NiCo modified oxide ceramic particle reinforced iron-based composite material and casting method and application thereof
By depositing NiCo plating on the surface of ZTA ceramic particles and mixing them with iron powder and silicate water glass, the problem of poor dispersion of oxide ceramic particles in metal matrix is solved, the wear resistance and toughness of composite materials are improved, and the use is extended life.
Patent Information
- Application Number
- CN202411051284.7
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-08-01
- Publication Date
- 2024-11-19
AI Technical Summary
Traditional single steel materials have poor wear resistance under severe working conditions, which can easily lead to breakage, and the oxide ceramic particles are poorly dispersed in metal substrates, limiting the service life of the composite material.
The casting method of NiCo modified oxide ceramic particles reinforced iron-based composite materials is adopted. By surface activation and sensitization of irregular ZTA ceramic particles, NiCo plating is deposited by chemical co-deposition, combining iron powder and silicate water glass, The porous preform is formed, and the composite material is finally prepared by bottom-filling casting.
It improves the interface bonding performance between ceramic particles and metal matrix, enhances the wear resistance and toughness of composite materials, and extends the service life of composite materials.
Smart Images

Figure CN118976882A_ABST
Abstract
Description
Technical Field
[0001] The invention belongs to the technical field of wear-resistant material preparation, and specifically relates to a NiCo modified oxide ceramic particle reinforced iron-based composite material and a casting method and application thereof. Background Art
[0002] With the increasing depletion of traditional energy, energy conservation has become one of the important means to deal with the global energy crisis. However, impact abrasive wear in industrial fields such as mining, building materials, metallurgy, marine engineering, power and railways is the main cause of heavy machinery equipment failures, and a large amount of energy is consumed in the maintenance and production of equipment wear-resistant parts.
[0003] Traditional single steel materials often have problems such as poor wear resistance and mismatch between strength and toughness, which can easily lead to catastrophic breakage accidents under harsh service conditions. Therefore, the primary issue facing the field of wear-resistant materials is to develop new wear-resistant materials with excellent comprehensive properties such as strength, toughness and wear resistance, and significantly reduce the material consumption of moving parts. Ceramic particle reinforced metal matrix composites have both the high hardness and high wear resistance of the ceramic particle reinforcement phase and the toughness of the metal matrix, and are expected to become an ideal material to replace traditional single metal wear-resistant parts. Commonly used ceramic particles are carbide ceramics and oxide ceramics, among which Al 2 O 3 Ceramics are widely used in practical applications due to their low cost, high hardness and good thermal matching with steel substrates.
[0004] But Al 2 O 3 The poor wettability between ceramic and steel matrix results in insufficient interface bonding performance, which seriously limits the service life of composite materials. Metallization of ceramic particle surface can effectively improve the surface activity of ceramic particles, thereby improving the bonding performance of heterogeneous interfaces of composite materials, further enhancing the mechanical properties and wear resistance of composite materials, and obtaining the key preparation technology of advanced composite wear-resistant linings. Summary of the invention
[0005] The technical problem to be solved by the present invention is to provide a NiCo modified oxide ceramic particle reinforced iron-based composite material and a casting method and application thereof in view of the deficiencies in the above-mentioned prior art, so as to solve the technical problem of poor dispersion of oxide ceramic particles in a metal matrix. The prepared wear-resistant composite material has both high wear resistance and good service safety under harsh working conditions. The present invention adopts the following technical solutions:
[0006] A method for casting a NiCo modified oxide ceramic particle reinforced iron-based composite material comprises the following steps:
[0007] The irregular ZTA ceramic particles are surface activated and sensitized, and then a NiCo coating is deposited on the surface of the ZTA ceramic particles by chemical co-deposition.
[0008] The metallized ZTA ceramic particles are mixed evenly with iron powder and silicate water glass solution so that the iron powder is coated on the surface of the metallized ZTA ceramic particles, and then the mixture is injected into a mold to form a porous preform;
[0009] The porous preform is dried, and finally the porous preform is prepared into a composite material by bottom casting.
[0010] Preferably, acetone is used to clean the oil stains and impurities on the surface of the ZTA ceramic particles, and then ultrasonic cleaning is performed, the water bath is heated to 60-80° C., ultrasonic cleaning is performed for 10-15 minutes, and then the dried ZTA ceramic particles are activated and sensitized.
[0011] Preferably, the activation and sensitization treatments are specifically:
[0012] In SnCl 2 The irregular ZTA ceramic particles were activated in the solution for 10-30 min and then heated in PdCl 2 The sensitization treatment was carried out in the solution for 10 to 30 minutes, and finally NaH 2 PO 2 Remove excess Pd ions.
[0013] Preferably, in the process of depositing a NiCo coating on the surface of ZTA ceramic particles by chemical co-deposition, the mass ratio of Ni:Co in the chemical co-deposition plating solution is (1-4):(4-1), trisodium citrate is used as a complexing agent, and boric acid is used to adjust the pH.
[0014] Preferably, NaH 2 PO 2 The concentration of is 10-30 g / L, the concentration of the complexing agent is 20-50 g / L, the deposition temperature is 60-90°C, the deposition time is 2-12 h, and the plating solution is changed every 1.5-2 h.
[0015] Preferably, the metallized ZTA ceramic particles are uniformly mixed with iron powder and silicate water glass solution as follows:
[0016] The plated ZTA ceramic particles are stirred and mixed with 10wt.% to 20wt.% of iron powder and 2wt.% to 5wt.% of silicate, and the mixture is dispersed in an eight-hole mold, and then dried in a vacuum drying oven to obtain a porous preform, and then the porous preform is sintered at a high temperature of 1200 to 1400°C.
[0017] Preferably, the stirring speed is 150-200 rpm, the time is 1-2 h, the drying temperature is 70-90 ° C, the drying time is 30-60 min, and the vacuum degree is maintained at 0.5-1.5×10 -1 Pa, sintering time is 1 to 2 hours, and vacuum degree is maintained at 0.5 to 2×10 -3 Pa, the heating rate of the first 800°C during high-temperature sintering is 10°C / min, and the heating rate of the high-temperature stage is 5°C / min.
[0018] Preferably, the porous preform is dried at 350-500° C. for 5-10 hours, and finally the porous preform is prepared into a composite material by bottom casting at 1450-1600° C.
[0019] Another technical solution of the present invention is to use NiCo modified oxide ceramic particles to reinforce iron-based composite materials.
[0020] Another technical solution of the present invention is to apply the NiCo modified oxide ceramic particle reinforced iron-based composite material to the wear-resistant liner.
[0021] Compared with the prior art, the present invention has at least the following beneficial effects:
[0022] A casting method for NiCo modified oxide ceramic particles reinforced iron-based composite materials, in which NiCo coating is applied to the surface of ZTA ceramic particles by chemical co-deposition, solving the problems of poor interface and uneven composition in the step-by-step deposition process. Transition metals Ni and Co improve the surface activity of ZTA ceramic particles, thereby improving the wettability between ZTA ceramic particles and metal matrix, and enhancing the bonding performance of heterogeneous interfaces of composite materials. The patent of the present invention uses perlite multiple slag removal technology to purify iron, reducing defects such as impurities and pores in castings, while improving the fluidity of molten iron. During the solidification process, the bonding phase Fe between particles in the preform forms a multi-component alloy through diffusion with NiCo on the surface of ZTA ceramics, further improving the interface bonding strength between ZTA ceramic particles and Fe matrix. Due to the high hardness of ZTA ceramic particles, they can effectively resist the wear of abrasives and thus protect the matrix. At the same time, the metal matrix with excellent toughness supports the ZTA ceramic particles. Therefore, the prepared composite liner has both high strength, high toughness and high wear resistance.
[0023] Furthermore, acetone was used to dissolve and remove oil stains and impurities on the surface of ZTA, thereby improving the adsorption capacity of the ceramic surface.
[0024] Furthermore, activation and sensitization treatments were used to etch a large number of tiny pits on the surface of ZTA ceramics, increasing its specific surface area.
[0025] Furthermore, the precious metal Pd is attached to the etching pits on the surface of the ZTA ceramic particles, which provides activation sites for the deposition of NiCo and improves the deposition efficiency.
[0026] Furthermore, defects such as inclusions and pores seriously affect the mechanical properties and wear resistance of castings. Therefore, an efficient purification process can improve the fluidity of molten iron and extend the service life of composite materials.
[0027] Furthermore, the transition metal NiCo has good wettability with the ZTA ceramic particles, and can form multi-component metal multi-layers at the heterogeneous interface during the casting and infiltration process to achieve metallurgical bonding.
[0028] Furthermore, the high porosity in the porous preform can provide capillary force for the casting infiltration of molten iron and increase the casting infiltration depth, while its good strength can ensure that the ZTA ceramic particles are not dispersed under the impact of high-temperature molten iron, thereby achieving the positioning and compounding of ceramic particles in the metal matrix.
[0029] In summary, the present invention adopts activation + sensitization treatment to improve the catalytic activity of the surface of ZTA ceramic particles, and coats the surface of ZTA ceramic particles with NiCo coating by chemical co-deposition, thereby improving the interface bonding performance between the ceramic particles and the iron matrix, and the bonding method is metallurgical bonding, thereby enhancing the wear resistance of the composite material liner.
[0030] The technical solution of the present invention is further described in detail below through the accompanying drawings and embodiments. BRIEF DESCRIPTION OF THE DRAWINGS
[0031] Figure 1 This is a photo of the NiCo coating coated with ZTA particles after chemical co-deposition in Example 1 of the present invention;
[0032] Figure 2 This is a photograph of the composite material prepared in Example 1 of the present invention. DETAILED DESCRIPTION
[0033] The technical solution of the present invention will be described clearly and completely below. Obviously, the described embodiments are only part of the embodiments of the present invention, not all of them. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.
[0034] In the present invention, unless otherwise specified, all the embodiments and preferred implementation methods mentioned herein can be combined with each other to form a new technical solution.
[0035] In the present invention, unless otherwise specified, all technical features and preferred features mentioned herein can be combined with each other to form a new technical solution.
[0036] In the present invention, unless otherwise specified, percentage (%) or part refers to the weight percentage or weight part relative to the composition.
[0037] In the present invention, unless otherwise specified, the components or preferred components involved can be combined with each other to form a new technical solution.
[0038] In the present invention, unless otherwise specified, the numerical range "a-b" represents an abbreviation of any real number combination between a and b, where a and b are real numbers. For example, the numerical range "6-22" means that all real numbers between "6-22" have been listed in this document, and "6-22" is just an abbreviation of these numerical combinations.
[0039] The “range” disclosed in the present invention is in the form of a lower limit and an upper limit, which can be one or more lower limits, and one or more upper limits, respectively.
[0040] In the present invention, the term "and / or" used herein refers to any combination and all possible combinations of one or more of the associated listed items, and includes these combinations.
[0041] In the present invention, unless otherwise specified, each reaction or operation step can be carried out sequentially or in accordance with the sequence. Preferably, the reaction method herein is carried out sequentially.
[0042] Unless otherwise specified, the professional and scientific terms used herein have the same meanings as those familiar to those skilled in the art. In addition, any method or material similar or equivalent to the described content may also be applied to the present invention.
[0043] The invention provides a NiCo modified oxide ceramic particle reinforced iron-based composite material and a casting method and application thereof. ZTA ceramic particles are activated and sensitized, a NiCo coating is deposited on the surface of the ZTA ceramic particles by a chemical deposition method, the modified ZTA particles, Fe powder and silicate are evenly mixed, the Fe powder is evenly wrapped on the surface of the ceramic particles, the mixture is then injected into an eight-hole polytetrafluoroethylene mold, and dried in a vacuum oven to obtain a ceramic porous preform, and a ceramic preform with good porosity and crushing strength is obtained by high-temperature sintering; the preform is fixed to the bottom of a sand mold, and a ZTA ceramic particle reinforced steel-based composite liner is prepared by a bottom-injection sand casting method; the NiCo coating co-deposited on the surface of the ZTA ceramic particles of the invention has uniform composition and structure, is sintered with Fe powder at high temperature, forms a metal sintering neck between the ceramic particles, and generates a multi-component alloy transition layer by diffusion between the ceramic particles and the high-chromium cast iron during infiltration, thereby improving the wear resistance of the composite material.
[0044] The present invention provides a method for casting a NiCo modified oxide ceramic particle reinforced iron-based composite material, comprising the following steps:
[0045] S1. Select crushed ZTA ceramic particles as the reinforcement phase, use acetone to ultrasonically clean the ZTA ceramic particles, heat them in a water bath to 60-80° C., ultrasonically clean them for 10-15 minutes, then rinse them with deionized water, and dry them in a vacuum oven;
[0046] S2, activating and sensitizing ZTA ceramic particles on a magnetic stirrer;
[0047] In the range of 5-15 g / L SnCl 2 The solution was sensitized for 10 to 30 minutes, followed by 0.1 to 0.5 g / L PdCl 2 The solution was activated and finally treated with 5-15 g / L NaH 2 PO 2 The solution removes excess Pd ions.
[0048] S3, depositing a NiCo coating on the surface of the ZTA ceramic particles by chemical co-deposition;
[0049] The Ni:Co ratio in the plating solution is (1-4): (4-1), NaH 2 PO 2 The concentration of the complexing agent C is 10-30 g / L. 6 H 5 O 7 Na 3 The concentration is 20-50 g / L, the deposition temperature is 60-90°C, the deposition time is 2-12 h, and the plating solution is changed every 1.5-2 h.
[0050] S4, the surface metallized ZTA ceramic particles obtained in step S3, 10-20wt.% Fe powder and 2-5wt.% silicate water glass are mixed in a stirrer to obtain a mixture, the mixture is injected into 8-hole polytetrafluoroethylene and then dried in a vacuum oven, and then sintered in a vacuum box furnace, and a preform is obtained after cooling in the furnace;
[0051] The stirring speed of the stirrer is 150-200 rpm, and the time is 1-2 hours.
[0052] The drying temperature of the vacuum oven is 70-90°C, the drying time is 30-60 min, and the vacuum degree is maintained at 0.5-1.5×10 -1 Pa.
[0053] The preform is sintered in a vacuum box furnace at 1200-1400°C for 1-2 hours, and the vacuum degree of the furnace is maintained at 0.5-2×10 -3 Pa.
[0054] During the heating process, the heating rate of the first 800°C was 10°C / min, and the heating rate of the high temperature stage was 5°C / min.
[0055] The size of the preform is 120×120×30 mm, and the size of the hole is Φ20×30 mm.
[0056] S5. Fix the preform obtained in step S4 at the bottom of the cavity, dry it in a heat treatment furnace, melt the molten iron in a medium frequency induction melting furnace, use perlite to slag and purify it multiple times, and deoxygenate the molten iron with pure aluminum; use a bottom pouring casting method to inject the molten iron into the quartz sand cavity, cool it to room temperature, and box it to obtain a ZTA ceramic particle reinforced iron-based composite wear-resistant liner.
[0057] The reaction temperature of the heat treatment furnace is 350-500°C, and the insulation time is 5-10h.
[0058] The DC voltage for smelting molten iron is 400-500V, the DC current is 80-100A, the medium frequency voltage is 650-750V, the medium frequency power is 50-70KW, and the medium frequency is 3000-3500Hz.
[0059] Casting infiltration under negative pressure helps to improve the fluidity and capillary force of molten iron. The casting infiltration temperature is 1450-1600℃.
[0060] A NiCo modified oxide ceramic particle reinforced iron-based composite material, the wear resistance of which is 3.2 to 5.4 times that of Cr15.
[0061] The NiCo modified oxide ceramic particle reinforced iron-based composite material prepared by the method of the invention can be applied to wear-resistant lining plates.
[0062] In order to make the purpose, technical solutions and advantages of the embodiments of the present invention clearer, the technical solutions in the embodiments of the present invention will be clearly and completely described below in conjunction with the drawings in the embodiments of the present invention. Obviously, the described embodiments are part of the embodiments of the present invention, rather than all of the embodiments. The components of the embodiments of the present invention described and shown in the drawings here can usually be arranged and designed in various different configurations. Therefore, the following detailed description of the embodiments of the present invention provided in the drawings is not intended to limit the scope of the claimed invention, but merely represents selected embodiments of the present invention. Based on the embodiments in the present invention, all other embodiments obtained by ordinary technicians in this field without making creative work are within the scope of protection of the present invention.
[0063] Example 1
[0064] The ZTA ceramic particles were ultrasonically cleaned in acetone, heated to 60 °C in a water bath, ultrasonically cleaned for 10 min, then rinsed with deionized water and dried in a vacuum oven;
[0065] Subsequently, the ZTA ceramic particles were activated and sensitized on a magnetic stirrer. The ZTA ceramic particles were hydrated in 5 g / L SnCl 2 The solution was sensitized for 10 min, followed by 0.1 g / L PdCl 2 The solution was activated and then treated with 5 g / L NaH 2 PO 2 The solution removes excess Pd ions;
[0066] The NiCo coating was deposited on the surface of ZTA ceramic particles by chemical co-deposition. The Ni:Co ratio in the plating solution was 1:4 and the NaH 2 PO 2 The concentration of 10g / L, complexing agent C 6 H 5 O 7 Na 3 The concentration is 20g / L, the deposition temperature is 60℃, the deposition time is 2h, and the plating solution is changed every 1.5h;
[0067] Surface metallized ZTA ceramic particles, 10wt.% Fe powder and 2wt.% silicate water glass were mixed evenly in a stirrer at a stirring speed of 150rpm for 1h. The mixture was injected into 8-hole polytetrafluoroethylene and then dried in a vacuum oven at 70℃ for 30min. The vacuum degree was maintained at 0.5×10 -1 Pa;
[0068] The preform was sintered in a vacuum box furnace at 1200 °C for 1 h, and the vacuum degree of the furnace was maintained at 0.5 × 10 -3 Pa; the heating rate of the first 800°C during the heating process is 10°C / min, and the heating rate of the high temperature stage is 5°C / min. The preform is cooled in the furnace to obtain a size of 120×120×30mm, and the size of the hole is Φ20×30mm;
[0069] The preform is fixed at the bottom of the cavity and dried in a heat treatment furnace at 350°C for 5 hours;
[0070] The molten iron is melted by a medium frequency induction melting furnace, with a DC voltage of 400V, a DC current of 80A, an medium frequency voltage of 650V, a medium frequency power of 50KW, and a medium frequency of 3000Hz. Perlite is used for multiple slag removal and purification, and pure aluminum is used to deoxygenate the molten iron;
[0071] The molten iron was poured into the quartz sand mold cavity by bottom casting method, the casting temperature was 1450℃, cooled to room temperature, and boxed to obtain ZTA ceramic particle reinforced iron-based composite wear-resistant lining, whose wear resistance was 3.2 times that of Cr15.
[0072] See also Figure 1 , it can be seen from the comparison of the surface morphology of ZTA ceramic particles in the figure that the ceramic particles are milky white before plating, and the surface becomes gray-brown after the NiCo coating is coated on its surface by chemical co-deposition, and the coating is evenly distributed on the irregular ZTA ceramic surface, thereby improving the surface activity of the ZTA ceramic particles. Therefore, the plating efficiency of this method is higher than that of step-by-step chemical deposition, and the bonding performance between the prepared coating and the ceramic is better than that of physical vapor deposition.
[0073] See also Figure 2 The ceramic particles are dispersed in the high chromium cast iron, and the interface between the ZTA ceramic and the metal matrix is well bonded, and no obvious holes and defects are found. Therefore, by depositing a NiCo coating on the surface of the ZTA ceramic particles, the interface bonding performance of the composite material can be effectively improved, and the wear resistance of the composite material can be further improved.
[0074] Example 2
[0075] The ZTA ceramic particles were ultrasonically cleaned in acetone, heated to 65 °C in a water bath, and ultrasonically cleaned for 12 min, then rinsed with deionized water and dried in a vacuum oven;
[0076] Subsequently, the ZTA ceramic particles were activated and sensitized on a magnetic stirrer. The ZTA ceramic particles were hydrated in 10 g / L SnCl 2 The solution was sensitized for 20 min, followed by 0.2 g / L PdCl 2 The solution was activated and then treated with 10 g / L NaH 2 PO 2 The solution removes excess Pd ions;
[0077] The NiCo coating was deposited on the surface of ZTA ceramic particles by chemical co-deposition. The Ni:Co ratio in the plating solution was 2:3 and the NaH 2 PO 2 The concentration of complexing agent C is 15g / L. 6 H 5 O 7 Na 3 The concentration is 30g / L, the deposition temperature is 70℃, the deposition time is 6h, and the plating solution is changed every 1.6h;
[0078] The surface metallized ZTA ceramic particles, 16wt.% Fe powder and 3wt.% silicate water glass were mixed in a stirrer at a stirring speed of 170rpm for 1.5h. The mixture was injected into 8-hole polytetrafluoroethylene and then dried in a vacuum oven at 80℃ for 40min. The vacuum degree was maintained at 1.0×10 -1 Pa;
[0079] The preform was sintered in a vacuum box furnace at 1300°C for 1.5 h, with the vacuum degree of the furnace maintained at 1.0×10 -3 Pa; the heating rate of the first 800°C during the heating process is 10°C / min, and the heating rate of the high temperature stage is 5°C / min. The preform is cooled in the furnace to obtain a size of 120×120×30mm, and the size of the hole is Φ20×30mm;
[0080] The preform is fixed at the bottom of the cavity and dried in a heat treatment furnace at 400°C for 6 hours;
[0081] The molten iron is melted by a medium frequency induction melting furnace, with a DC voltage of 450V, a DC current of 85A, an medium frequency voltage of 700V, a medium frequency power of 55KW, and a medium frequency of 3200Hz. Perlite is used for multiple slag removal and purification, and pure aluminum is used to deoxygenate the molten iron;
[0082] The molten iron was poured into the quartz sand mold cavity by bottom casting method, the casting temperature was 1500℃, cooled to room temperature, and boxed to obtain ZTA ceramic particle reinforced iron-based composite wear-resistant lining plate, whose wear resistance was 3.9 times that of Cr15.
[0083] Example 3
[0084] The ZTA ceramic particles were ultrasonically cleaned in acetone, heated to 75 °C in a water bath, and ultrasonically cleaned for 10 min, then rinsed with deionized water and dried in a vacuum oven;
[0085] Subsequently, the ZTA ceramic particles were activated and sensitized on a magnetic stirrer. The ZTA ceramic particles were hydrated in 10 g / L SnCl 2 The solution was sensitized for 25 min, followed by 0.4 g / L PdCl 2 The solution was activated and then 10 g / L NaH 2 PO 2 The solution removes excess Pd ions;
[0086] The NiCo coating was deposited on the surface of ZTA ceramic particles by chemical co-deposition. The Ni:Co ratio in the plating solution was 3:2 and the NaH 2 PO 2 The concentration of the complexing agent C is 25g / L. 6 H 5 O7 Na 3 The concentration is 40g / L, the deposition temperature is 85℃, the deposition time is 10h, and the plating solution is changed every 2h;
[0087] The surface metallized ZTA ceramic particles, 18wt.% Fe powder and 4wt.% silicate water glass were mixed in a stirrer at a stirring speed of 180rpm for 1.5h. The mixture was injected into 8-hole polytetrafluoroethylene and then dried in a vacuum oven at 85℃ for 50min. The vacuum degree was maintained at 1.4×10 -1 Pa;
[0088] The preform was sintered in a vacuum box furnace at 1300 °C for 1.5 h, with the furnace vacuum maintained at 1.5 × 10 -3 Pa; the heating rate of the first 800°C during the heating process is 10°C / min, and the heating rate of the high temperature stage is 5°C / min. The preform is cooled in the furnace to obtain a size of 120×120×30mm, and the size of the hole is Φ20×30mm;
[0089] The preform is fixed at the bottom of the cavity and dried in a heat treatment furnace at 450°C for 9 hours;
[0090] The molten iron is melted by a medium frequency induction melting furnace, with a DC voltage of 480V, a DC current of 95A, an medium frequency voltage of 740V, a medium frequency power of 65KW, and a medium frequency of 3400Hz. Perlite is used for multiple slag removal and purification, and pure aluminum is used to deoxygenate the molten iron;
[0091] The molten iron was poured into the quartz sand mold cavity by bottom casting method, the casting temperature was 1550℃, cooled to room temperature, and boxed to obtain ZTA ceramic particle reinforced iron-based composite wear-resistant lining, whose wear resistance was 5.4 times that of Cr15.
[0092] Example 4
[0093] The ZTA ceramic particles were ultrasonically cleaned in acetone, heated to 80 °C in a water bath, and ultrasonically cleaned for 15 min, then rinsed with deionized water and dried in a vacuum oven;
[0094] Subsequently, the ZTA ceramic particles were activated and sensitized on a magnetic stirrer. The ZTA ceramic particles were hydrated in 15 g / L SnCl 2 The solution was sensitized for 30 min, followed by 0.5 g / L PdCl 2 The solution was activated and then treated with 15 g / L NaH 2 PO 2 The solution removes excess Pd ions;
[0095] The NiCo coating was deposited on the surface of ZTA ceramic particles by chemical co-deposition. The Ni:Co ratio in the plating solution was 4:1 and the NaH 2 PO 2 The concentration of complexing agent C is 30g / L. 6 H 5 O 7 Na 3 The concentration is 50g / L, the deposition temperature is 90℃, the deposition time is 12h, and the plating solution is changed every 2h;
[0096] The surface metallized ZTA ceramic particles, 20wt.% Fe powder and 5wt.% silicate water glass were mixed evenly in a stirrer at a stirring speed of 200rpm for 2h. The mixture was injected into 8-hole polytetrafluoroethylene and then dried in a vacuum oven at 90℃ for 60min. The vacuum degree was maintained at 1.5×10 -1 Pa;
[0097] The preform was sintered in a vacuum box furnace at 1400 °C for 2 h, with the vacuum degree of the furnace maintained at 2 × 10 -3 Pa; the heating rate of the first 800°C during the heating process is 10°C / min, and the heating rate of the high temperature stage is 5°C / min. The preform is cooled in the furnace to obtain a size of 120×120×30mm, and the size of the hole is Φ20×30mm;
[0098] The preform is fixed at the bottom of the cavity and dried in a heat treatment furnace at 500°C for 10 hours;
[0099] The molten iron is melted by a medium frequency induction melting furnace, with a DC voltage of 500V, a DC current of 100A, a medium frequency voltage of 750V, a medium frequency power of 70KW, and a medium frequency of 3500Hz. Perlite is used for multiple slag removal and purification, and pure aluminum is used to deoxygenate the molten iron;
[0100] The molten iron was poured into the quartz sand mold cavity by bottom casting method, the casting temperature was 1600℃, cooled to room temperature, and boxed to obtain ZTA ceramic particle reinforced iron-based composite wear-resistant lining plate, whose wear resistance was 4.6 times that of Cr15.
[0101] In summary, the present invention provides a NiCo modified oxide ceramic particle reinforced iron-based composite material, a casting method and application thereof, and adopts a casting infiltration method to prepare an oxide ceramic particle reinforced iron-based composite material, which provides a theoretical basis and engineering value for the industrial application of high-strength and high-toughness wear-resistant linings; the "core-shell structure" NiCo coating wrapped around ZTA effectively improves the surface activity of the ceramic particles, forms a metallurgical bond between the ZTA ceramic particles and the Fe matrix, improves the bonding strength of the heterogeneous interface, increases the wear resistance of the composite lining, and extends the service life of the composite lining.
[0102] Finally, it should be noted that the above embodiments are only used to illustrate the technical solutions of the present invention, rather than to limit it. Although the present invention has been described in detail with reference to the aforementioned embodiments, those skilled in the art should understand that they can still modify the technical solutions described in the aforementioned embodiments, or replace some or all of the technical features therein with equivalents. However, these modifications or replacements do not cause the essence of the corresponding technical solutions to deviate from the scope of the technical solutions of the embodiments of the present invention.
Claims
1. A method for casting a NiCo modified oxide ceramic particle reinforced iron-based composite material, characterized in that: The following steps are involved: The irregular ZTA ceramic particles were surface activated and sensitized, and then a NiCo coating was deposited on the surface of the ZTA ceramic particles by chemical co-deposition. The metallized ZTA ceramic particles are mixed with iron powder and silicate water glass solution so that the iron powder is coated on the surface of the metallized ZTA ceramic particles, and then the mixture is injected into a mold to form a porous preform; The porous preform is dried, and finally the porous preform is prepared into a composite material by a bottom injection casting method.
2. The method for casting NiCo modified oxide ceramic particles reinforced iron-based composite materials according to claim 1, characterized in that: The oil stains and impurities on the surface of the ZTA ceramic particles were cleaned with acetone, and then ultrasonic cleaning was performed. The water bath was heated to 60-80°C and ultrasonic cleaning was performed for 10-15 minutes. The dried ZTA ceramic particles were then activated and sensitized.
3. The casting method of NiCo modified oxide ceramic particles reinforced iron-based composite material according to claim 1, characterized in that: The activation and sensitization treatments are as follows: The irregular ZTA ceramic particles were activated in SnCl2 solution for 10 to 30 min, then sensitized in PdCl2 solution for 10 to 30 min, and finally the excess Pd ions were removed by NaH2PO2.
4. The casting method of NiCo modified oxide ceramic particles reinforced iron-based composite material according to claim 1, characterized in that: In the process of depositing a NiCo coating on the surface of ZTA ceramic particles by chemical co-deposition, the mass ratio of Ni:Co in the chemical co-deposition plating solution is (1-4):(4-1), trisodium citrate is used as a complexing agent, and boric acid is used to adjust the pH.
5. The casting method of NiCo modified oxide ceramic particles reinforced iron-based composite material according to claim 4, characterized in that: The concentration of NaH2PO2 is 10-30 g / L, the concentration of the complexing agent is 20-50 g / L, the deposition temperature is 60-90°C, the deposition time is 2-12 hours, and the plating solution is changed every 1.5-2 hours.
6. The method for casting NiCo modified oxide ceramic particles reinforced iron-based composite materials according to claim 1, characterized in that: The metallized ZTA ceramic particles are mixed evenly with iron powder and silicate water glass solution as follows: The coated ZTA ceramic particles are stirred and mixed with 10wt.% to 20wt.% of iron powder and 2wt.% to 5wt.% of silicate, and the mixture is dispersed in an eight-hole mold. The mixture is then dried in a vacuum dryer to obtain a porous preform, and then the porous preform is sintered at a high temperature of 1200 to 1400°C.
7. The method for casting a NiCo modified oxide ceramic particle reinforced iron-based composite material according to claim 6, characterized in that: The stirring speed is 150-200 rpm, the time is 1-2 hours, the drying temperature is 70-90 ° C, the drying time is 30-60 minutes, and the vacuum degree is maintained at 0.5-1.5×10 -1 Pa, sintering time is 1 to 2 hours, and vacuum degree is maintained at 0.5 to 2×10 -3 Pa, the heating rate of the first 800 °C during high-temperature sintering is 10 °C / min, and the heating rate of the high-temperature stage is 5 °C / min.
8. The method for casting NiCo modified oxide ceramic particles reinforced iron-based composite materials according to claim 1, characterized in that: The porous preform is dried at 350-500 DEG C for 5-10 hours, and finally the porous preform is prepared into a composite material by bottom casting at 1450-1600 DEG C.
9. A NiCo modified oxide ceramic particle reinforced iron-based composite material prepared according to the method of any one of claims 1 to 8.
10. Application of the NiCo modified oxide ceramic particle reinforced iron-based composite material according to claim 9 to a wear-resistant liner.
Citation Information
Cited By
Casting-infiltration preparation method of TiB2 and ultrahigh-toughness steel composite material
CN120382142A