Honeycomb ceramic carrier, preparation method thereof and catalytic body containing honeycomb ceramic carrier
By designing a honeycomb ceramic carrier with a special diagonal structure in the cross-section of quadrilateral, the problems of bending and low yield of the carrier wall are solved, the structural strength and yield of the carrier are improved, and the service life of the mold is extended.
Patent Information
- Application Number
- CN202411044766.X
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-07-31
- Publication Date
- 2024-11-19
- Estimated Expiration
- 2044-07-31
AI Technical Summary
In the process of increasing the pore density and wall thickness, existing honeycomb ceramic carriers are prone to bending problems in the partition wall, which affects the catalytic efficiency and structural strength, resulting in low yield, short service life, and large flow resistance of mold clay materials with right-angle structures, which is easy to This leads to bending next door and low yield.
A honeycomb ceramic carrier design with a quadrilateral cross-section compartment, wherein one pair of diagonal angles of the quadrilateral cross-section has an inner recess or chamfer, and the other pair of diagonal angles does not have an inner recess or chamfer, improving the bending of the partition wall through a special diagonal structure The temperature increase rate and sintering temperature are controlled during the sintering process to improve the compressive strength and thermal stability of the carrier.
Without increasing mold wear, the partition bending of thin-walled ceramic carrier is significantly reduced, the yield is improved, the structural strength and thermal stability of the carrier are enhanced, and the service life of the mold is extended.
Smart Images

Figure CN118976542A_ABST
Abstract
Description
Technical Field
[0001] The invention relates to the field of ceramic carrier catalysts, and in particular to a honeycomb ceramic carrier, a preparation method thereof and a catalytic body containing the honeycomb ceramic carrier. Background Art
[0002] With the upgrading of vehicle exhaust emission regulations, carbon monoxide (CO), hydrocarbons (C x H y ) and nitrogen oxides (NO x ) and other harmful gases are becoming more stringent, which puts higher requirements on the pore density and wall thickness of honeycomb ceramic carriers. High-density, thin-walled honeycomb ceramic materials can make harmful substances in exhaust gas react with the precious metal coating on the surface of the ceramic material more quickly to achieve harmless catalytic reaction.
[0003] At present, the honeycomb ceramic carriers provided by the prior art still have the following problems to be solved: 1. As the carrier pore density increases and the wall thickness decreases, the difficulty of product molding increases. The molding of thin-walled products easily leads to bending of the partition walls, and the bending of the partition walls of the carrier will have a serious impact on the overall performance of the carrier; 2. The curved lattice walls will affect the flow of exhaust gas in the catalyst, and cause uneven heat conduction due to the partition walls, reducing the catalytic efficiency; 3. The curved partition walls may block the gas channel, affect the exhaust gas treatment efficiency, and cause engine performance to decline; 4. The curved partition walls will reduce the structural strength and stability of the cordierite honeycomb ceramics, shorten the service life, and require frequent replacement or maintenance; 5. At present, high-pore density, thin-walled carriers are generally right-angle or rounded structures. The stress concentration at the right angles can easily lead to damage to the carrier, and the short service life affects the comprehensive performance of the carrier. Secondly, the right-angle structure mold mud has a large flow resistance, which can easily lead to bending of the partition walls and a low yield rate.
[0004] Therefore, how to improve the structural strength of the ceramic carrier used to carry the catalyst and reduce the bending of the partition walls of the thin-walled ceramic carrier with a honeycomb structure without increasing the degree of mold wear, thereby improving the yield, needs to be solved urgently. Summary of the invention
[0005] The object of the present invention is to provide a honeycomb ceramic carrier, a preparation method thereof and a catalyst body containing the honeycomb ceramic carrier, so as to improve the structural strength of the honeycomb ceramic carrier used to carry the catalyst, and reduce the bending phenomenon of the partition walls of the thin-walled ceramic carrier with a honeycomb structure without increasing the degree of mold wear, thereby improving the yield.
[0006] To achieve the above object, the present invention provides the following technical solutions:
[0007] A honeycomb ceramic carrier, comprising:
[0008] ontology;
[0009] A plurality of compartments with a hollow structure in the body, the compartments penetrating the body to form a honeycomb structure;
[0010] The compartment has a quadrilateral cross section, a pair of opposite corners of the quadrilateral cross section have an inner recess or a chamfer, and the other pair of opposite corners of the quadrilateral cross section do not have an inner recess or a chamfer.
[0011] In some embodiments of the present invention, in one of the compartments, in a pair of opposite corners having the inner recess or chamfer, two apex corners have the same shape and size;
[0012] Alternatively, in one of the compartments, in a pair of opposite corners having the inner recess or chamfer, two apex corners have different shapes and / or different sizes.
[0013] In some embodiments of the present invention, the four compartments constitute a repeating unit, and the repeating unit has a symmetry center;
[0014] Wherein, the top corners of the four compartments in the repeating unit located inside the repeating unit have the recessed portion or chamfered corner, or the top corners of the four compartments in the repeating unit located inside the repeating unit do not have the recessed portion or chamfered corner.
[0015] In some embodiments of the present invention, the number of the compartments is at least twelve;
[0016] Wherein, each of the compartments constitutes a quarter of at least two repeating units.
[0017] In some embodiments of the present invention, in a repeating unit, the apex corners of the four compartments located inside the repeating unit and having the inner concave portion or chamfer are enclosed and form a reinforced intersection at the position of the symmetry center;
[0018] Alternatively, in a repeating unit, the vertices of the four compartments located inside the repeating unit and presenting outwardly convex right angles are enclosed and form a common intersection at the position of the symmetry center.
[0019] In some embodiments of the present invention, the inner concave portion is an inner concave right angle, a rounded angle, or an inner concave flower angle;
[0020] The concave right angle is configured to be concave relative to the interior of the compartment where it is located, and the rounded corner is configured to be convex or concave relative to the interior of the compartment where it is located.
[0021] In some embodiments of the present invention, the water absorption rate of the honeycomb ceramic carrier is 14-28%.
[0022] In some embodiments of the present invention, the honeycomb ceramic substrate has one or more of the following features:
[0023] The water absorption rate of the honeycomb ceramic carrier is 14-28%;
[0024] The compressive strength of the ceramic carrier in the longitudinal direction is 9 to 10.5 MPa;
[0025] The thermal expansion coefficient CTE of the ceramic carrier in the longitudinal direction in the temperature range of 25 to 800° C. is 0.2×10 -6 ~0.5×10 -6 ℃ -1 ;
[0026] The isostatic strength of the ceramic carrier is 3.1 to 6.3 MPa;
[0027] The thermal shock parameter TSP of the ceramic carrier is 650°C to 750°C, preferably 700°C to 750°C;
[0028] The size of the ceramic carrier in the longitudinal direction is 3 to 5.5 inches;
[0029] The radial dimension of the ceramic carrier is 3.7 to 5.6 inches;
[0030] In the ceramic carrier, the density of the compartment is 600 to 1200 cpsi;
[0031] The thickness of the partition wall between two adjacent compartments in the ceramic carrier is 2 to 4 mils.
[0032] In some embodiments of the present invention, in each of the compartments, two apex angles of a pair of diagonal angles without the inner recess or chamfer are right angles, and each right angle is formed by two first straight line segments, one of the first straight line segments has a length of A1, and the other of the first straight line segments has a length of B1;
[0033] Each vertex of a pair of diagonal corners having the inner concave portion is formed by two second straight line segments, wherein the length of one of the second straight line segments is A2, and the length of the other second straight line segment is B2;
[0034] Among them, (A2 / A1)*100%=5-25%, preferably 15-25%, (B2 / B1)*100%=5-25%, preferably 15-25%.
[0035] In some embodiments of the present invention, in each of the compartments, two apex angles of a pair of diagonal angles without the inner recess or chamfer are right angles, and each right angle is formed by two first straight line segments, one of the first straight line segments has a length of A1, and the other of the first straight line segments has a length of B1;
[0036] Each vertex of a pair of opposite corners with the chamfer is formed by a third straight line segment, the projection length of the third straight line segment in the direction where one of the first straight line segments is located is A3, and the projection length of the third straight line segment in the direction where another of the first straight line segments is located is B3;
[0037] Among them, (A3 / A1)*100%=5-25%, preferably 15-25%, (B3 / B1)*100%=5-25%, preferably 15-25%.
[0038] In some embodiments of the present invention, in each of the compartments, two apex angles of a pair of diagonal angles without the inner recess or chamfer are right angles, and each right angle is formed by two first straight line segments, one of the first straight line segments has a length of A1, and the other of the first straight line segments has a length of B1;
[0039] Each vertex of a pair of diagonal corners having the inner concave portion is formed by an arc segment, the projection length of the arc segment in the direction where one of the first straight line segments is located is A4, and the projection length of the arc segment in the direction where another of the first straight line segments is located is B4;
[0040] Among them, (A4 / A1)*100%=5-25%, preferably 15-25%, (B4 / B1)*100%=5-25%, preferably 15-25%.
[0041] In some embodiments of the present invention, in each of the compartments, two apex angles of a pair of diagonal angles without the inner recess or chamfer are right angles, and each right angle is formed by two first straight line segments, one of the first straight line segments has a length of A1, and the other of the first straight line segments has a length of B1;
[0042] Each vertex of a pair of diagonal angles having the inner concave portion is composed of four sequentially connected fourth straight line segments, the sum of the projection lengths of the four fourth straight line segments in the direction where one of the first straight line segments is located is A5, and the sum of the projection lengths of the four fourth straight line segments in the direction where another of the first straight line segments is located is B5;
[0043] Among them, (A5 / A1)*100%=5-25%, preferably 15-25%, (B5 / B1)*100%=5-25%, preferably 15-25%.
[0044] In some embodiments of the present invention, the raw materials of the ceramic carrier include inorganic raw materials, organic additives, binders and water;
[0045] The inorganic raw materials are talc, kaolin, alumina and optionally silicon oxide and aluminum hydroxide, wherein the talc is preferably flaky talc, more preferably flaky talc with D50=5-20 μm; the kaolin is preferably raw kaolin and / or cooked kaolin, the raw kaolin is more preferably flaky raw kaolin, the flaky raw kaolin is more preferably flaky raw kaolin with D50=5-20 μm, the cooked kaolin is more preferably cooked kaolin with D50=4-15 μm, the silicon oxide is preferably silicon oxide with D50=1-10 μm, and the aluminum oxide is preferably aluminum oxide with D50=1-10 μm;
[0046] The organic auxiliary agent is at least one of alkyl polyether, fatty alcohol polyoxyethylene ether, xanthan gum, potassium laurate, and glycerol random polyether;
[0047] The binder is at least one of hydroxymethyl cellulose, ethyl cellulose and carboxymethyl cellulose.
[0048] In some embodiments of the present invention, based on the total amount of inorganic raw materials as 100wt.%, the talc accounts for 20-40wt.%, the kaolin accounts for 20-60wt.%, the alumina accounts for 10-20wt.%, the silicon oxide accounts for 0-10wt.%, the organic additive accounts for 2-10wt.% relative to the total amount of inorganic raw materials, the binder accounts for 3-15wt.% relative to the total amount of inorganic raw materials, and the water accounts for 25-50wt.% relative to the total amount of inorganic raw materials.
[0049] Preferably, the kaolin comprises 10-30 wt.% of flaky raw kaolin and 10-30 wt.% of cooked kaolin, based on the total amount of inorganic raw materials being 100 wt.%.
[0050] In order to achieve the above object, the present invention also provides the following technical solutions:
[0051] A method for preparing a honeycomb ceramic carrier, the method comprising the following steps:
[0052] S1, mixing inorganic raw materials to obtain dry materials;
[0053] S2, the dry material obtained in step S1 is mixed with an organic additive, a binder, and water in sequence through wet mixing, kneading, mud kneading, extrusion molding, drying, and cutting to obtain a green body;
[0054] S3, sintering the green body obtained in step S2 to obtain the honeycomb ceramic carrier;
[0055] Wherein, the compartment of the honeycomb ceramic carrier is formed during the extrusion molding process in step S2, and the compartment has a quadrilateral cross section, a pair of diagonals of the quadrilateral cross section have a recess or chamfer, and the other pair of diagonals of the quadrilateral cross section do not have a recess or chamfer.
[0056] In some embodiments of the present invention, in step S3, during the sintering process, the heating rate and the sintering temperature at least at part of the time vary with the sintering time.
[0057] In some embodiments of the present invention, in step S3, the sintering temperature is 1000° C. to 1450° C., the sintering time is at least 13 hours, and the heating rate is greater than 25° C. / h.
[0058] In some embodiments of the present invention, in step S2, the wet mixing includes: putting the dry material, binder, and organic additive into a plowshare mixer for dry mixing, and then spraying water for wet mixing;
[0059] The mud preparation includes: putting the wet mixed raw materials into a mesh mud preparation machine to prepare the mud under vacuum conditions;
[0060] The extrusion molding comprises: putting the raw material after mud kneading into an extruder, preferably at least one selected from a single-screw extruder, a twin-screw extruder or a hydraulic extruder, for molding;
[0061] The drying comprises: using a microwave dryer to dry and shape;
[0062] The cutting includes: cutting with a blank cutting machine.
[0063] In order to achieve the above object, the present invention also provides the following technical solutions:
[0064] A catalyst body, comprising the above-mentioned honeycomb ceramic carrier, wherein the inner wall surface of the compartment of the honeycomb ceramic carrier is coated with a catalyst;
[0065] Preferably, the catalyst coating thickness at the top corner positions having the inner concave portion or chamfered structure is 0.06-0.08 μm, and the coating thickness at other positions is 0.07 μm.
[0066] Further areas of applicability will become apparent from the description provided in the present disclosure.
[0067] The description and specific examples in this summary are intended for purposes of illustration only and are not intended to limit the scope of the present disclosure.
[0068] Compared with the prior art, the present invention has the following beneficial effects through the above technical solution:
[0069] The present invention improves the structural strength of a ceramic carrier for carrying a catalyst and reduces the bending phenomenon of the partition wall of a thin-walled ceramic carrier with a honeycomb structure without increasing the degree of mold wear, thereby improving the yield rate. BRIEF DESCRIPTION OF THE DRAWINGS
[0070] In order to more clearly illustrate the technical solutions in the embodiments of the present invention, the drawings required for use in the description of the embodiments will be briefly introduced below. Obviously, the drawings described below are only some implementation plans of the present invention. For those skilled in the art, other drawings can be obtained based on these drawings without paying any creative work.
[0071] Figure 1 A schematic structural diagram of a compartment of a honeycomb ceramic carrier provided in the first embodiment of the present invention;
[0072] Figure 2 A schematic structural diagram of a compartment of a honeycomb ceramic carrier provided in a second embodiment of the present invention;
[0073] Figure 3 A schematic structural diagram of a compartment of a honeycomb ceramic carrier provided in a third embodiment of the present invention;
[0074] Figure 4 A schematic structural diagram of a compartment of a honeycomb ceramic carrier provided in a fourth embodiment of the present invention;
[0075] Figure 5 A schematic structural diagram of a compartment of a honeycomb ceramic carrier provided in a fifth embodiment of the present invention;
[0076] Figure 6 A schematic diagram of the dimensions of the compartments of the honeycomb ceramic carrier provided in the first embodiment of the present invention;
[0077] Figure 7 A schematic diagram of the dimensions of the compartments of the honeycomb ceramic carrier provided in the second embodiment of the present invention;
[0078] Figure 8 A schematic diagram of the dimensions of the compartments of the honeycomb ceramic carrier provided in the third embodiment of the present invention;
[0079] Fig. 9 A schematic diagram of the dimensions of the compartments of the honeycomb ceramic carrier provided in the fourth embodiment of the present invention;
[0080] Fig.10 A schematic diagram of the dimensions of the compartments of the honeycomb ceramic carrier provided in the fifth embodiment of the present invention;
[0081] Fig.11 A schematic diagram of the structure of a honeycomb ceramic carrier provided in one embodiment of the present invention;
[0082] Fig.12 for Fig.11 A schematic cross-sectional view of a honeycomb ceramic carrier;
[0083] Fig.13 A flowchart of a preparation method provided in one embodiment of the present invention.
[0084] The main reference numerals in the drawings of this application specification are described as follows:
[0085] 1-main body; 2-compartment; 31-reinforced intersection; 32-ordinary intersection. DETAILED DESCRIPTION
[0086] The technical solutions in the embodiments of the present invention are described clearly and completely below. Obviously, the described embodiments are only a part of the embodiments of the present invention, rather than all the embodiments. Based on the embodiments in the present invention, all other embodiments obtained by those skilled in the art without creative work belong to the scope of protection of the present invention. It should be understood that the specific embodiments described herein are only used to illustrate and explain the present invention, and are not used to limit the present invention.
[0087] Any specific numerical value disclosed herein (including the endpoint of the numerical range) is not limited to the exact value of the numerical value, but should be understood to also cover values close to the exact value, such as all possible numerical values within the range of ±5% of the exact value. In addition, for the disclosed numerical range, the endpoint values of the range, the endpoint values and the specific point values in the range, and the specific point values can be arbitrarily combined to obtain one or more new numerical ranges, and these new numerical ranges should also be regarded as specifically disclosed herein.
[0088] The terms used in the present disclosure are only intended to describe specific exemplary embodiments and are not intended to be limiting. Unless the context clearly indicates otherwise, the singular forms "one", "a kind of" and "the" as used in the present disclosure may be intended to also include plural forms. The terms "comprising", "including", "containing" and "having" are inclusive, thus illustrating the presence of the features, elements, compositions, steps, integers, operations and / or components, but do not exclude the presence or addition of one or more other features, integers, steps, operations, elements, components and / or their collections. Although the open term "comprising" should be understood as a non-limiting term for describing and claiming the various embodiments described in the present disclosure, in some aspects, the term may be alternatively understood as a more restrictive and limited term, such as "consisting of" or "consisting essentially of". Thus, for any given embodiment of a narration composition, material, component, element, feature, integer, operation and / or process step, the present disclosure also particularly includes an embodiment consisting of or essentially consisting of such a composition, material, component, element, feature, integer, operation and / or process step. In the case of "consisting of," alternative embodiments exclude any additional compositions, materials, components, elements, features, integers, operations and / or process steps, while in the case of "consisting essentially of," any additional compositions, materials, components, elements, features, integers, operations and / or process steps that materially affect the basic and novel characteristics are excluded from such embodiments, but any compositions, materials, components, elements, features, integers, operations and / or process steps that do not materially affect the basic and novel characteristics may be included in the embodiments.
[0089] Any method steps, processes, and operations described in the present disclosure should not be construed as necessarily requiring their performance in the particular order discussed or illustrated, unless expressly identified as a certain order of performance. It should also be understood that additional or alternative steps may be used unless otherwise stated.
[0090] In this application, except for the contents explicitly described, any matters or items not mentioned are directly applicable to those known in the art without any changes. Moreover, any embodiment described in this disclosure can be freely combined with one or more other embodiments described in this disclosure, and the technical solutions or technical ideas formed thereby are regarded as part of the original disclosure or original record of this application, and should not be regarded as new contents that have not been disclosed or anticipated in this disclosure, unless a person skilled in the art considers that the combination is obviously unreasonable.
[0091] Unless otherwise specified, the terms used herein have the same meaning as commonly understood by those skilled in the art. If a term is defined herein and its definition is different from the commonly understood meaning in the art, the definition herein shall prevail.
[0092] Unless otherwise stated, when % is mentioned herein, it means wt. %.
[0093] It is worth noting that "cpsi" in the present application specification refers to channels per square inch, which means "the number of channels per square inch of cross-section", which is generally referred to as "mesh size"; and "mil" in the present application specification refers to "mil" or "milliinch", which is a unit of length, and the conversion relationship is 1 inch (inch) = 1000 mil (mil), 1 mil = 25.4 μm (micrometer), 25.4 mm = 1000 mil.
[0094] In the context of the present invention, calcined kaolin is used interchangeably with cooked kaolin.
[0095] It should be noted that the "thermal expansion coefficient" in the present application specification refers to the ratio of the change in length of a solid substance in a certain direction when the temperature changes by 1°C to its length at 20°C (i.e., standard laboratory environment); further, the thermal expansion coefficient of the ceramic carrier recorded in the present application specification refers to the thermal expansion coefficient in the longitudinal direction of the ceramic carrier; it is worth emphasizing that it is well known to those skilled in the art that the longitudinal axis of the above-mentioned ceramic carrier refers to the A-axis.
[0096] It is understood that the "water absorption rate" in the specification of this application refers to the dry mass and the mass after saturation after the ceramic carrier sample is placed in water and absorbed water to saturation. The water absorption rate recorded in the specification of this application is measured under the following standards: the ceramic carrier provided by the present invention is made into a sample block of 25*25*25mm±0.5mm, and the dry weight of the sample block is weighed; after vacuuming with a vacuum pump for 10 minutes, it is boiled in a microwave oven, and after being placed at room temperature, the excess water of the sample block is blown away with an air gun, and the weight of the sample block is weighed to calculate the water absorption rate; the dry weight is the sample taken out of the kiln without additional drying.
[0097] It should be noted that the "ratio of the size of the vertex with the non-convex right-angle design to the side length where the vertex is located" in the specification of this application refers to the ratio of the side length of the quadrilateral compartment occupied by the non-convex right-angle design structure; "the thickness of the partition wall between two adjacent compartments" refers to the thickness of the porous wall between the compartments, which is the thickness between the sides of the quadrilateral compartment not occupied by the non-convex right-angle design structure; "the size of the ceramic carrier in the longitudinal direction" refers to the distance from the inlet end to the outlet end of the honeycomb structure ceramic carrier; "the radial size of the ceramic carrier" refers to the diameter of the inlet end face or the outlet end face of the honeycomb structure ceramic carrier. The cross-sectional shape of the carrier in some embodiments is any one of a circle, an ellipse, and a polygon. In the case of an ellipse, the radial size refers to the size of the major axis of the ellipse. In the case of a polygon or other shape, the radial size refers to the longest dimension of the shape.
[0098] First aspect
[0099] See also Fig.11 and Fig.12 A honeycomb ceramic carrier comprises: a body 1; a plurality of compartments 2 with a hollow structure in the body 1, the compartments 2 penetrate the body 1 to form a honeycomb structure; wherein the compartments 2 have a quadrilateral cross section, a pair of diagonal corners of the quadrilateral cross section have an inner recess or chamfer, and the other pair of diagonal corners of the quadrilateral cross section do not have an inner recess or chamfer.
[0100] In the prior art, ceramic carriers with high pore density and thin-walled structures generally have straight-through compartments with right angles or rounded corners. The stress concentration at the right angle position may easily lead to overall damage to the ceramic carrier, thereby reducing the product life and affecting the comprehensive performance of the carrier. Secondly, the mold clay used to press out the right-angle structure will also have the disadvantage of large flow resistance due to the inherent morphological properties of the right-angle shape itself, which may easily lead to bending and skewing of the inner wall of the compartment of the ceramic carrier, thereby resulting in low product yield. The present invention provides a honeycomb ceramic carrier with "a quadrilateral cross section, a pair of diagonals of the quadrilateral cross section having a straight-through compartment with an inner recess or chamfer and the other pair of diagonals of the quadrilateral cross section having no inner recess or chamfer", which can reduce the bending of thin-walled honeycomb ceramic partitions without increasing the degree of wear of the honeycomb ceramic mold, thereby significantly improving the product yield.
[0101] See also Figures 1 to 12 In some embodiments of the present invention, in one of the compartments 2, in a pair of opposite corners having the inner recess or chamfer, the two apex corners have the same shape and size.
[0102] In some embodiments of the present invention, in one of the compartments 2, in a pair of opposite corners having the inner recess or chamfer, two apex corners have different shapes and / or different sizes.
[0103] See also Figures 1 to 12 In some embodiments of the present invention, the four compartments 2 constitute a repeating unit having a center of symmetry; wherein the top corners of the four compartments 2 in the repeating unit, which are located inside the repeating unit, have the recessed portion or chamfered corner.
[0104] See also Figures 1 to 12 In some embodiments of the present invention, the four compartments 2 constitute a repeating unit having a center of symmetry; wherein the top corners of the four compartments 2 in the repeating unit that are located inside the repeating unit have the recessed portion or chamfered portion, and the top corners of the four compartments 2 in the repeating unit that are located inside the repeating unit do not have the recessed portion or chamfered portion.
[0105] See also Figures 1 to 5 , Fig.11 as well as Fig.12 In some embodiments of the present invention, the number of the compartments 2 is at least twelve; wherein each of the compartments 2 constitutes a quarter of at least two of the repeating units.
[0106] See also Figures 1 to 5 , Fig.11 as well as Fig.12 In some embodiments of the present invention, in a repeating unit, the vertices of the four compartments 2 located inside the repeating unit and in a convex right angle are enclosed and form a common intersection 32 at the position of the symmetry center.
[0107] See also Figures 1 to 5 , Fig.11 as well as Fig.12 In some embodiments of the present invention, in a repeating unit, the top corners of the four compartments 2 located inside the repeating unit and having the recessed portion or chamfered angle are enclosed and a reinforced intersection 31 is formed at the position of the symmetry center.
[0108] See also Figures 1 to 5 , Fig.11 as well as Fig.12 The radial dimension of the reinforced intersection 31 is obviously larger than the radial dimension of the ordinary intersection 32; it can be understood that, when other parameters are the same, the increase in the radial dimension of the structure at this location can improve the structural strength of the honeycomb ceramic carrier, thereby enhancing the durability of the honeycomb ceramic carrier and reducing or even avoiding the occurrence of adverse phenomena such as distortion and deformation of the inner wall of the compartment.
[0109] See also Figure 1 and Figure 6 In some embodiments of the present invention, the recessed portion is a recessed right angle, and the recessed right angle is configured to be recessed relative to the interior of the compartment 2 where it is located.
[0110] See also Figure 3 , Figure 4 , Figure 7 and Figure 8 In some embodiments of the present invention, the inner recess is a rounded corner, and the rounded corner is configured to be convex or concave relative to the interior of the compartment 2 where it is located.
[0111] In some embodiments of the present invention, the water absorption rate of the honeycomb ceramic carrier is 14-28%, preferably 16-24%. The water absorption rate is, for example, 14%, 16%, 18%, 20%, 22%, 24%, 26% and 28%, any range consisting of these values and any value falling between the above values.
[0112] In some embodiments of the present invention, the compressive strength of the ceramic carrier in the longitudinal direction is 9 to 10.5 MPa. The compressive strength is, for example, 9 MPa, 9.1 MPa, 9.2 MPa, 9.3 MPa, 9.4 MPa, 9.5 MPa, 9.6 MPa, 9.7 MPa, 9.8 MPa, 9.9 MPa, 10 MPa, 10.1 MPa, 10.2 MPa, 10.3 MPa, 10.4 MPa and 10.5 MPa, any range consisting of these values and any value falling between the above values.
[0113] In some embodiments of the present invention, the thermal expansion coefficient CTE of the ceramic carrier in the longitudinal direction within a temperature range of 25 to 800° C. is 0.2×10 -6 ~0.5×10 -6 ℃ -1 The thermal expansion coefficient is, for example, 0.2×10 -6 ℃ -1 , 0.25×10 -6 ℃ -1 , 0.3×10 -6 ℃ -1 , 0.35×10 -6 ℃ -1 , 0.4×10 -6 ℃ -1 , 0.45×10 -6 ℃ -1 , 0.5×10 -6 ℃ -1 , any ranges consisting of these values and any values falling between the above values.
[0114] In some embodiments of the present invention, the isostatic strength of the ceramic carrier is 3.1-6.3 MPa. The isostatic strength is, for example, 3.1 MPa, 3.3 MPa, 3.5 MPa, 3.7 MPa, 4 MPa, 4.2 MPa, 4.4 MPa, 4.6 MPa, 4.8 MPa, 5 MPa, 5.2 MPa, 5.4 MPa, 5.6 MPa, 5.8 MPa, 6 MPa, 6.1 MPa and 6.3 MPa, any ranges consisting of these values and any values falling between the above values.
[0115] In some embodiments of the present invention, the thermal shock parameter TSP of the ceramic carrier is 650°C to 750°C, preferably 700 to 750°C.
[0116] In some embodiments of the present invention, the longitudinal length of the ceramic carrier is 3 to 5.5 inches. The longitudinal length is, for example, 3 inches, 3.2 inches, 3.4 inches, 3.6 inches, 3.8 inches, 4 inches, 4.2 inches, 4.4 inches, 4.6 inches, 4.8 inches, 5 inches, 5.2 inches, 5.4 inches and 5.5 inches, any ranges formed by these values and any values falling between the above values.
[0117] In some embodiments of the present invention, the radial dimension of the ceramic carrier is 3.7 to 5.6 inches, such as 3.7 inches, 3.8 inches, 4 inches, 4.2 inches, 4.4 inches, 4.6 inches, 4.8 inches, 5 inches, 5.2 inches, 5.4 inches and 5.6 inches, any range formed by these values and any value falling between the above values.
[0118] In some embodiments of the present invention, in the ceramic carrier, the density of the compartment 2 is 600-1200 cpsi. The density of the compartment is, for example, 600 cpsi, 700 cpsi, 800 cpsi, 900 cpsi, 1000 cpsi, 1100 cpsi and 1200 cpsi, any range consisting of these values and any value falling between the above values.
[0119] In some embodiments of the present invention, the thickness of the partition wall between two adjacent compartments 2 in the ceramic carrier is 2-4 mil.
[0120] See also Figure 1 and Figure 6 In some embodiments of the present invention, in each of the compartments 2, the two vertices in a pair of diagonals without the recessed portion or chamfered angle are both right angles, and each right angle is composed of two first straight line segments, one of which has a length of A1, and the other has a length of B1; each vertices in a pair of diagonals with the recessed portion are composed of two second straight line segments, one of which has a length of A2, and the other has a length of B2; wherein, (A2 / A1)*100%=5~25%, preferably 15~25%, (B2 / B1)*100%=5~25%, preferably 15~25%,
[0121] See also Figure 2 and Figure 7In some embodiments of the present invention, in each of the compartments 2, the two vertices of a pair of diagonals without the inner recess or chamfer are right angles, and each right angle is composed of two first straight line segments, the length of one first straight line segment is A1, and the length of the other first straight line segment is B1; each vertices of a pair of diagonals with the chamfer is composed of a third straight line segment, the projection length of the third straight line segment in the direction of one of the first straight line segments is A3, and the projection length of the third straight line segment in the direction of the other first straight line segment is B3; wherein, (A3 / A1)*100%=5~25%, preferably 15~25%, (B3 / B1)*100%=5~25%, preferably 15~25%.
[0122] See also Figure 3 , Figure 4 , Figure 7 and Figure 8 In some embodiments of the present invention, in each of the compartments 2, the two vertices of a pair of diagonals without the inner recess or chamfer are right angles, and each right angle is composed of two first straight line segments, the length of one first straight line segment is A1, and the length of the other first straight line segment is B1; each vertices of a pair of diagonals with the inner recess is composed of an arc segment, the projection length of the arc segment in the direction of one of the first straight line segments is A4, and the projection length of the arc segment in the direction of the other first straight line segment is B4; wherein, (A4 / A1)*100%=5~25%, preferably 15~25%, (B4 / B1)*100%=5~25%, preferably 15~25%.
[0123] See also Figure 5 and Fig.10 In some embodiments of the present invention, in each of the compartments 2, the two vertices of a pair of diagonals without the recessed portion or chamfered angle are both right angles, and each right angle is composed of two first straight line segments, the length of one first straight line segment is A1, and the length of the other first straight line segment is B1; each vertices of a pair of diagonals with the recessed portion is composed of four sequentially connected fourth straight line segments, the sum of the projection lengths of the four fourth straight line segments in the direction of one of the first straight line segments is A5, and the sum of the projection lengths of the four fourth straight line segments in the direction of another of the first straight line segments is B5; wherein, (A5 / A1)*100%=5~25%, preferably 15~25%, (B5 / B1)*100%=5~25%, preferably 15~25%.
[0124] It can be understood that the present invention provides a straight-through honeycomb ceramic body with special compartments, and the compartments are quadrilaterals with a pair of special diagonal structures. In the honeycomb ceramic body, the compartments are arranged in mirror symmetry with the adjacent compartments. The special structures of the diagonals of the compartments include beveled edges, inner arc edges, outer arc edges, and inner right-angle structures. The honeycomb ceramic carrier with this structure improves the problem of the bending of the partition walls, and its yield rate and the comprehensive performance of the carrier are similar to those of the four chamfered and rounded honeycomb ceramics, which reduces the wear of the honeycomb ceramic mold; the above-mentioned special compartment structure can improve the fluidity of the mud, reduce and avoid the bending of the partition walls, improve the compressive strength of the honeycomb ceramic body, and improve the yield rate. This structure can reduce the wear on the mold and reduce the amount of catalyst coating.
[0125] In some embodiments of the present invention, the raw materials of the ceramic carrier include inorganic raw materials, organic additives, binders and water.
[0126] In some embodiments of the present invention, the inorganic raw materials are talc, kaolin, alumina and optionally silicon oxide and aluminum hydroxide.
[0127] In some embodiments of the present invention, the talc is preferably flaky talc, more preferably flaky talc with D50=5-20 μm.
[0128] In some embodiments of the present invention, the kaolin is preferably raw kaolin and / or cooked kaolin, the raw kaolin is more preferably flaky raw kaolin, the flaky raw kaolin is more preferably flaky raw kaolin with D50=5-20 μm, and the cooked kaolin is more preferably cooked kaolin with D50=4-15 μm.
[0129] In some embodiments of the present invention, the silicon oxide is preferably silicon oxide with D50=1 to 10 μm, and the aluminum oxide is preferably aluminum oxide with D50=1 to 10 μm.
[0130] In some embodiments of the present invention, the organic auxiliary agent is at least one of alkyl polyether, fatty alcohol polyoxyethylene ether, xanthan gum, potassium laurate, and glycerol random polyether.
[0131] In some embodiments of the present invention, the binder is at least one of hydroxymethyl cellulose, ethyl cellulose, and carboxymethyl cellulose.
[0132] In some embodiments of the present invention, based on the total amount of inorganic raw materials as 100wt.%, the talc accounts for 20-40wt.%, the kaolin accounts for 20-60wt.%, the aluminum oxide accounts for 10-20wt.%, the silicon oxide accounts for 0-10wt.%, the organic additive accounts for 2-10wt.% relative to the total amount of inorganic raw materials, the binder accounts for 3-15wt.% relative to the total amount of inorganic raw materials, and the water accounts for 25-50wt.% relative to the total amount of inorganic raw materials.
[0133] Preferably, the kaolin comprises 10-30 wt.% of flaky raw kaolin and 10-30 wt.% of cooked kaolin, based on the total amount of inorganic raw materials being 100 wt.%.
[0134] Second aspect
[0135] See also Fig.13 A method for preparing a honeycomb ceramic carrier comprises the following steps: S1, mixing inorganic raw materials to obtain dry materials; S2, mixing the dry materials obtained in step S1 with organic additives, binders and water in sequence through wet mixing, kneading, mud kneading, extrusion molding, drying and cutting to obtain a green body; S3, sintering the green body obtained in step S2 to obtain the above-mentioned honeycomb ceramic carrier; wherein, during the extrusion molding process in step S2, a compartment 2 of the honeycomb ceramic carrier is formed, and the compartment 2 has a quadrilateral cross section, a pair of opposite corners of the quadrilateral cross section have an inner recess or chamfer, and the other pair of opposite corners of the quadrilateral cross section do not have an inner recess or chamfer.
[0136] In some embodiments of the present invention, in step S3, during the sintering process, the heating rate and the sintering temperature at least at part of the time vary with the sintering time.
[0137] In some embodiments of the present invention, in step S3, the sintering temperature is 1000° C. to 1450° C., the sintering time is at least 13 hours, and the heating rate is greater than 25° C. / h.
[0138] In some embodiments of the present invention, in the step S2, the wet mixing includes: putting the dry material, binder, and organic additive into a plowshare mixer for dry mixing, and then wet mixing after spraying water; the mud kneading includes: putting the raw materials after wet mixing into a mesh mud kneading machine, and kneading under vacuum conditions; the extrusion molding includes: putting the raw materials after mud kneading into an extruder, preferably selected from at least one of a single-screw extruder, a twin-screw extruder or a hydraulic extruder, for molding, and then obtaining the compartment 2 through a mold; the drying includes: using a microwave dryer for drying and molding; the cutting includes: using a blank cutting machine for cutting.
[0139] Through the above preparation method, a straight-through honeycomb ceramic body with special compartments can be obtained, and the compartments are quadrilaterals with a pair of special diagonal structures. In the honeycomb ceramic body, the compartments are arranged in mirror symmetry with adjacent compartments. The product has uniform stress distribution, uniform mud extrusion, high yield rate, good compression and seismic resistance, reduced catalyst coating, and small mold loss. The straight-through honeycomb ceramic special structure of the present invention achieves the effects of reducing carrier wave walls, improving yield rate, improving compressive strength, reducing the amount of precious metal coating, and enhancing the service life of the mold. That is, the yield rate of the honeycomb ceramic carrier of this special structure is about 10%-20% higher than that of the right-angle structure, and the service life of the mold is much higher than that of the four-corner rounded structure. The change in the groove width of the mold for every 5000 meters of extrusion is between 0.1-0.2mil, which is similar to the change in the groove width of the rectangular structure mold. The coating thickness of the precious metal at the special structure is about 1 / 2 of the right-angle structure. The honeycomb ceramic carrier of the quadrilateral compartment with a pair of special diagonal structures of the present invention has a higher yield rate than the right-angle structure, and the coating amount of precious metal is reduced. The service life of the mold with rounded corners is increased, and the advantages of rounded corners and right-angle structures are combined.
[0140] The third aspect
[0141] A catalytic body comprises the above-mentioned honeycomb ceramic carrier, wherein the inner wall surface of the compartment 2 of the honeycomb ceramic carrier is coated with a catalyst; preferably, the catalyst coating thickness at the top corner position having the inner concave portion or chamfered structure is 0.06-0.08 μm, and the coating thickness at other positions is 0.07 μm.
[0142] Example 1
[0143] In this embodiment, 35wt.% of flaky talc, 19.2wt.% of flaky raw kaolin, 25.6wt.% of calcined kaolin, 5wt.% of silicon oxide, 15.2wt.% of aluminum oxide, 8.0wt.% of a binder and 3.9wt.% of a lubricant accounting for the total amount of inorganic raw materials are added to a plowshare mixer and dry mixed for 10 minutes at a rotation speed of 500rpm; after the dry mixing, 32wt.% of water relative to the inorganic raw materials is added for wet mixing for 15 minutes at a rotation speed of 500rpm; a honeycomb structure is then extruded using a 600-mesh, 3.7-inch diameter die; the cut length is 3.1 inches; and then dried at 50°C for 0.3h; the obtained green body is first heated at 250-310°C for 7h to debind, then sintered at 1430°C for 6h, and then naturally cooled to obtain the honeycomb ceramic carrier.
[0144] Example 2
[0145] In this embodiment, 25wt.% of flaky talc, 24.8wt.% of flaky raw kaolin, 30wt.% of calcined kaolin, 4wt.% of silicon oxide, 16.2wt.% of aluminum oxide, 8.6wt.% of the total amount of inorganic raw materials, and 3.5wt.% of the lubricant are added to a plow mixer and dry mixed for 10 minutes at a rotation speed of 500rpm; after the dry mixing, 33wt.% of water relative to the inorganic raw materials is added for wet mixing, the wet mixing time is 15min, and the rotation speed is 500rpm; then a honeycomb structure is extruded using a 750 mesh, 4.66-inch diameter die; the cut length is 3.1 inches; then it is dried at 50°C for 0.4h; the obtained green body is first heated at 250-310°C for 7h to debind, then sintered at 1430°C for 6h, and then naturally cooled to obtain the honeycomb ceramic carrier.
[0146] Example 3
[0147] In this embodiment, 30.6wt.% of flaky talc, 22.2wt.% of flaky raw kaolin, 30wt.% of calcined kaolin, 4wt.% of silicon oxide, 13.2wt.% of aluminum oxide, 8.6wt.% of a binder and 3.5wt.% of a lubricant accounting for the total amount of inorganic raw materials are added to a plowshare mixer and dry mixed for 10 minutes at a rotation speed of 500rpm; after the dry mixing, 33wt.% of water relative to the inorganic raw materials is added for wet mixing for 15 minutes at a rotation speed of 500rpm; then a honeycomb structure is extruded using a 800 mesh, 4.66-inch diameter die; the cut length is 5 inches; then it is dried at 50°C for 0.3h; the obtained green body is first heated at 250-310°C for 7h to debind, then sintered at 1430°C for 6h, and then naturally cooled to obtain the honeycomb ceramic carrier.
[0148] Example 4
[0149] In this embodiment, 35wt.% of flaky talc, 14.2wt.% of flaky raw kaolin, 30wt.% of calcined kaolin, 4.6wt.% of silicon oxide, 16.2wt.% of aluminum oxide, 7.6wt.% of a binder and 3.5wt.% of a lubricant accounting for the total amount of inorganic raw materials are added to a plowshare mixer for dry mixing for 10 minutes at a rotation speed of 500rpm; after the dry mixing, 35wt.% of water relative to the inorganic raw materials is added for wet mixing for 15 minutes at a rotation speed of 500rpm; a honeycomb structure is then extruded using a 900 mesh, 4.66-inch diameter die; the cut length is 3.94 inches; and then dried at 50°C for 0.4h; the obtained green body is first heated at 250-310°C for 7h to debind, then sintered at 1430°C for 6h, and then naturally cooled to obtain the honeycomb ceramic carrier.
[0150] Example 5
[0151] In this embodiment, 36wt.% of flaky talc, 19.2wt.% of flaky raw kaolin, 24.6wt.% of calcined kaolin, 4wt.% of silicon oxide, 16.2wt.% of aluminum oxide, 8.6wt.% of the total amount of inorganic raw materials, and 3.5wt.% of the lubricant are added to a plow mixer and dry mixed for 10 minutes at a rotation speed of 500rpm; after the dry mixing, 33wt.% of water relative to the inorganic raw materials is added for wet mixing, the wet mixing time is 15min, and the rotation speed is 500rpm; then a honeycomb structure is extruded using a 1200 mesh, 5.2-inch diameter die; the cut length is 3.94 inches; then it is dried at 50°C for 0.4h; the obtained green body is first heated at 250-310°C for 7h to debind, then sintered at 1430°C for 6h, and then naturally cooled to obtain the honeycomb ceramic carrier.
[0152] Example 6
[0153] In this embodiment, 25wt.% of flaky talc, 29.2wt.% of flaky raw kaolin, 25.6wt.% of calcined kaolin, 4wt.% of silicon oxide, 16.2wt.% of aluminum oxide, 12wt.% of a binder and 1.5wt.% of a lubricant accounting for the total amount of inorganic raw materials are added to a plowshare mixer and dry mixed for 10 minutes at a rotation speed of 500rpm; after the dry mixing, 50wt.% of water relative to the inorganic raw materials is added for wet mixing for 15 minutes at a rotation speed of 500rpm; a honeycomb structure is then extruded using a 600-mesh, 3.7-inch diameter die; the cut length is 3.1 inches; and then dried at 50°C for 0.3h; the obtained green body is first heated at 250-310°C for 7h to debind, then sintered at 1430°C for 6h, and then naturally cooled to obtain the honeycomb ceramic carrier.
[0154] Example 7
[0155] In this embodiment, 30wt.% of flaky talc, 23.2wt.% of flaky raw kaolin, 28.6wt.% of calcined kaolin, 4wt.% of silicon oxide, 14.2wt.% of aluminum oxide, 8.6wt.% of a binder and 3.5wt.% of a lubricant accounting for the total amount of inorganic raw materials are added to a plowshare mixer and dry mixed for 10 minutes at a rotation speed of 500rpm; after the dry mixing, 33wt.% of water relative to the inorganic raw materials is added for wet mixing for 15 minutes at a rotation speed of 500rpm; a honeycomb structure is then extruded using a 750 mesh, 3.7-inch diameter die; the cut length is 3.1 inches; and then dried at 50°C for 0.4h; the obtained green body is first heated at 250-310°C for 7h to debind, then sintered at 1430°C for 6h, and then naturally cooled to obtain the honeycomb ceramic carrier.
[0156] Example 8
[0157] In this embodiment, 38wt.% of flaky talc, 12wt.% of flaky raw kaolin, 30wt.% of calcined kaolin, 3wt.% of silicon oxide, 17wt.% of aluminum oxide, and 7wt.% of a binder and 7wt.% of a lubricant accounting for the total amount of inorganic raw materials are added to a plowshare mixer and dry mixed for 10 minutes at a rotation speed of 500rpm; after the dry mixing, 30wt.% of water relative to the inorganic raw materials is added for wet mixing for 15 minutes at a rotation speed of 500rpm; then a honeycomb structure is extruded using a 800-mesh, 3.7-inch diameter die; the cut length is 3.1 inches; then it is dried at 50°C for 0.4h; the obtained green body is first heated at 250-310°C for 7h to debind, then sintered at 1430°C for 6h, and then naturally cooled to obtain the honeycomb ceramic carrier.
[0158] Example 9
[0159] In this embodiment, 40wt.% of flaky talc, 20.2wt.% of flaky raw kaolin, 25.6wt.% of calcined kaolin, 3wt.% of silicon oxide, 11.2wt.% of aluminum oxide, and 6wt.% of a binder and 9wt.% of a lubricant accounting for the total amount of inorganic raw materials are added to a plowshare mixer and dry mixed for 10 minutes at a rotation speed of 500rpm; after the dry mixing, 29wt.% of water relative to the inorganic raw materials is added for wet mixing for 15 minutes at a rotation speed of 500rpm; a honeycomb structure is then extruded using a 900 mesh, 4.66-inch diameter die; the cut length is 3.1 inches; and then dried at 50°C for 0.4h; the obtained green body is first heated at 250-310°C for 7h to debind, then sintered at 1430°C for 6h, and then naturally cooled to obtain the honeycomb ceramic carrier.
[0160] Example 10
[0161] In this embodiment, 25wt.% of flaky talc, 24.2wt.% of flaky raw kaolin, 30wt.% of calcined kaolin, 4wt.% of silicon oxide, 16.8wt.% of aluminum oxide, 10wt.% of a binder and 2.5wt.% of a lubricant accounting for the total amount of inorganic raw materials are added to a plowshare mixer and dry mixed for 10 minutes at a rotation speed of 500rpm; after the dry mixing, 45wt.% of water relative to the inorganic raw materials is added for wet mixing for 15 minutes at a rotation speed of 500rpm; a honeycomb structure is then extruded using a 1200 mesh, 4.66-inch diameter die; the cut length is 5 inches; and then dried at 50°C for 0.4h; the obtained green body is first heated at 250-310°C for 7h to debind, then sintered at 1430°C for 6h, and then naturally cooled to obtain the honeycomb ceramic carrier.
[0162] Embodiment 11
[0163] In this embodiment, 30wt.% of flaky talc, 22.2wt.% of flaky raw kaolin, 30wt.% of calcined kaolin, 6wt.% of silicon oxide, 11.8wt.% of aluminum oxide, 9.2wt.% of the total amount of inorganic raw materials, and 2.6wt.% of the lubricant are added to a plow mixer and dry mixed for 10 minutes at a rotation speed of 500rpm; after the dry mixing, 39wt.% of water relative to the inorganic raw materials is added for wet mixing, the wet mixing time is 15min, and the rotation speed is 500rpm; then a honeycomb structure is extruded using a 600-mesh, 5.2-inch diameter die; the cut length is 3.94 inches; then it is dried at 50°C for 0.5h; the obtained green body is first heated at 250-310°C for 7h to debind, then sintered at 1430°C for 6h, and then naturally cooled to obtain the honeycomb ceramic carrier.
[0164] Example 12
[0165] In this embodiment, 37wt.% of flaky talc, 22.2wt.% of flaky raw kaolin, 25.6wt.% of calcined kaolin, 3wt.% of silicon oxide, 16.2wt.% of aluminum oxide, 8.6wt.% of the total amount of inorganic raw materials, and 3.5wt.% of the lubricant are added to a plow mixer and dry mixed for 10 minutes at a rotation speed of 500rpm; after the dry mixing, 33wt.% of water relative to the inorganic raw materials is added for wet mixing, the wet mixing time is 15min, and the rotation speed is 500rpm; then a honeycomb structure is extruded using a 600-mesh, 5.2-inch diameter die; the cut length is 3.94 inches; then it is dried at 50°C for 0.4h; the obtained green body is first heated at 250-310°C for 7h to debind, then sintered at 1430°C for 6h, and then naturally cooled to obtain the honeycomb ceramic carrier.
[0166] Embodiment 13
[0167] In this embodiment, 30wt.% of flaky talc, 23.2wt.% of flaky raw kaolin, 28.6wt.% of calcined kaolin, 3wt.% of silicon oxide, 15.2wt.% of aluminum oxide, 6.5wt.% of a binder and 5.5wt.% of a lubricant accounting for the total amount of inorganic raw materials are added to a plowshare mixer and dry mixed for 10 minutes at a rotation speed of 500rpm; after the dry mixing, 33wt.% of water relative to the inorganic raw materials is added for wet mixing for 15 minutes at a rotation speed of 500rpm; a honeycomb structure is then extruded using a 750 mesh, 5.2-inch diameter die; the cut length is 3.94 inches; and then dried at 50°C for 0.4h; the obtained green body is first heated at 250-310°C for 7h to debind, then sintered at 1430°C for 6h, and then naturally cooled to obtain the honeycomb ceramic carrier.
[0168] Embodiment 14
[0169] In this embodiment, 33wt.% of flaky talc, 22.2wt.% of flaky raw kaolin, 26.6wt.% of calcined kaolin, 5wt.% of silicon oxide, 13.2wt.% of aluminum oxide, 12wt.% of a binder and 2wt.% of a lubricant accounting for the total amount of inorganic raw materials are added to a plowshare mixer and dry mixed for 10 minutes at a rotation speed of 500rpm; after the dry mixing, 33wt.% of water relative to the inorganic raw materials is added for wet mixing for 15 minutes at a rotation speed of 500rpm; a honeycomb structure is then extruded using a 750 mesh, 5.2-inch diameter die; the cut length is 3.94 inches; and then dried at 50°C for 0.4h; the obtained green body is first heated at 250-310°C for 7h to debind, then sintered at 1430°C for 6h, and then naturally cooled to obtain the honeycomb ceramic carrier.
[0170] Embodiment 15
[0171] In this embodiment, 20wt.% of flaky talc, 25.2wt.% of flaky raw kaolin, 30.6wt.% of calcined kaolin, 8wt.% of silicon oxide, 16.2wt.% of aluminum oxide, 10wt.% of a binder and 3.5wt.% of a lubricant accounting for the total amount of inorganic raw materials are added to a plowshare mixer and dry mixed for 10 minutes at a rotation speed of 500rpm; after the dry mixing, 41wt.% of water relative to the inorganic raw materials is added for wet mixing for 15 minutes at a rotation speed of 500rpm; a honeycomb structure is then extruded using a 750 mesh, 5.2-inch diameter die; the cut length is 3.94 inches; and then dried at 50°C for 0.4h; the obtained green body is first heated at 250-310°C for 7h to debind, then sintered at 1430°C for 6h, and then naturally cooled to obtain the honeycomb ceramic carrier.
[0172] Comparative Example 1
[0173] In this embodiment, 36wt.% of flaky talc, 20.2wt.% of flaky raw kaolin, 26.6wt.% of calcined kaolin, 3wt.% of silicon oxide, 12.2wt.% of aluminum oxide, 9wt.% of the total amount of inorganic raw materials, and 5wt.% of the lubricant are added to a plow mixer and dry mixed for 10 minutes at a rotation speed of 500rpm; after the dry mixing, 33wt.% of water relative to the inorganic raw materials is added for wet mixing for 15 minutes at a rotation speed of 500rpm; then a honeycomb structure is extruded using a 600-mesh, 3.7-inch diameter die; the cut length is 3.1 inches; then it is dried at 50°C for 0.4h; the obtained green body is first heated at 250-310°C for 7h to debind, then sintered at 1430°C for 6h, and then naturally cooled to obtain the honeycomb ceramic carrier.
[0174] Comparative Example 2
[0175] In this embodiment, 32wt.% of flaky talc, 21.2wt.% of flaky raw kaolin, 28.6wt.% of calcined kaolin, 3wt.% of silicon oxide, 13.2wt.% of aluminum oxide, and 7wt.% of a binder and 6wt.% of a lubricant accounting for the total amount of inorganic raw materials are added to a plowshare mixer and dry mixed for 10 minutes at a rotation speed of 500rpm; after the dry mixing, 33wt.% of water relative to the inorganic raw materials is added for wet mixing for 15 minutes at a rotation speed of 500rpm; a honeycomb structure is then extruded using a 750 mesh, 4.66-inch diameter die; the cut length is 3.1 inches; and then dried at 50°C for 0.4h; the obtained green body is first heated at 250-310°C for 7h to debind, then sintered at 1430°C for 6h, and then naturally cooled to obtain the honeycomb ceramic carrier.
[0176] Comparative Example 3
[0177] In this embodiment, 25wt.% of flaky talc, 20.2wt.% of flaky raw kaolin, 32.6wt.% of calcined kaolin, 5wt.% of silicon oxide, 17.2wt.% of aluminum oxide, 3wt.% of a binder and 10wt.% of a lubricant accounting for the total amount of inorganic raw materials are added to a plowshare mixer and dry mixed for 10 minutes at a rotation speed of 500rpm; after the dry mixing, 28wt.% of water relative to the inorganic raw materials is added for wet mixing for 15 minutes at a rotation speed of 500rpm; then a honeycomb structure is extruded using a 800-mesh, 4.66-inch diameter die; the cut length is 5 inches; then it is dried at 50°C for 0.4h; the obtained green body is first heated at 250-310°C for 7h to debind, then sintered at 1430°C for 6h, and then naturally cooled to obtain the honeycomb ceramic carrier.
[0178] Comparative Example 4
[0179] In this embodiment, 39wt.% of flaky talc, 10.2wt.% of flaky raw kaolin, 30.6wt.% of calcined kaolin, 4wt.% of silicon oxide, 16.2wt.% of aluminum oxide, and 15wt.% of a binder and 2wt.% of a lubricant accounting for the total amount of inorganic raw materials are added to a plowshare mixer and dry mixed for 10 minutes at a rotation speed of 500rpm; after the dry mixing, 50wt.% of water relative to the inorganic raw materials is added for wet mixing for 15 minutes at a rotation speed of 500rpm; a honeycomb structure is then extruded using a 600-mesh, 3.7-inch diameter die; the cut length is 3.1 inches; and then dried at 50°C for 0.4h; the obtained green body is first heated at 250-310°C for 7h to debind, then sintered at 1430°C for 6h, and then naturally cooled to obtain the honeycomb ceramic carrier.
[0180] Comparative Example 5
[0181] In this embodiment, 30wt.% of flaky talc, 29.8wt.% of flaky raw kaolin, 15wt.% of calcined kaolin, 10wt.% of silicon oxide, 16.2wt.% of aluminum oxide, 12wt.% of a binder and 2wt.% of a lubricant accounting for the total amount of inorganic raw materials are added to a plowshare mixer and dry mixed for 10 minutes at a rotation speed of 500rpm; after the dry mixing, 45wt.% of water relative to the inorganic raw materials is added for wet mixing for 15 minutes at a rotation speed of 500rpm; a honeycomb structure is then extruded using a 750 mesh, 4.66-inch diameter die; the cut length is 3.1 inches; and then dried at 50°C for 0.4h; the obtained green body is first heated at 250-310°C for 7h to debind, then sintered at 1430°C for 6h, and then naturally cooled to obtain the honeycomb ceramic carrier.
[0182] Comparative Example 6
[0183] In this embodiment, 25wt.% of flaky talc, 28.2wt.% of flaky raw kaolin, 26.6wt.% of calcined kaolin, 4wt.% of silicon oxide, 16.2wt.% of aluminum oxide, 10wt.% of a binder and 3.5wt.% of a lubricant accounting for the total amount of inorganic raw materials are added to a plowshare mixer and dry mixed for 10 minutes at a rotation speed of 500rpm; after the dry mixing, 46wt.% of water relative to the inorganic raw materials is added for wet mixing for 15 minutes at a rotation speed of 500rpm; then a honeycomb structure is extruded using a 800 mesh, 4.66-inch diameter die; the cut length is 5 inches; then it is dried at 50°C for 0.4h; the obtained green body is first heated at 250-310°C for 7h to debind, then sintered at 1430°C for 6h, and then naturally cooled to obtain the honeycomb ceramic carrier.
[0184] Comparative Example 7
[0185] In this embodiment, 31wt.% of flaky talc, 29.2wt.% of flaky raw kaolin, 10.6wt.% of calcined kaolin, 10wt.% of silicon oxide, 19.2wt.% of aluminum oxide, and 7wt.% of a binder and 6wt.% of a lubricant accounting for the total amount of inorganic raw materials are added to a plowshare mixer and dry mixed for 10 minutes at a rotation speed of 500rpm; after the dry mixing, 36wt.% of water relative to the inorganic raw materials is added for wet mixing for 15 minutes at a rotation speed of 500rpm; a honeycomb structure is then extruded using a 750 mesh, 4.66-inch diameter die; the cut length is 5 inches; and then dried at 50°C for 0.4h; the obtained green body is first heated at 250-310°C for 7h to debind, then sintered at 1430°C for 6h, and then naturally cooled to obtain the honeycomb ceramic carrier.
[0186] Comparative Example 8
[0187] In this embodiment, 25wt.% of flaky talc, 24.8wt.% of flaky raw kaolin, 30wt.% of calcined kaolin, 4wt.% of silicon oxide, 16.2wt.% of aluminum oxide, and 5wt.% of a binder and 8wt.% of a lubricant accounting for the total amount of inorganic raw materials are added to a plowshare mixer and dry mixed for 10 minutes at a rotation speed of 500rpm; after the dry mixing, 29wt.% of water relative to the inorganic raw materials is added for wet mixing for 15 minutes at a rotation speed of 500rpm; a honeycomb structure is then extruded using a 750 mesh, 4.66-inch diameter die; the cut length is 5 inches; and then dried at 50°C for 0.4h; the obtained green body is first heated at 250-310°C for 7h to debind, then sintered at 1430°C for 6h, and then naturally cooled to obtain the honeycomb ceramic carrier.
[0188] Comparative Example 9
[0189] In this embodiment, 29wt.% of flaky talc, 25.8wt.% of flaky raw kaolin, 25wt.% of calcined kaolin, 4wt.% of silicon oxide, 16.2wt.% of aluminum oxide, 3.5wt.% of a binder and 10wt.% of a lubricant accounting for the total amount of inorganic raw materials are added to a plowshare mixer and dry mixed for 10 minutes at a rotation speed of 500rpm; after the dry mixing, 28wt.% of water relative to the inorganic raw materials is added for wet mixing for 15 minutes at a rotation speed of 500rpm; a honeycomb structure is then extruded using a 750 mesh, 4.66-inch diameter die; the cut length is 5 inches; and then dried at 50°C for 0.4h; the obtained green body is first heated at 250-310°C for 7h to debind, then sintered at 1430°C for 6h, and then naturally cooled to obtain the honeycomb ceramic carrier.
[0190] The parameters of the above-mentioned embodiments and comparative examples are compared and listed in Table 1 below.
[0191] Table 1 Parameter comparison of various embodiments and comparative examples
[0192]
[0193]
[0194]
[0195] In Example 2, compared with Example 1, the cell density and diameter were changed to produce a honeycomb ceramic structure.
[0196] In Example 3, compared with Example 1, the cell density, wall thickness, length and diameter are changed to produce a honeycomb ceramic structure.
[0197] Compared with Example 1, Example 4 changes the pore density, wall thickness, length, diameter, and special structure ratio to produce a honeycomb ceramic structure.
[0198] Compared with Example 1, Example 5 changes the pore density, wall thickness, length, diameter, and special structure ratio to produce a honeycomb ceramic structure.
[0199] Compared with Example 1, Example 6 changes the compartment structure and the proportion of special structures to produce the honeycomb ceramic structure.
[0200] Compared with Example 1, Example 7 changes the pore density and the proportion of special structures to produce a honeycomb ceramic structure.
[0201] Compared with Example 1, Example 8 changes the pore density, wall thickness, and special structure ratio to produce a honeycomb ceramic structure.
[0202] Compared with Example 1, Example 9 changes the pore density, diameter, and special structure ratio to produce a honeycomb ceramic structure.
[0203] Compared with Example 1, Example 10 changes the cell density, diameter, length, and special structure ratio to produce a honeycomb ceramic structure.
[0204] Compared with Example 1, Example 11 changes the diameter, length, and special structure ratio to produce a honeycomb ceramic structure.
[0205] Compared with Example 1, Example 12 changes the wall thickness, diameter, length, and special structure ratio to produce a honeycomb ceramic structure.
[0206] Compared with Example 1, Example 13 changes the pore density, diameter, length, and special structure ratio to produce a honeycomb ceramic structure.
[0207] Compared with Example 1, Example 14 changes the pore density, wall thickness, diameter, length, and special structure ratio to produce a honeycomb ceramic structure.
[0208] Compared with Example 1, Example 15 changes the pore density, wall thickness, diameter, length, and special structure ratio to produce a honeycomb ceramic structure.
[0209] In Comparative Example 1, compared with Example 1, the cell structure was changed to produce a honeycomb ceramic structure.
[0210] In Comparative Example 2, compared with Example 1, the cell structure, pore density and diameter were changed to produce a honeycomb ceramic structure.
[0211] In Comparative Example 3, compared with Example 1, the cell structure, pore density, wall thickness, diameter and length were changed to produce a honeycomb ceramic structure.
[0212] In Comparative Example 4, compared with Example 1, the cell structure, diameter, and length were changed to produce a honeycomb ceramic structure.
[0213] In Comparative Example 5, compared with Example 1, the cell structure, cell density and length were changed to produce a honeycomb ceramic structure.
[0214] In Comparative Example 6, compared with Example 1, the cell structure, pore density, wall thickness and length were changed to produce a honeycomb ceramic structure.
[0215] In Comparative Example 7, compared with Example 1, the cell density, length, and diameter were changed to produce a honeycomb ceramic structure.
[0216] In Comparative Example 8, compared with Example 1, the cell density, length, diameter, and special structure ratio were changed to produce a honeycomb ceramic structure.
[0217] Compared with Example 1, Comparative Example 9 changes the pore density, length, diameter, compartment structure, and special structure ratio to produce a honeycomb ceramic structure.
[0218] The performance test results of the honeycomb ceramic carriers obtained in the above-mentioned embodiments and comparative examples are listed in Table 2 below.
[0219] Table 2 Performance test results of honeycomb ceramic carriers obtained in various embodiments and comparative examples
[0220]
[0221]
[0222] Table 2 is a performance comparison of the cordierite honeycomb ceramic carriers prepared in various embodiments and comparative examples, mainly involving specific specifications, carrier yield, thermal expansion coefficient, thermal shock, isostatic pressing, catalyst coating thickness, change in mold groove width, A-axis compressive strength and other test results. Thermal expansion coefficient: using a thermal expansion meter to test the deformation of the product from room temperature to 800°C; A-axis compression: using a servo computerized universal material testing machine for testing, using a 25±0.5mm sample; thermal shock: using a muffle furnace, heating the muffle furnace to 650°C and keeping it warm for 30 minutes, taking it out and placing it at room temperature for rapid cooling without cracking. Catalyst coating thickness: obtained by imager testing.
[0223] Die slot width variation: obtained through imager testing. Every 5,000 meters of cordierite honeycomb ceramic carrier produced is tested to measure the change in die slot width before and after production.
[0224] It can be seen from Examples 1 to 15 in Table 2 that the compressive strength of the honeycomb ceramic carrier with special structure compartments is similar to the compressive strength of the honeycomb ceramic carrier with rounded corners in Comparative Examples 4 to 6. The compressive strength of the honeycomb ceramic carrier with special structure compartments is higher than that of Comparative Examples 1 to 3, and its yield rate is much higher than that of Comparative Examples 1-3, basically more than 20% higher. The coating thickness of the precious metal of the honeycomb ceramic carrier with special structure compartments is much lower than that of Comparative Examples 1-3, basically 50% lower. Compared with Comparative Examples 4 to 6, Examples 1 to 15 have very low wear on the mold. The change in the width of the mold groove for every 5,000 meters of extrusion of the special compartment mechanism is about 10% of that of the full rounded corner structure, which greatly improves the service life of the mold and reduces the cost of the product. Compared with Comparative Examples 4 to 6, the yield rate of Examples 1 to 15 is 10% higher. The special corner ratio exceeding 30% will greatly reduce the yield rate.
[0225] In addition, the "thermal shock resistance" in this application specification is also called thermal shock resistance or thermal stability, which refers to the ability of a material to withstand drastic temperature changes or hot and cold alternations within a certain starting temperature range without being damaged. This is the temperature that can withstand hot and cold alternations without damage, which is the thermal shock parameter, and is generally measured after three cycles of experiments. The sample is thermally cycled three times at the above temperature without cracking. The isostatic pressure test method is: the sample is wrapped with a rubber sleeve, placed in an isostatic pressure tester filled with water, and pressure is applied. The pressure is maintained for 5 minutes without cracking. The above carrier can complete the test at 2-7MPa.
[0226] The honeycomb ceramic has the following structural characteristics, and the coefficient of thermal expansion (CTE) measured at 25°C to 800°C is 0.2x10 -6 ~0.5×10 -6 ℃ -1 The thermal shock parameter (TSP) of the honeycomb ceramic structure is 650-750°C, that is, it will not crack after three thermal cycles at the above temperature. The isostatic pressure test method is: the sample is wrapped with a rubber sleeve and placed in an isostatic pressure tester filled with water. Pressure is applied and maintained for 5 minutes without cracking sound. The above-mentioned carrier can complete the test at 2-7MPa.
[0227] The above is only a specific implementation of the present invention, but the protection scope of the present invention is not limited thereto. Any technician familiar with the technical field can easily think of changes or substitutions within the technical scope disclosed by the present invention, which should be covered within the protection scope of the present invention. Therefore, the protection scope of the present invention shall be based on the protection scope of the claims. In addition, the specification uses specific examples to illustrate the principles and implementation methods of the present invention. The description of the above embodiments is only used to help understand the method of the present invention and its core idea. The content of this specification should not be understood as a limitation on the present invention.
Claims
1. A honeycomb ceramic carrier, characterized in that: The honeycomb ceramic carrier comprises: Ontology(1); A plurality of compartments (2) with a hollow structure in the body, wherein the compartments (2) penetrate the body (1) to form a honeycomb structure; The compartment (2) has a quadrilateral cross section, a pair of opposite corners of the quadrilateral cross section have an inner recess or a chamfer, and the other pair of opposite corners of the quadrilateral cross section do not have an inner recess or a chamfer.
2. The honeycomb ceramic carrier according to claim 1, characterized in that: In one of the compartments (2), in a pair of opposite corners having the inner recess or chamfer, two apex corners have the same shape and size; Alternatively, in one of the compartments (2), in a pair of opposite corners having the inner recess or chamfer, the two apex corners have different shapes and / or different sizes.
3. The honeycomb ceramic carrier according to claim 1, characterized in that: The four compartments (2) constitute a repeating unit, and the repeating unit has a symmetry center; Wherein, the top corners of the four compartments (2) in the repeating unit, which are located inside the repeating unit, have the recessed portion or chamfered portion, or the top corners of the four compartments (2) in the repeating unit, which are located inside the repeating unit, do not have the recessed portion or chamfered portion.
4. The honeycomb ceramic carrier according to claim 3, characterized in that: The number of the compartments (2) is at least twelve; Wherein, each of the compartments (2) constitutes a quarter of at least two repeating units.
5. The honeycomb ceramic carrier according to claim 3, characterized in that: In a repeating unit, the apex corners of the four compartments (2) located inside the repeating unit and having the inner concave portion or chamfer are enclosed and form a reinforced intersection (31) at the position of the symmetry center; Alternatively, in a repeating unit, the vertices of the four compartments (2) located inside the repeating unit and presenting outwardly convex right angles are enclosed and form a common intersection (32) at the position of the symmetry center.
6. The honeycomb ceramic carrier according to claim 1, characterized in that: The inner concave portion is an inner concave right angle, a rounded angle or an inner concave flower angle; The concave right angle is configured to be concave relative to the interior of the compartment (2) in which it is located, and the rounded corner is configured to be convex or concave relative to the interior of the compartment (2) in which it is located.
7. The honeycomb ceramic carrier according to any one of claims 1 to 6, characterized in that: The honeycomb ceramic substrate has one or more of the following features: The water absorption rate of the honeycomb ceramic carrier is 14-28%; The compressive strength of the honeycomb ceramic carrier in the longitudinal direction is 9 to 10.5 MPa; The thermal expansion coefficient CTE of the honeycomb ceramic carrier in the longitudinal direction within the temperature range of 25 to 800° C. is 0.2×10 -6 ~0.5×10 -6 ℃ -1 ; The isostatic strength of the honeycomb ceramic carrier is 3.1-6.3 MPa; The thermal shock parameter TSP of the ceramic carrier is 650°C to 750°C, preferably 700°C to 750°C; The size of the ceramic carrier in the longitudinal direction is 3 to 5.5 inches; The radial dimension of the ceramic carrier is 3.7 to 5.6 inches; In the ceramic carrier, the density of the compartment (2) is 600 to 1200 cpsi; And / or, the thickness of the partition wall between two adjacent compartments (2) in the ceramic carrier is 2 to 4 mils.
8. The honeycomb ceramic carrier according to any one of claims 1 to 7, characterized in that: In each of the compartments (2), the two apex angles of a pair of opposite corners without the inner recess or chamfer are both right angles, and each right angle is formed by two first straight line segments, one of the first straight line segments has a length of A1, and the other of the first straight line segments has a length of B1; Each vertex of a pair of diagonal corners having the inner concave portion is formed by two second straight line segments, wherein the length of one of the second straight line segments is A2, and the length of the other second straight line segment is B2; Among them, (A2 / A1)*100%=5-25%, preferably 15-25%, (B2 / B1)*100%=5-25%, preferably 15-25%.
9. The honeycomb ceramic carrier according to any one of claims 1 to 7, characterized in that: In each of the compartments (2), the two apex angles of a pair of opposite corners without the inner recess or chamfer are both right angles, and each right angle is formed by two first straight line segments, one of the first straight line segments has a length of A1, and the other of the first straight line segments has a length of B1; Each vertex of a pair of opposite corners with the chamfer is formed by a third straight line segment, the projection length of the third straight line segment in the direction where one of the first straight line segments is located is A3, and the projection length of the third straight line segment in the direction where another of the first straight line segments is located is B3; Among them, (A3 / A1)*100%=5-25%, preferably 15-25%, (B3 / B1)*100%=5-25%, preferably 15-25%.
10. The honeycomb ceramic carrier according to any one of claims 1 to 7, characterized in that: In each of the compartments (2), the two apex angles of a pair of opposite corners without the inner recess or chamfer are both right angles, and each right angle is formed by two first straight line segments, one of the first straight line segments has a length of A1, and the other of the first straight line segments has a length of B1; Each vertex of a pair of diagonal corners having the inner concave portion is formed by an arc segment, the projection length of the arc segment in the direction where one of the first straight line segments is located is A4, and the projection length of the arc segment in the direction where another of the first straight line segments is located is B4; Among them, (A4 / A1)*100%=5-25%, preferably 15-25%, (B4 / B1)*100%=5-25%, preferably 15-25%.
11. The honeycomb ceramic carrier according to any one of claims 1 to 7, characterized in that: In each of the compartments (2), the two apex angles of a pair of opposite corners without the inner recess or chamfer are both right angles, and each right angle is formed by two first straight line segments, one of the first straight line segments has a length of A1, and the other of the first straight line segments has a length of B1; Each vertex of a pair of diagonal angles having the inner concave portion is composed of four sequentially connected fourth straight line segments, the sum of the projection lengths of the four fourth straight line segments in the direction where one of the first straight line segments is located is A5, and the sum of the projection lengths of the four fourth straight line segments in the direction where another of the first straight line segments is located is B5; Among them, (A5 / A1)*100%=5-25%, preferably 15-25%, (B5 / B1)*100%=5-25%, preferably 15-25%.
12. The honeycomb ceramic carrier according to claims 1 to 7, characterized in that: The raw materials of the ceramic carrier include inorganic raw materials, organic additives, binders and water; The inorganic raw materials are talc, kaolin, alumina and optionally silicon oxide and aluminum hydroxide, wherein the talc is preferably flaky talc, more preferably flaky talc with D50=5-20 μm; the kaolin is preferably raw kaolin and / or cooked kaolin, the raw kaolin is more preferably flaky raw kaolin, the flaky raw kaolin is more preferably flaky raw kaolin with D50=5-20 μm, the cooked kaolin is more preferably cooked kaolin with D50=4-15 μm, the silicon oxide is preferably silicon oxide with D50=1-10 μm, and the aluminum oxide is preferably aluminum oxide with D50=1-10 μm; The organic auxiliary agent is at least one of alkyl polyether, fatty alcohol polyoxyethylene ether, xanthan gum, potassium laurate, and glycerol random polyether; The binder is at least one of hydroxymethyl cellulose, ethyl cellulose and carboxymethyl cellulose.
13. The honeycomb ceramic carrier according to claim 12, characterized in that: Based on the total amount of inorganic raw materials as 100wt.%, the talc accounts for 20-40wt.%, the kaolin accounts for 20-60wt.%, the alumina accounts for 10-20wt.%, the silicon oxide accounts for 0-10wt.%, the organic additive accounts for 2-10wt.% relative to the total amount of inorganic raw materials, the binder accounts for 3-15wt.% relative to the total amount of inorganic raw materials, and the water accounts for 25-50wt.% relative to the total amount of inorganic raw materials. Preferably, the kaolin comprises 10-30 wt.% of flaky raw kaolin and 10-30 wt.% of cooked kaolin, based on the total amount of inorganic raw materials being 100 wt.%.
14. The method for preparing a honeycomb ceramic carrier according to any one of claims 1 to 13, characterized in that: The preparation method The following steps are involved: S1, mixing inorganic raw materials to obtain dry materials; S2, the dry material obtained in step S1 is mixed with an organic additive, a binder, and water in sequence through wet mixing, kneading, mud kneading, extrusion molding, drying, and cutting to obtain a green body; S3, sintering the green body obtained in step S2 to obtain the honeycomb ceramic carrier; The compartment (2) of the honeycomb ceramic carrier is formed during the extrusion molding process in step S2, wherein the compartment (2) has a quadrilateral cross section, a pair of diagonals of the quadrilateral cross section have an inner recess or chamfer, and the other pair of diagonals of the quadrilateral cross section do not have an inner recess or chamfer.
15. The preparation method according to claim 14, characterized in that: In the step S3, during the sintering process, the heating rate and the sintering temperature at least at a certain moment change with the sintering time.
16. The preparation method according to claim 14, characterized in that: In the step S3, the sintering temperature is 1000° C. to 1450° C., the sintering time is at least 13 hours, and the heating rate is greater than 25° C. / h.
17. The preparation method according to claim 14, characterized in that: In the step S2, the wet mixing includes: putting the dry material, the binder, and the organic additive into a plowshare mixer for dry mixing, and then spraying water for wet mixing; The mud preparation includes: putting the wet mixed raw materials into a mesh mud preparation machine to prepare the mud under vacuum conditions; The extrusion molding comprises: feeding the raw material after mud kneading into an extruder, preferably at least one selected from a single-screw extruder, a twin-screw extruder or a hydraulic extruder, to mold it, and then obtaining the compartment (2) through a mold; The drying comprises: using a microwave dryer to dry and shape; The cutting includes: cutting with a blank cutting machine.
18. A catalyst, characterized in that: The catalytic body comprises a honeycomb ceramic carrier as claimed in any one of claims 1 to 13, wherein a catalyst is coated on the inner wall surface of the compartment (2) of the honeycomb ceramic carrier; Preferably, the catalyst coating thickness at the top corner position having the inner concave portion or chamfered structure is 0.06-0.08 μm, and the coating thickness at other positions is 0.07 μm.
Citation Information
Patent Citations
Low-stress honeycomb ceramic heat accumulator forming mold and method for preparing same
CN101306555A
Ceramic honeycomb structural body and catalyst comprising the same
CN1098029A
Honeycomb structure
JP2010227846A
Honeycomb structure and exhaust gas cleaning apparatus
JP2012250901A
Pattern-plugged honeycomb bodies, particulate filters, and extrusion dies therefor
US20190374896A1
Cited By
Cylindrical honeycomb carrier and catalytic body
CN119549201A
Honeycomb ceramic carrier, preparation method therefor, and catalytic body containing honeycomb ceramic carrier
WO2025156928A1
Cylindrical honeycomb carrier and catalytic body
WO2026113100A1