be resin microparticles having both inorganic and organic properties. Among them, from the viewpoint of the hardness of the formed writing feel improving layer and the viewpoint of easily reducing the linear expansion coefficient α of the writing feel improving film, inorganic microparticles or resin microparticles having both inorganic and organic properties are preferred, and resin microparticles having both inorganic and organic properties are particularly preferred.
[0071] Examples of the inorganic fine particles include fine particles made of silica, alumina, titania, zirconium oxide, tin oxide, indium oxide, cadmium oxide, antimony oxide, etc. Among these, silica fine particles are preferred.
[0072] As organic microparticles, melamine resin microparticles, acrylic resin microparticles (e.g., polymethyl methacrylate resin microparticles, etc.), acrylic-styrene copolymer microparticles, polycarbonate microparticles, polyethylene microparticles, polystyrene microparticles, benzoguanamine resin microparticles, etc. can be listed. The resin constituting the resin microparticles may be cross-linked. Among these, acrylic resin microparticles are preferred, and polymethyl methacrylate resin microparticles are more preferred from the viewpoint of optical properties and hardness.
[0073] As the resin fine particles having both inorganic and organic properties, silicone fine particles (for example, Tospar series manufactured by Momentive Corporation) are suitable.
[0074] In order to further improve dispersibility, it is also preferred that the surface of the microparticles is modified with a surface modifier.
[0075] In addition, the shape of the particles can be spherical or non-spherical. In the case of non-spherical, the shape can be irregular, or a shape with a large aspect ratio such as a needle or a scale. It should be noted that in this specification, "irregular shape" is not a regular shape such as a spherical or elliptical shape, but an irregular shape with multiple corners or faces.
[0076] Regarding the obtained writing feel-improving layer, the shape of the microparticles is preferably spherical, and particularly preferably true spherical, from the viewpoint of easily adjusting the average value, maximum value, minimum value, and standard deviation of the frictional force described later to the desired range and from the viewpoint of easily reducing the linear expansion coefficient α of the writing feel-improving film.
[0077] The fine particles may be used alone or in combination of two or more.
[0078] The content of the microparticles in the composition for forming the writing feel improving layer is preferably 0.1 to 20 parts by mass, more preferably 0.5 to 17 parts by mass, particularly preferably 1 to 14 parts by mass, further preferably 3 to 12 parts by mass, and particularly preferably 6 to 11 parts by mass, relative to 100 parts by mass of the curable component. By making the content of the microparticles within the above range, it is easy to adjust the average value, maximum value, minimum value, and standard deviation of the friction force of the obtained writing feel improving layer described later to the desired range, and it is easy to reduce the linear expansion coefficient α of the writing feel improving film. In particular, by combining with a protective film, it is easy to exert an excellent anti-curling effect.
[0079] (2-3) Surface Conditioner
[0080] The composition for forming a writing feel improving layer according to the present embodiment preferably contains a surface conditioner.
[0081] By containing a surface regulator, the occurrence of stripe defects and unevenness in the formed writing feel improvement layer is suppressed. As a result, the film thickness becomes uniform, the writing feel improvement film presents a more excellent appearance, and is easy to have the desired optical properties (haze value and total light transmittance, etc.). In addition, the surface of the writing feel improvement layer of the writing feel improvement film is easy to present a good surface state, so it is easy to adjust the average value, maximum value, minimum value, and standard deviation of the friction force described later to the desired range, which can make the writing feel of the writing feel improvement layer better. In addition, it is easy to reduce the linear expansion coefficient α of the writing feel improvement film, especially by combining it with a protective film, so that it is easy to exert an excellent anti-curling effect.
[0082] Examples of the surface conditioner include silicone-based surface conditioners consisting of silicone-based polymers, fluorine-based surface conditioners consisting of fluorine-based polymers, acrylic-based surface conditioners consisting of acrylic-based polymers, and vinyl-based surface conditioners consisting of vinyl-based polymers.
[0083] Here, silicone polymer refers to a polymer mainly containing polysiloxane chains, and fluorine polymer refers to a polymer having a fluorine-substituted monomer as a main monomer unit. In addition, acrylic polymer refers to a polymer having an acrylic ester as a main monomer unit. And, vinyl polymer refers to a polymer containing a monomer having a vinyl group as a main monomer unit.
[0084] The surface conditioner may be used alone or in combination of two or more.
[0085] Among these, silicone-based surface conditioners and fluorine-based surface conditioners are preferred from the viewpoint of surface conditioning performance and compatibility with other components.
[0086] As the silicone-based surface conditioner, a surface conditioner composed of polydimethylsiloxane or modified polydimethylsiloxane is preferred, and a surface conditioner composed of polydimethylsiloxane is more preferred.
[0087] As the fluorine-based surface conditioning agent, it is preferably a surface conditioning agent containing a fluorine-based polymer having a perfluoroalkyl group or a fluorinated alkenyl group in the main chain or the side chain. As commercially available products, BYK-340 manufactured by Bicchemigapan, Fattener 650A manufactured by Neos, Megafax RS-75 manufactured by DIC, Megafax RS-90 manufactured by DIC, V-8FM manufactured by Osaka Organic Chemical Industry Co., Ltd., etc. can be preferably listed, but are not limited to them.
[0088] When the composition for forming the writing feel improvement layer contains a surface conditioner, the content of the surface conditioner in the composition for forming the writing feel improvement layer is preferably 0.01 to 10 parts by mass, more preferably 0.1 to 5 parts by mass, particularly preferably 0.5 to 3 parts by mass, and further preferably 0.8 to 2 parts by mass relative to 100 parts by mass of the curable component. By making the content of the surface conditioner within the above range, the appearance of the writing feel improvement film can be made better. In addition, it is easy to adjust the average value, maximum value, minimum value, and standard deviation of the friction force described later to the desired range, so that the writing feel of the writing feel improvement layer can be made better.
[0089] (2-4) Other ingredients
[0090] The composition for forming the writing feel improving layer may further contain other components in addition to the above components. Examples of other components include silicon dioxide nanoparticles, photopolymerization initiators, ultraviolet absorbers, antioxidants, light stabilizers, antistatic agents, silane coupling agents, antioxidants, thermal polymerization inhibitors, surfactants, storage stabilizers, plasticizers, lubricants, defoamers, organic fillers, wettability improvers, and coating surface improvers.
[0091] By making the composition for forming the writing feel improving layer contain silica nanoparticles, the hardness and scratch resistance of the formed writing feel improving layer can be effectively improved, and further, curling can be easily suppressed. In addition, the optical properties (haze value and total light transmittance, etc.) of the writing feel improving film can be improved, and the occurrence of roughness when using the writing feel improving film can be effectively suppressed.
[0092] The average particle size of the silica nanoparticles is preferably 1 to 300 nm, more preferably 5 to 100 nm, and particularly preferably 10 to 50 nm.
[0093] The average particle size of the silica nanoparticles can be measured using a laser diffraction scattering particle size distribution analyzer.
[0094] The silica nanoparticles may be in the form of an organosol (colloidal). The organosol form improves the dispersibility of the silica nanoparticles and improves the homogeneity and light transmittance of the formed writing feel improving layer.
[0095] When the composition for forming a writing feel improving layer contains silica nanoparticles, the content of the silica nanoparticles in the composition for forming a writing feel improving layer is preferably 5 to 50 parts by mass, more preferably 10 to 35 parts by mass, and particularly preferably 15 to 25 parts by mass based on 100 parts by mass of the curable component.
[0096] By setting the blending ratio of the silica nanoparticles to the above range, the homogeneity and light transmittance of the formed writing feel improving layer can be maintained more satisfactorily.
[0097] When the composition for forming a writing feel improving layer contains an active energy ray-curable component as a curable component, it is preferable to further contain a photopolymerization initiator. By containing a photopolymerization initiator, the curing reaction by irradiation with active energy rays can be more easily performed.
[0098] Examples of the photopolymerization initiator used include benzoin, benzoin methyl ether, benzoin ethyl ether, benzoin isopropyl ether, benzoin n-butyl ether, benzoin isobutyl ether, acetophenone, dimethylaminoacetophenone, 2,2-dimethoxy-2-phenylacetophenone, 2,2-diethoxy-2-phenylacetophenone, 2-hydroxy-2-methyl-1-phenylpropane-1-one, 1-hydroxycyclohexyl phenyl ketone, 2-methyl-1-[4-(methylthio)phenyl]-2-morpholino-propane-1 -ketone, 4-(2-hydroxyethoxy)phenyl-2(hydroxy-2-propyl)ketone, benzophenone, p-phenylbenzophenone, 4,4'-diethylaminobenzophenone, dichlorobenzophenone, 2-methylanthraquinone, 2-ethylanthraquinone, 2-tert-butylanthraquinone, 2-aminoanthraquinone, 2-methylthioxanthone, 2-ethylthioxanthone, 2-chlorothioxanthone, 2,4-dimethylthioxanthone, 2,4-diethylthioxanthone, benzyl dimethyl ketal, acetophenone dimethyl ketal, p-dimethylaminobenzoate, etc. These may be used alone or in combination of two or more.
[0099] When the composition for forming a writing feel improving layer contains a photopolymerization initiator, the content of the photopolymerization initiator in the composition for forming a writing feel improving layer is preferably 1 to 20 parts by mass, more preferably 2 to 10 parts by mass, based on 100 parts by mass of the curable component, from the viewpoint of the effect of adding the photopolymerization initiator.
[0100] The writing feel improving layer-forming composition may contain a solvent for the purpose of improving coating properties, adjusting viscosity, adjusting solid content concentration, and the like.
[0101] The solvent used is not particularly limited as long as the curing components and the like are dissolved and the microparticles and the like are dispersed. Specific examples of the solvent include alcohols such as methanol, ethanol, isopropanol, butanol, and octanol; ketones such as acetone, methyl ethyl ketone, methyl isobutyl ketone, and cyclohexanone; esters such as ethyl acetate, butyl acetate, ethyl lactate, and γ-butyrolactone; ethers such as ethylene glycol monomethyl ether (methyl cellosolve), ethylene glycol monoethyl ether (ethyl cellosolve), diethylene glycol monobutyl ether (butyl cellosolve), and propylene glycol monomethyl ether; aromatic hydrocarbons such as benzene, toluene, and xylene; amides such as N,N-dimethylformamide, N,N-dimethylacetamide, and N-methylpyrrolidone; and the like.
[0102] These solvents can be used alone or in combination of two or more.
[0103] The content of the solvent is preferably in the range of 10 to 300 parts by mass, more preferably 30 to 200 parts by mass, based on 100 parts by mass of the curable component.
[0104] (3) Method for forming writing feel improving layer
[0105] The writing feel-improving layer can be formed by applying the writing feel-improving layer-forming composition on the writing feel-improving film base layer to a desired film thickness, and drying and curing the resulting coating.
[0106] As a method for applying the composition for forming a writing feel improving layer, a conventionally known coating method such as a bar coating method, a knife coating method, a roll coating method, a plate coating method, a die coating method, a gravure coating method, etc. can be used.
[0107] The drying temperature of the coating film of the obtained writing feel improving layer-forming composition is usually 40 to 120° C., and the drying time is usually about 30 seconds to 5 minutes.
[0108] When the curable component in the writing feel improving layer-forming composition is active energy ray-curable, the coating film of the writing feel improving layer-forming composition can be cured by irradiating the coating film with active energy rays such as ultraviolet rays and electron beams.
[0109] Ultraviolet irradiation can be performed using a high-pressure mercury lamp, an H lamp manufactured by Heleus, Inc., a xenon lamp, or the like. The amount of ultraviolet irradiation is preferably an illuminance of 50 to 1000 mW / cm 2 , Light intensity 50~1000mJ / cm 2 , more preferably 100 to 500 mW / cm 2 , Light intensity 100~500mJ / cm 2 .
[0110] The electron beam irradiation can be performed using an electron beam accelerator or the like, and the irradiation amount of the electron beam is preferably about 10 to 1000 krad.
[0111] When the curable component in the writing feel improving layer-forming composition has thermosetting properties, the coating film of the writing feel improving layer-forming composition can be cured by heating the coating film at a predetermined temperature for a predetermined time.
[0112] The thickness of the writing feel improving layer is not particularly limited, but is preferably 0.8 to 30 μm, more preferably 1 to 20 μm or more, particularly preferably 2 to 15 μm, further preferably 3 to 12 μm, preferably 4 to 10 μm, and most preferably 5 to 8 μm. By making the thickness of the writing feel improving layer within the above range, the writing feel when writing on paper with a ballpoint pen can be reproduced more well. In addition, it is easy to reduce the linear expansion coefficient α of the writing feel improving film, and especially by combining it with a protective film, it is easy to exert an excellent anti-curling effect.
[0113] In the writing feel improving film with a protective film of the present invention, the linear expansion coefficient α (×10 -5 / K) and the linear expansion coefficient β (×10 -5 / K) needs to satisfy the formula: -6.5<(α-β)<6.5.
[0114] As long as the linear expansion coefficient α of the writing feel improving film is equal to the linear expansion coefficient β of the protective film described later (×10 -5 / K) satisfies the formula: -6.5<(α-β)<6.5, and is not particularly limited, but is usually greater than 0 and less than 50 (×10 -5 / K), preferably 1 to 30 (×10 -5 / K), more preferably 1.3 to 10 (×10 -5 / K), particularly preferably 1.5 to 8 (×10 -5 / K). This makes it easy to satisfy the above formula.
[0115] The expansion and contraction in the longitudinal direction of a test piece having a width of 4.5 mm and a length of 15 mm is measured at a temperature increase rate of 5°C / min in the range of 30 to 70°C using a thermomechanical analyzer to calculate the linear expansion coefficient α of the writing feel improving film.
[0116] In order to obtain a writing feel-improving film with a protective film satisfying the above formula, a protective film having an appropriate linear expansion coefficient may be selected in relation to the writing feel-improving film to be used.
[0117] The average value of the frictional force between the writing feel improving film (writing feel improving layer) and a stylus pen during writing is preferably 100 to 1200 mN, more preferably 200 to 800 mN, particularly preferably 250 to 500 mN, and further preferably 300 to 400 mN.
[0118] The maximum value of the frictional force between the writing feel improving film (writing feel improving layer) and a stylus pen during writing is preferably 200 to 1500 mN, particularly preferably 250 to 1000 mN, and further preferably 300 to 600 mN.
[0119] The minimum value of the frictional force between the writing feel improving film (writing feel improving layer) and the stylus pen during writing is preferably 80 to 1200 mN, more preferably 120 to 1000 mN, particularly preferably 200 to 700 mN, and further preferably 240 to 500 mN.
[0120] The standard deviation of the frictional force between the writing feel improving film (writing feel improving layer) and a stylus pen during writing is preferably 10 to 60 mN, more preferably 14 to 45 mN, and particularly preferably 16 to 30 mN.
[0121] By making any or all of the average value, maximum value, minimum value, and standard deviation of the friction force within the above range, the vibration sense transmitted to the hand holding the stylus pen can easily and well reproduce the vibration sense obtained when writing on paper with a ballpoint pen. It should be noted that the physical properties related to the friction force can be measured by the method described in the examples described later.
[0122] The writing feel improving layer of the writing feel improving film of the present invention has excellent scratch resistance. In the evaluation of scratch resistance using steel wool, preferably no appearance change is observed. Specifically, the surface of the writing feel improving layer is scratched at 250 g / cm2 using #0000 steel wool in accordance with JIS K5600-5-10. 2 After rubbing for 10 cm and 10 times with a load of , the scratches on the surface are preferably not damaged. Thus, when used on the surface of a display body such as a touch panel, excellent surface protection can be exerted, and the beauty of the touch panel can be well maintained.
[0123] The scratch resistance can be evaluated by the method described in the test examples described later.
[0124] The pencil hardness of the writing feel improvement film (writing feel improvement layer) of the present invention is preferably H or more, preferably 2H or more, particularly preferably 3H or more, and further preferably 4H or more. In addition, the pencil hardness is usually 9H or less, preferably 7H or less, and more preferably 5H or less. By having this hardness, it has excellent scratch resistance, and when used on the surface of a display body such as a touch panel, it exerts excellent surface protection. In particular, the surface is not easily damaged, so the beauty of the touch panel can be well maintained.
[0125] The pencil hardness can be measured according to JIS K5600 using a pencil scratch hardness tester.
[0126] The total light transmittance (%) of the writing feel improving film of the present invention is preferably 80 (%) or more, more preferably 85% or more, and particularly preferably 90% or more. As a result, the writing feel improving film has excellent transparency and can also exhibit good image recognition when applied to a touch panel. The upper limit of the total light transmittance is usually 100%.
[0127] The total light transmittance can be measured using a haze meter in accordance with JIS K 7361-1.
[0128] The haze (%) of the writing feel improving film (writing feel improving layer) of the present invention is preferably 0 to 50%, more preferably 1 to 40%, particularly preferably 5 to 30, and further preferably 10 to 22%. Thus, the writing feel improving film has excellent transparency and can also exhibit good image recognition when applied to a touch panel.
[0129] The haze can be measured using a haze meter in accordance with JIS K 7136:2000.
[0130] 2) Protective film
[0131] In the writing feel improving film with a protective film of the present invention, the protective film has the function of preventing the surface of the writing feel improving film from being damaged and dirt from being attached.
[0132] The protective film may include only a protective film base layer, or may include a protective film base layer and an adhesive layer.
[0133] (1) Protective film substrate layer
[0134] The material of the protective film substrate layer according to the present embodiment is not particularly limited, and examples thereof include conventionally known materials used as protective film substrate layers of optical films. Specifically, examples thereof include the same materials as exemplified as the above-mentioned writing feel improving film substrate layer.
[0135] Among them, from the viewpoint of handleability, ease of acquisition, and easier achievement of the effects of the present invention, preferred are polyethylene terephthalate films, polybutylene terephthalate films, polyethylene naphthalate films, polycarbonate films, polypropylene films, polyimide films, polyetherimide films, polymethylpentene films, polyphenylene sulfide films, and liquid crystal polymer films, and more preferred are polyethylene terephthalate films, polypropylene films, and polycarbonate films.
[0136] The protective film base material layer may be a single layer formed of one of these films, or may be a layer in which two or more of these films are laminated.
[0137] The protective film substrate layer can be subjected to surface treatment such as oxidation and convexification and primer treatment in the same manner as described in the above-mentioned writing feel improving film substrate layer. These surface treatment methods are appropriately selected depending on the type of the protective film substrate layer.
[0138] From the viewpoint of operability, cost, etc., the thickness of the protective film substrate layer can be appropriately set. The thickness of the protective film substrate layer is preferably 10 to 300 μm, more preferably 20 to 200 μm, particularly preferably 25 to 150 μm, further preferably 30 to 120 μm, and more preferably 35 to 110 μm. As a result, the relationship between the linear expansion coefficients α and β is easily satisfied, and the interlayer peeling force described later is easily within the specified range.
[0139] (2) Adhesive layer
[0140] When the protective film has an adhesive layer, the protective film base layer and the writing feel improving film can be more easily and firmly bonded to each other via the adhesive layer.
[0141] As the adhesive constituting the adhesive layer, an adhesive commonly used in optical film applications can be used. Examples thereof include acrylic adhesives, rubber adhesives, silicone adhesives, urethane adhesives, polyester adhesives, polyvinyl ether adhesives, etc. In addition, the adhesive can be any one of an emulsion type, a solvent type, or a solvent-free type. Furthermore, the adhesive may have a cross-linked structure or may not have a cross-linked structure.
[0142] Among these, from the viewpoint of exhibiting the desired adhesion, optical properties, and excellent durability, an acrylic adhesive containing a (meth)acrylate polymer as a base polymer is preferred, and an acrylic adhesive containing a (meth)acrylate polymer as a base polymer and having a cross-linked structure is more preferred. It should be noted that in this specification, "polymer" also includes the concept of "copolymer".
[0143] The monomer units constituting the (meth)acrylate polymer can be appropriately adjusted from the viewpoints of transparency, adhesive strength, etc., and are particularly preferably monomers containing an alkyl (meth)acrylate and a monomer having a reactive functional group in the molecule (reactive functional group-containing monomer).
[0144] The (meth)acrylate polymer can exhibit preferred adhesiveness by containing a (meth)acrylate alkyl ester as a monomer unit constituting the polymer. As the (meth)acrylate alkyl ester, one having an alkyl group with 1 to 20 carbon atoms is preferred. The alkyl group may be linear or branched, or may have a cyclic structure.
[0145] As the (meth)acrylic acid alkyl esters having 1 to 20 carbon atoms in the alkyl group, for example, methyl (meth)acrylate, ethyl (meth)acrylate, propyl (meth)acrylate, n-butyl (meth)acrylate, n-pentyl (meth)acrylate, n-hexyl (meth)acrylate, 2-ethylhexyl (meth)acrylate, isooctyl (meth)acrylate, n-decyl (meth)acrylate, n-dodecyl (meth)acrylate, myristyl (meth)acrylate, palmityl (meth)acrylate, stearyl (meth)acrylate, cyclohexyl (meth)acrylate, isobornyl (meth)acrylate, adamantyl (meth)acrylate, etc. can be listed. Among them, from the viewpoint of easily adjusting the interlayer peeling force described later to the desired value, methyl (meth)acrylate and 2-ethylhexyl (meth)acrylate can be preferably listed. They can be used alone or in combination of two or more.
[0146] The (meth)acrylate polymer preferably contains 30 to 99.9% by mass of an alkyl (meth)acrylate as a monomer unit constituting the polymer, particularly preferably 50 to 99.5% by mass, and further preferably 70 to 99% by mass, relative to all monomer units. By setting the content within this range, it is easy to adjust the interlayer peeling force described later to a desired value.
[0147] The (meth)acrylate polymer contains a monomer containing a reactive functional group as a monomer unit constituting the polymer, and thus reacts with a crosslinking agent described below via the reactive functional group derived from the monomer containing the reactive functional group, thereby forming a crosslinked structure (three-dimensional network structure) to obtain a pressure-sensitive adhesive having a desired cohesive force.
[0148] As the monomer containing reactive functional groups, preferably there can be listed monomers having hydroxyl groups in the molecule (hydroxyl-containing monomers), monomers having carboxyl groups in the molecule (carboxyl-containing monomers), monomers having amino groups in the molecule (amino-containing monomers), etc. Among them, from the viewpoint of easily adjusting the crosslinking density, easily obtaining the adhesive with the desired cohesive force, and the viewpoint of the interlayer peeling force described later, preferably hydroxyl-containing monomers or carboxyl-containing monomers. These monomers containing reactive functional groups can be used alone or in combination of two or more.
[0149] Examples of hydroxyl-containing monomers include hydroxyalkyl (meth)acrylates such as 2-hydroxyethyl (meth)acrylate, 2-hydroxypropyl (meth)acrylate, 3-hydroxypropyl (meth)acrylate, 2-hydroxybutyl (meth)acrylate, 3-hydroxybutyl (meth)acrylate, and 4-hydroxybutyl (meth)acrylate. Among the above, hydroxyalkyl (meth)acrylates having a hydroxyalkyl group having 1 to 4 carbon atoms are preferred. These may be used alone or in combination of two or more.
[0150] As the carboxyl group-containing monomer, for example, ethylenically unsaturated carboxylic acids such as acrylic acid, methacrylic acid, crotonic acid, maleic acid, itaconic acid, and citraconic acid can be cited. Among them, acrylic acid is preferred from the viewpoint of easily satisfying the interlayer peeling force described later. These can be used alone or in combination of two or more.
[0151] In the (meth)acrylate polymer, as a monomer unit constituting the polymer, it is preferred that 0.1 to 20% by mass of a monomer containing a reactive functional group is contained relative to all monomer units, more preferably 0.5 to 10% by mass, and particularly preferably 0.8 to 3% by mass. Thus, the (meth)acrylate polymer is likely to undergo a desired crosslinking reaction between crosslinking agents, and as a result, the obtained adhesive is likely to have good cohesive force, and the interlayer peeling force described later is likely to be adjusted to a desired value.
[0152] The (meth)acrylate polymer may further contain other monomers as monomers constituting the polymer. Examples of the other monomers include (meth)acrylates containing alicyclic structures such as glycidyl (meth)acrylate, dicyclopentanyl (meth)acrylate, adamantyl (meth)acrylate, isobornyl (meth)acrylate, dicyclopentenyl (meth)acrylate, and dicyclopentenyloxyethyl (meth)acrylate; (meth)acrylate alkoxyalkyl esters such as methoxyethyl (meth)acrylate and ethoxyethyl (meth)acrylate; non-crosslinked acrylamides such as acrylamide and methacrylamide; non-crosslinked (meth)acrylates having tertiary amino groups such as N,N-dimethylaminoethyl (meth)acrylate and N,N-dimethylaminopropyl (meth)acrylate; vinyl acetate; styrene, etc. Among them, from the viewpoint of the cohesive force of the obtained (meth)acrylate polymer (A) and the viewpoint of the interlayer peeling force described later, glycidyl (meth)acrylate is preferred, and glycidyl methacrylate is particularly preferred. These may be used alone or in combination of two or more.
[0153] The (meth)acrylate polymer preferably contains 0.1 to 10% by mass of other monomers as monomer units constituting the polymer, particularly preferably 0.2 to 5% by mass, and further preferably 0.3 to 1% by mass, relative to all monomer units. This makes it easy for the obtained adhesive to have good cohesive force, and it is easy to adjust the interlayer peeling force described later to a desired value.
[0154] The polymerization method of the (meth)acrylate polymer in the present embodiment can be a random polymer or a block polymer. In addition, the acrylic polymer can be obtained by polymerizing the above-mentioned monomers using a conventional method. It can be prepared by polymerization, for example, by emulsion polymerization, solution polymerization, suspension polymerization, bulk polymerization, aqueous solution polymerization, etc. Among them, from the viewpoint of stability during polymerization and ease of handling during use, it is preferably prepared by solution polymerization in an organic solvent.
[0155] The weight average molecular weight of the (meth)acrylate polymer is preferably 100,000 to 3,000,000, more preferably 300,000 to 2,000,000, particularly preferably 450,000 to 1,500,000, and further preferably 600,000 to 1,000,000. This makes it easier for the resulting adhesive to have good cohesive force and to adjust the interlayer peeling force described below to a desired value.
[0156] It should be noted that the adhesive composition described in this embodiment may contain one of the above-mentioned (meth)acrylate polymers, or may contain two or more of them. In addition, the adhesive composition described in this embodiment may contain the above-mentioned (meth)acrylate polymer and other (meth)acrylate polymers.
[0157] The crosslinking agent can crosslink the (meth)acrylate polymer by heating the adhesive composition to form a good three-dimensional network structure, thereby further improving the cohesive force of the resulting adhesive and making it easier to adjust the interlayer peeling force described below to a desired value.
[0158] Examples of the crosslinking agent include preferably a crosslinking agent that reacts with a reactive functional group possessed by the (meth)acrylate polymer, and examples thereof include isocyanate crosslinking agents, epoxy crosslinking agents, amine crosslinking agents, melamine crosslinking agents, aziridine crosslinking agents, hydrazine crosslinking agents, aldehyde crosslinking agents, oxazoline crosslinking agents, metal alkoxide crosslinking agents, metal chelate crosslinking agents, metal salt crosslinking agents, and ammonium salt crosslinking agents.
[0159] Among the examples of the crosslinking agent, isocyanate crosslinking agents, epoxy crosslinking agents, and aziridine crosslinking agents are preferably used from the viewpoint of being easy to react with the reactive functional groups possessed by the (meth)acrylate polymer and being easy to adjust the interlayer peeling force described later to a desired value. It should be noted that the crosslinking agent can be used alone or in combination of two or more.
[0160] When the adhesive composition contains a crosslinking agent and a (meth)acrylate polymer, the content of the crosslinking agent in the adhesive composition is preferably 0.01 to 5 parts by mass, more preferably 0.1 to 4 parts by mass, particularly preferably 0.5 to 3 parts by mass, and further preferably 1 to 2 parts by mass relative to 100 parts by mass of the (meth)acrylate polymer. As a result, the obtained adhesive is likely to exert a more excellent cohesive force, and it is easy to adjust the interlayer peeling force described later to a desired value.
[0161] In addition, the pressure-sensitive adhesive layer may contain other components depending on the purpose.
[0162] Other components include tackifiers, plasticizers, antistatic agents, ultraviolet absorbers, silane coupling agents, rust inhibitors, antioxidants, light stabilizers, softeners, refractive index adjusters, etc. It should be noted that the polymerization solvent and dilution solvent described below are not included in the additives constituting the adhesive composition.
[0163] When the adhesive composition contains a plasticizer, the content of the crosslinking agent in the adhesive composition is preferably 0.1 to 50 parts by mass, more preferably 1 to 35 parts by mass, particularly preferably 4 to 20 parts by mass, and further preferably 8 to 15 parts by mass relative to 100 parts by mass of the (meth)acrylate polymer. As a result, the obtained adhesive is likely to exert a more excellent cohesive force and it is easy to adjust the interlayer peeling force described later to a desired value.
[0164] The thickness of the adhesive layer is not particularly limited, but is preferably 3 to 300 μm, more preferably 5 to 200 μm, particularly preferably 10 to 100 μm, further preferably 15 to 60 μm, and particularly preferably 20 to 35 μm. This makes it easier to satisfy the relationship between the linear expansion coefficients α and β, and the interlayer peeling force described later can easily reach a predetermined range.
[0165] (3) Protective film
[0166] The method for producing the protective film having an adhesive layer is not particularly limited, and can be formed, for example, by applying the adhesive layer-forming composition on the protective film substrate layer to a desired film thickness by a known coating method and drying the resulting coating.
[0167] The pressure-sensitive adhesive layer-forming composition generally contains a base polymer, a solvent, and a cross-linking agent, and may contain fine particles, a tackifier, a plasticizer, an antistatic agent, an ultraviolet absorber, and the like as desired.
[0168] In the writing feel improving film with a protective film of the present invention, as described later, the linear expansion coefficient β (×10 -5 / K) and the linear expansion coefficient α (×10 -5 / K) needs to satisfy the formula: -6.5<(α-β)<6.5.
[0169] That is, the relationship between the protective film used and the writing feel improving film used must have a linear expansion coefficient that satisfies the above formula.
[0170] Specifically, as long as the linear expansion coefficient β (×10 -5 The relationship between the linear expansion coefficient α of the writing feel improving film satisfies the formula: -6.5<(α-β)<6.5, and is not particularly limited, but is usually greater than 0 and less than 50 (×10 -5 / K), preferably 1 to 15 (×10 -5 / K), more preferably 1.3 to 10 (×10 -5 / K), particularly preferably 1.5 to 8 (×10 -5 / K). Thus, the above formula can be easily satisfied.
[0171] The linear expansion coefficient of the protective film was determined by measuring the expansion and contraction in the longitudinal direction of a test piece having a width of 4.5 mm and a length of 15 mm at a heating rate of 5°C / min using a thermomechanical analyzer. The linear expansion coefficient (×10 -5 / K).
[0172] The tensile elastic modulus of the protective film is usually 10 to 3000 (MPa).
[0173] By setting the tensile elastic modulus of the protective film within this range, the protective film tends to be easily peeled off from the writing feel improving film. In addition, since the excellent surface protectiveness is easily exerted, the quality of the writing feel improving film can be well maintained.
[0174] The tensile elastic modulus is a value measured in accordance with JIS K7127:1999.
[0175] 3) Writing feel improvement film with protective film
[0176] The writing feel-improving film with a protective film of the present invention is obtained by laminating a protective film on at least one side of the above-mentioned writing feel-improving film.
[0177] When the protective film has an adhesive layer, the protective film and the writing feel-improving film are laminated in such a manner that at least one side of the writing feel-improving film is in contact with the adhesive layer.
[0178] The writing feeling improving film with a protective film of the present invention can be in the form of a long strip (belt) or a short strip (single sheet).
[0179] The schematic diagram of the layer constitution of the writing feel improving film with a protective film of the present invention is shown in Figure 1 It should be noted that Figure 1 , describes an example of the layer constitution of a writing feel improving film with a protective film when the protective film has a pressure-sensitive adhesive layer.
[0180] Figure 1 (a) shows that the writing feel improving film 10a and the protective film 20a are stacked in such a manner that the writing feel improving layer 2a is in contact with the adhesive layer 3a of the protective film 20a, Figure 1 (b) shows that the writing feel improving film 10b and the protective film 20b are stacked in such a manner that the writing feel improving film base material layer 1b is in contact with the adhesive layer 3b of the protective film 20a, Figure 1 (c) shows that on the writing feel improving layer 2c side of the writing feel improving film 10c, the protective film 20a is laminated in such a manner that the writing feel improving layer 2c is in contact with the adhesive layer 3c of the protective film 20c, and on the writing feel improving film base layer 1c side, the protective film 20c' is laminated in such a manner that the writing feel improving film base layer 1c is in contact with the adhesive layer 3c' of the protective film 20c.
[0181] Specific examples of the layer constitution of the writing feel-improving film with a protective film of the present invention include the following.
[0182] (1) Protective film base layer / writing feel improving film base layer / writing feel improving layer
[0183] (2) Protective film base layer / adhesive layer / writing feel improving film base layer / writing feel improving layer
[0184] (3) Writing feel improving film base material layer / writing feel improving layer / protective film base material layer
[0185] (4) Writing feel improving film base material layer / writing feel improving layer / adhesive layer / protective film base material layer
[0186] (5) Protective film substrate layer 1 / writing feel improving film substrate layer / writing feel improving layer / protective film substrate layer 2
[0187] (6) Protective film substrate layer 1 / adhesive layer 2 / writing feel improving film substrate layer / writing feel improving layer / protective film substrate layer 2
[0188] (7) Protective film substrate layer 1 / writing feel improving film substrate layer / writing feel improving layer / adhesive layer 2 / protective film substrate layer 2
[0189] (8) Protective film substrate layer 1 / adhesive layer 1 / writing feel improving film substrate layer / writing feel improving layer / adhesive layer 2 / protective film substrate layer 2
[0190] In the writing feel-improving film with protective films of the present invention, when protective films are laminated on both surfaces of the writing feel-improving film, the two protective films may be the same as or different from each other.
[0191] Among them, a writing feel improving film with a protective film in which the protective film is laminated on the writing feel improving layer of the writing feel improving film is preferred because the writing feel improving layer is directly protected and the quality of the writing feel improving layer is more easily maintained.
[0192] The writing feel improving film with a protective film can be produced by overlapping the writing feel improving film and the protective film and press-bonding (laminating) them.
[0193] When the protective film has an adhesive layer, the protective film and the writing feel-improving film can be laminated by a known method so that the adhesive layer is in contact with the writing feel-improving film.
[0194] As described above, the writing feel improving film with a protective film of the present invention has a linear expansion coefficient of α (×10 -5 / K), the linear expansion coefficient of the protective film is set to β(×10 -5 / K), the formula: -6.5<(α-β)<6.5 is satisfied. The writing feel improving film with a protective film of the present invention preferably satisfies the formula: -6.0<(α-β)<6.0, more preferably satisfies the formula: -3.0<(α-β)<3.0, particularly preferably satisfies the formula: -1.0<(α-β)<1.0, and further preferably satisfies the formula: -0.5<(α-β)<0.5.
[0195] The (α-β) value of the writing feel improving film with a protective film is below -6.5. When it is above 6.5, the writing feel improving film with a protective film is exposed to a high temperature state (40 to 60°C) for a long time during storage and transportation, or is exposed to a high temperature state (50 to 90°C) during processing, resulting in curling on the film due to temperature changes during processing, which may lead to deterioration in the quality of the writing feel improving film (the function of the writing feel improving film to improve the writing feel using a stylus pen is impaired).
[0196] Since the values of α and β satisfy the relationship described above, the writing feel improving film with a protective film of the present invention can effectively suppress the occurrence of curling caused by temperature changes during storage, transportation, processing, etc. of the writing feel improving film with a protective film, and as a result, the quality of the writing feel improving film can be maintained.
[0197] The fact that the writing feel improving film with a protective film of the present invention is less prone to curling due to temperature changes can be confirmed as follows: for example, when a sample (A4 size) of the writing feel improving film with a protective film of the present invention is placed in an oven maintained at 70°C with the protective film side facing downward, the maximum height of the curling that occurs is generally less than 50 mm, preferably less than 40 mm, even after being left for 1 hour.
[0198] Here, the "maximum curl height" is the maximum vertical distance between the horizontal test bench and the protective film. Figure 2 As shown in (a), when a mountain-shaped curl occurs, the maximum height of the curl is the distance (height) shown by h1. Figure 2 As shown in (b), when valley-shaped curling occurs, the maximum height of the curl is the distance (height) indicated by h2.
[0199] The writing feeling improving film with protective film is as described above Figure 1 When there are two protective films as shown in (c), from the viewpoint of suppressing the occurrence of curling, it is preferred that β of the two protective films respectively satisfy the above requirements.
[0200] That is, the writing feel improving film with a protective film of the present invention must select and use a protective film having a linear expansion coefficient that satisfies the above formula with the writing feel improving film used, or select and use a writing feel improving film having a linear expansion coefficient that satisfies the above formula with the protective film used.
[0201] The writing feeling improving film with a protective film of the present invention can be produced in the following manner: for example, several sheets having various linear expansion coefficients β (×10 -5 / K) protective film (step (i)); measuring the linear expansion coefficient α (×10 -5 / K) (step (ii)); then, the protective film is selected in a manner satisfying the formula: -6.5<(α-β)<6.5, and the writing feeling improvement film and the protective film are formed into Figure 1 (a)~ Figure 1 The layers are laminated (bonded) in the form of the layer structure (c).
[0202] In the writing feel improving film with a protective film of the present invention, the interlayer peeling force between the writing feel improving film and the protective film is preferably 800 mN / 25 mm or less. Here, "interlayer peeling force between the writing feel improving film and the protective film" refers to the interlayer peeling force between the surface of the writing feel improving layer of the writing feel improving film and the protective film, and / or the interlayer peeling force between the surface of the base material layer of the writing feel improving film and the protective film. This is described in detail below.
[0203] In the writing feel improving film with a protective film of the present invention, the interlayer peeling force between the surface of the writing feel improving layer of the writing feel improving film and the protective film is preferably 800 mN / 25 mm or less, more preferably 500 mN / 25 mm or less, particularly preferably 300 mN / 25 mm or less, and further preferably 250 mN / 25 mm or less.
[0204] It should be noted that when the protective film is not laminated on the substrate side of the writing feel improving film, the interlayer peeling force between the surface of the writing feel improving layer and the protective film is preferably 220 mN / 25 mm or less, more preferably 200 mN / 25 mm or less, particularly preferably 180 mN / 25 mm or less, and particularly preferably 160 mN / 25 mm or less, from the viewpoint of peelability from the writing feel improving layer. From the viewpoint of preventing the undesirable situation of floating or peeling from the writing feel improving film when exposed to temperature changes, the lower limit of the interlayer peeling force between the writing feel improving film and the protective film is preferably 50 mN / 25 mm or more, more preferably 80 mN / 25 mm or more, and particularly preferably 100 mN / 25 mm or more.
[0205] In the writing feel improving film with a protective film of the present invention, the interlayer peeling force between the surface of the substrate layer of the writing feel improving film and the protective film is preferably 800 mN / 25 mm or less, more preferably 500 mN / 25 mm or less, particularly preferably 300 mN / 25 mm or less, further preferably 200 mN / 25 mm or less, and particularly preferably 170 mN / 25 mm or less. From the viewpoint of preventing the undesirable situation of inadvertent floating and peeling from the writing feel improving film when exposed to temperature changes, the lower limit of the interlayer peeling force between the writing feel improving film and the protective film is preferably 50 mN / 25 mm or more, more preferably 80 mN / 25 mm or more, and particularly preferably 100 mN / 25 mm or more.
[0206] By having such interlayer peeling force, the occurrence of curling caused by temperature changes during storage, transportation, processing, etc. can be more effectively controlled, the quality of the writing feel improving film can be maintained, and the protective film can be easily peeled off from the writing feel improving film during use.
[0207] The interlayer peeling force between the writing feel improving film and the protective film can be measured by the method described in Examples.
[0208] The writing feel improving film with a protective film of the present invention can be used as a writing feel improving film constituting the outermost surface of a touch panel (image display device with a position detection function) to which a stylus pen is applied by peeling off the protective film from the writing feel improving film.
[0209] Specifically, the writing feel improving film is laminated on a cover material in a touch panel having a display module such as a liquid crystal (LCD) module, a light emitting diode (LED) module, an organic electroluminescent (organic EL) module, a touch sensor, etc., so that the cover material is in contact with the writing feel improving film substrate layer. The writing feel improving film can be attached via an adhesive layer.
[0210] The stylus pen using the writing feel improving film is not particularly limited, and examples thereof include a stylus pen having a polyacetal pen tip, a stylus pen having a hard felt pen tip, and a stylus pen having an elastomer pen tip.
[0211] The above-described embodiments are described for easy understanding of the present invention and do not limit the present invention at all. Therefore, the elements disclosed in the above-described embodiments include all design changes and equivalents within the technical scope of the present invention.
[0212] For example, the writing feel-improving film with a protective film of the present invention may be laminated with other layers. Examples of the other layers include an adhesive layer laminated on the writing feel-improving film substrate layer side and a release film.
[0213] It should be noted that, in the present specification, when "X to Y" (X and Y are arbitrary numbers) is written, unless otherwise specified, it includes the meaning of "X or more and Y or less", and also includes the meaning of "preferably greater than X" or "preferably less than Y". In addition, when "X or more" (X is an arbitrary number) is written, unless otherwise specified, it includes the meaning of "preferably greater than X", and when "Y or less" (Y is an arbitrary number) is written, unless otherwise specified, it includes the meaning of "preferably less than Y".
[0214] Example
[0215] Hereinafter, the present invention will be described in more detail with reference to Examples and the like, but the scope of the present invention is not limited to these Examples and the like.
[0216] (Manufacturing Example 1) Preparation of a composition for forming a writing feel improving layer
[0217] An active energy ray-curable component containing a multifunctional urethane acrylate (product name "Optistar Z7530", manufactured by Arakawa Chemical Industries, Ltd.) 100 parts by mass (indicated as solid content conversion value. The same applies to the components other than the solvent below), 9.0 parts by mass of silicone fine particles (TOSPAR 1100, manufactured by Momentib, average particle size: 11.0 μm, true spherical), 1.0 parts by mass of a fluorine-based surface conditioner (Megaphak RS-90, manufactured by DIC Corporation), 0.3 parts by mass of a silicone-based surface conditioner (SH28, polydimethylsiloxane, manufactured by DAW TORAY CO., LTD.), and 85.5 parts by mass of 1-methoxy-2-propanol as a solvent were mixed to prepare a composition for forming a writing feel improving layer.
[0218] (Production Example 2) Preparation of Adhesive Layer-Forming Composition
[0219] 70 parts by mass of 2-ethylhexyl acrylate, 28.6 parts by mass of methyl acrylate, 0.3 parts by mass of glycidyl methacrylate and 1.1 parts by mass of acrylic acid were copolymerized to prepare a (meth)acrylate polymer. The molecular weight of the obtained (meth)acrylate polymer was measured by the method shown below, and the weight average molecular weight (Mw) was 800,000.
[0220] The weight average molecular weight (Mw) is a polystyrene-equivalent weight average molecular weight obtained by measuring using gel permeation chromatography (GPC) under the following conditions (GPC measurement).
[0221] (Measurement conditions)
[0222] ·GPC measuring device: HLC-8020, manufactured by Tosoh Corporation
[0223] ·GPC column (passed in the following order): manufactured by Tosoh Corporation
[0224] TSK guard column HXL-H
[0225] TSK gel GMHXL (×2)
[0226] TSK gel G2000HXL
[0227] ·Test solvent: tetrahydrofuran
[0228] ·Measurement temperature: 40℃
[0229] A composition for forming an adhesive layer is prepared by mixing 100 parts by mass of the (meth)acrylate polymer obtained as described above (representing the solid content conversion value. The same applies to the other components except the solvent below), 10.0 parts by mass of dibutoxyethoxyethyl adipate as a plasticizer, 1.9 parts by mass of an aziridine-based crosslinking agent (BXX-5134, manufactured by Toyochem Co., Ltd.) as a crosslinking agent, and 87 parts by mass of toluene as a solvent.
[0230] (Manufacturing Example 3) Preparation of Writing Feel Improvement Film a
[0231] In the polycarbonate / polymethyl methacrylate (PC / PMMA) laminated film [AW-10SU, thickness 200 μm (thickness ratio: PC / PMMA = about 2:1), linear expansion coefficient: 7.66×10 -5 / K, tensile elastic modulus: 1990 MPa, manufactured by WEIBLOCK ADBANT TECHNOLOGY CO., LTD.], the composition for forming a writing feel improving layer obtained in Production Example 1 was applied with a Meyer bar to a film thickness of 7 μm to form a coating film, and the coating film was placed in an oven maintained at 70° C. for 1 minute to dry.
[0232] Next, ultraviolet irradiation was performed using an ultraviolet irradiation device (Igland Tester ECS-401GX, manufactured by Igland Fix) with a high pressure mercury lamp as a light source under the following irradiation conditions to cure the coating film to produce a writing feel improving film a.
[0233] (UV irradiation conditions)
[0234] Lamp power: 2kW
[0235] Conveying speed: 4.23m / min
[0236] Illuminance: 240mW / cm 2
[0237] Light intensity: 307mJ / cm 2
[0238] (Manufacturing Example 4) Preparation of Writing Feel Improvement Film b
[0239] In Production Example 3, instead of the PC / PMMA laminated film, a polyethylene terephthalate (PET) film [LumiLa U403, thickness 188 μm, linear expansion coefficient: 1.68×10 -5 / K, tensile elastic modulus: 214 MPa, manufactured by Toray Industries, Inc.], the same procedure as in Production Example 3 was performed to produce a writing feel improving film b.
[0240] The linear expansion coefficient α (×10 -5 / K), total light transmittance (%), and haze (%).
[0241] In addition, the friction force and pencil hardness of the surfaces of the writing feel improving layers of the obtained writing feel improving films a and b were measured by the methods described below to evaluate the scratch resistance.
[0242] 〔Linear expansion coefficient〕
[0243] Using a thermomechanical analyzer (TMA4000SA, manufactured by Bruker AXS), the expansion and contraction in the longitudinal direction of a test piece having a width of 4.5 mm and a length of 15 mm was measured at a heating rate of 5°C / min, and the linear expansion coefficient α (×10-5 / K) in the range of 30 to 70°C was calculated.
[0244] The results are shown in Table 1.
[0245] 〔Total light transmittance〕
[0246] The obtained writing feel improving film was irradiated with light from the writing feel improving layer side after blank correction using a haze meter (NDH-5000, manufactured by Nippon Denshoku Industries) in accordance with JIS K7361-1 to measure the total light transmittance (%).
[0247] The total light transmittance of the writing feel improving film a was 90.4%, and the total light transmittance of the writing feel improving film b was 90.3%.
[0248] 〔Haze〕
[0249] According to JIS K 7136:2000, a haze meter (NDH-5000, manufactured by Nippon Denshoku Industries) was used to measure the haze value (%) of the obtained writing feel improving film by irradiating light from the writing feel improving layer side after blank correction.
[0250] The haze of the writing feel-improving film a was 20.4%, and the haze of the writing feel-improving film b was 20.2%.
[0251] 〔Friction force measurement〕
[0252] The friction force between the obtained writing feel improving films a and b and a stylus pen (product name "ACK-2003", pen tip material: felt, pen tip diameter: 0.5 mm, manufactured by Wacom Co., Ltd.) during writing was measured under the following conditions using a dynamic and static friction measuring machine (Traibo Master TL201Ts, manufactured by Trinitrable Co., Ltd.).
[0253] The average friction force of the writing feel improving film a was 310 mN, the maximum friction force was 350 mN, the minimum friction force was 240 mN, and the standard deviation of the friction force was 17 mN. The average friction force of the writing feel improving film b was 300 mN, the maximum friction force was 340 mN, the minimum friction force was 230 mN, and the standard deviation of the friction force was 18 mN.
[0254] (Measurement conditions)
[0255] Load: 200g
[0256] Test length: 10~100mm
[0257] Speed: 1.6 mm / s (vibration measurement conditions, dynamic friction coefficient measurement conditions)
[0258] Sampling interval: 50ms
[0259] Stylus tip angle: 45°
[0260] 〔Pencil hardness〕
[0261] The pencil hardness of the writing feel improving layer-side surface of the obtained writing feel improving films a and b was measured using a pencil scratch hardness tester (product name "No. 553-M", manufactured by Yasuda Seiki Seisaku-sho Co., Ltd.) in accordance with JIS K5600.
[0262] The pencil hardness of the writing feel improving films a and b is 4H.
[0263] 〔Scratch resistance〕
[0264] The writing feel improving layer side surface of the writing feel improving films a and b was coated with #0000 steel wool at a temperature of 250 g / cm 2 The writing feel improving layer was rubbed back and forth 10 times with a load of 100 and a sliding distance of 10 cm. Thereafter, the writing feel improving layer was visually checked for scratches under a three-wavelength fluorescent lamp and evaluated according to the following criteria.
[0265] ○: No change was observed in the appearance of the writing feel improving layer (the number of observed scratches was 0)
[0266] ×: Changes were observed in the appearance of the writing feel improving layer (the number of observed scratches was 1 or more)
[0267] As a result, both the writing feel improving films a and b were 0, and it was found that they had excellent scratch resistance.
[0268] (Example 1)
[0269] Production with Figure 1(a) A writing feel improving film having the same layer structure as shown in FIG. 1 and having a protective film.
[0270] In the protective film substrate layer C, a polycarbonate (PC) film (thickness: 100 μm, linear expansion coefficient: 7.70 (×10 -5 / K))〕, the adhesive layer forming composition obtained in Production Example 2 was applied to the substrate using an applicator capable of obtaining a desired film thickness so as to have a film thickness of 30 μm to form an adhesive layer coating. Thereafter, the coating was placed in an oven maintained at 100° C. for 1 minute to dry the coating, thereby obtaining a protective film including a protective film substrate layer and an adhesive layer.
[0271] The linear expansion coefficient of the protective film β(×10 -5 The results are shown in Table 1.
[0272] Next, the surface of the adhesive layer of the protective film obtained above and the writing feel improving layer of the writing feel improving film a obtained in Production Example 2 were bonded together to prepare a writing feel improving film with a protective film.
[0273] (Examples 2 to 4, Comparative Examples 1 and 2)
[0274] In the same manner as in Example 1, writing feel improving films with protective films of Examples 2 to 4 and Comparative Examples 1 and 2 were produced according to the method shown in Table 1.
[0275] In the table, the protective film base material layers D and E are as follows.
[0276] D: Polypropylene (PP) film (thickness: 120 μm)
[0277] E: PET film (thickness: 38 μm)
[0278] (Example 5)
[0279] The same operation as in Example 1 was performed, and the adhesive layer forming composition obtained in Production Example 2 was applied to the protective film substrate layer E (PET film, thickness: 38 μm) using an applicator that can obtain a desired film thickness so that the film thickness becomes 23 μm, thereby forming a coating film of the adhesive layer. Thereafter, the coating film was placed in an oven maintained at 100° C. for 1 minute to dry the coating film, thereby obtaining a protective film including the protective film substrate layer E and the adhesive layer.
[0280] The surface of the adhesive layer of the protective film was laminated to the surface side of the writing feel improving layer of the writing feel improving film a and the surface side of the base layer, respectively, to prepare a writing feel improving film with a protective film having a structure of protective film / writing feel improving film / protective film.
[0281] (Examples 6 and 7)
[0282] The same operation as in Example 5 was carried out, and the writing feel improving films with protective films of Examples 6 and 7 were produced in the manner shown in Table 2.
[0283] The linear expansion coefficients of the protective film β1, β2 (×10 -5 The results are shown in Table 2.
[0284] The linear expansion coefficient α (×10 -5 / K) and the linear expansion coefficient of the protective film β(×10 -5 The difference of K is shown in Tables 1 and 2.
[0285] The interlayer peeling force between the protective film and the writing feel improving film was measured for the writing feel improving films with protective films obtained in Examples 1 to 7 and Comparative Examples 1 and 2 by the method described below.
[0286] Furthermore, a curl test was performed by the method described below to evaluate the writing feel.
[0287] The results are shown in Tables 1 and 2.
[0288] 〔Interlayer peeling force〕
[0289] The writing feel improving films with protective films obtained in Examples 1 to 7 and Comparative Examples 1 to 2 were cut into test pieces of 25 mm in width and 110 mm in length. The test pieces were subjected to measurement of interlayer peeling force (adhesive force) (N / 25 mm) when the protective film was peeled off from the writing feel improving layer side of the writing feel improving film using a tensile tester (manufactured by TENSILON, ORIENTEC) in accordance with JIS Z0237:2009 at a peeling speed of 300 mm / min and a peeling angle of 180°.
[0290] In addition, for the writing feel improving films with protective films obtained in Examples 5 to 7, the interlayer peeling force (adhesive force) (N / 25 mm) when the protective film was peeled off from the substrate side of the writing feel improving film was measured by the same method as above.
[0291] The results are shown in Tables 1 and 2.
[0292] 〔Curl test〕
[0293] The obtained writing feel improving film with a protective film was cut into A4 size and placed in an oven maintained at 70° C. with the protective film side facing downward. After leaving for 1 hour, the maximum height (mm) of the curling occurred was measured.
[0294] In the table, a minus sign (-) indicates that the curl direction is a valley-shaped curl on the protective film side, and a minus sign (-) not indicated indicates that the curl direction is a mountain-shaped curl on the protective film side.
[0295] <Evaluation of writing feel>
[0296] Paper (product name "Channel Pass List", model: NO-S816B, size: B5, ruled line width: B ruled line, manufactured by Cokuyo Co., Ltd., 20 sheets stacked for use) and ballpoint pen (product name "Orendi EG 1.0", oil-based ballpoint pen, pen tip diameter: 1.0 mm, manufactured by BIC Co., Ltd.) were prepared. The evaluator wrote the characters "ABCDE" on the paper with the ballpoint pen.
[0297] Next, the protective film was peeled off from the writing feel improving layer of the writing feel improving film with a protective film after the curling test, and the film was attached to a glass plate (70 mm long, 150 mm wide, 1.2 mm thick) using a double-sided tape so that the writing feel improving layer was exposed. The characters "ABCDE" were written on the surface of the writing feel improving layer using the stylus pen used in the above friction force measurement.
[0298] The writing feel (x) of actual writing on paper with a ballpoint pen was compared with the writing feel (y) of writing on the writing feel improving layer with a stylus pen, and the writing feel was evaluated according to the following criteria.
[0299] (Evaluation Criteria)
[0300] ○: The writing feel (y) has a vibration and resistance feeling very similar to the writing feel (x), and the writing comfort is good.
[0301] △: The writing feel (y) has slightly greater vibration and resistance than the writing feel (x).
[0302] ×: The writing feel (y) is different from the writing feel (x) in terms of vibration and resistance.
[0303] [Table 1]
[0304] Table 1
[0305]
[0306] [Table 2]
[0307]
[0308] Tables 1 and 2 show that the writing feel improving films with protective films of Examples 1 to 7 having a value of (α-β) greater than −6.5 and less than 6.5 had a maximum curl height of 40 mm or less, and the occurrence of curling due to heat was suppressed.
[0309] It was also found that the writing feel was good and the quality of the writing feel improving layer was maintained.
[0310] On the other hand, it is understood that in Comparative Examples 1 and 2, the maximum curl height was 85 mm or more, and large curling occurred due to heat. As a result, the writing feel was poor, and curling occurred, thereby impairing the quality of the writing feel improving layer.
[0311] Description of Reference Numerals
[0312] 1a, 1b, 1c…writing feel improving film substrate layer
[0313] 2a, 2b, 2c…writing feel improvement layer
[0314] 3a, 3b, 3c, 3c' ... adhesive layer
[0315] 4a, 4b, 4c, 4c' ... protective film substrate layer
[0316] 10a, 10b, 10c ... Films for improving writing feel
[0317] 20a, 20b, 20c, 20c'…protective film
[0318] 30…Test bench
[0319] h1, h2... Maximum height of curl
Claims
1. A writing feel improving film with a protective film, wherein a protective film is laminated on at least one side of a writing feel improving film having a writing feel improving film substrate layer and a writing feel improving layer, It is characterized in that The linear expansion coefficient of the writing feel improving film is α(×10 -5 / K), the linear expansion coefficient of the protective film is set to β(×10 -5 / K), the formula is satisfied: -6.5<(α-β)<6.
5.
2. The writing feel-improving film with a protective film according to claim 1, wherein the protective film is laminated on the writing feel-improving layer side of the writing feel-improving film.
3. The writing feel improving film with a protective film according to claim 1 or 2, in, The protective film has an adhesive layer and a protective film base layer, and the writing feel improving film with a protective film is laminated so that at least one side of the writing feel improving film is in contact with the adhesive layer of the protective film.
4. The writing feel improving film with a protective film according to claim 1 or 2, It is characterized in that The linear expansion coefficient of the writing feel improving film is α(×10 -5 / K), the linear expansion coefficient of the protective film is set to β(×10 -5 / K), the formula is satisfied: -1.0<(α-β)<1.
0.
5. The writing feel improving film with a protective film according to claim 1 or 2, in, The linear expansion coefficient α (×10 -5 / K) is 1.5 or more and 8.0 or less (×10 -5 / K).
6. The writing feel improving film with a protective film according to claim 1 or 2, in, The interlayer peeling force between the writing feel improving film and the protective film is 800 mN / 25 mm or less.
Citation Information
Patent Citations
Writing feeling improving film
CN108070328A
Conductive film and liquid crystal handwriting board
CN108983513A
Heat-resistant resin laminated film, multilayer film with metal layer including same, and semiconductor device
CN1929994A
Self-repairable protective film with writing damping feeling
CN212800217U