Ceramic fiber-based concrete and preparation method thereof
Through the combination of ceramic fiber-based concrete and modification treatment, the problems of brittleness and low tensile strength of traditional concrete materials are solved, significantly improving the tensile properties of concrete and the mechanical properties of interface transition zones, and improving its long-term performance.
Patent Information
- Application Number
- CN202410877159.5
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-07-02
- Publication Date
- 2024-11-19
AI Technical Summary
Traditional concrete materials have problems such as high brittleness, low tensile strength and poor crack resistance. The concrete performance needs to be improved to meet construction and other engineering needs.
Using ceramic fiber-based concrete, materials such as regeneration of coarse aggregates, regeneration of fine aggregates, cement, composite zeolite powder, ceramic fibers, basalt fibers, boron fibers, butanolamine and perfluorohexylpropylsesquioxane Combination, surface modification treatment and synergistic effect to improve the mechanical properties of concrete.
It significantly improves the tensile properties of concrete and the mechanical properties of interface transition zones, reduces the water absorption and dry shrinkage of aggregates, enhances the dispersion and viscosity of fibers in concrete, and improves the long-term performance of concrete.
Abstract
Description
Technical Field
[0001] The invention relates to the field of concrete technology, in particular to a ceramic fiber-based concrete and a preparation method thereof. Background Art
[0002] As a traditional building material, concrete is widely used in engineering fields such as construction, roads, bridges, etc. due to its advantages such as high strength, durability and low cost. However, traditional concrete materials have some limitations, such as high brittleness, low tensile strength, poor crack resistance, etc. In order to overcome these shortcomings, researchers and engineers have been seeking ways to improve the performance of concrete.
[0003] As a new type of composite material, ceramic-based fiber has excellent properties such as high strength, high modulus, high temperature resistance, and corrosion resistance. Therefore, it has been widely used in aerospace, military, automotive and other fields. In recent years, the application of ceramic-based fibers in concrete and the preparation of ceramic fiber-based concrete has become one of the research hotspots in the field of building materials. Summary of the invention
[0004] The object of the present invention is to provide a ceramic fiber-based concrete and a preparation method thereof to solve the problems existing in the prior art.
[0005] In order to solve the above technical problems, the present invention provides the following technical solutions: a ceramic fiber-based concrete, wherein the raw materials of the ceramic fiber-based concrete include, by mass, 1000-1200 parts of recycled coarse aggregate, 500-800 parts of recycled fine aggregate, 200-300 parts of cement, 50-150 parts of composite zeolite powder, 100-150 parts of ceramic fiber, 50-100 parts of basalt fiber, 20-50 parts of boron fiber, 10-20 parts of butylpropanolamine, 10-18 parts of perfluorohexylpropylsilsesquioxane, 1-3 parts of water reducer, 200-240 parts of water, and 30-40 parts of a combination of calcium aluminate, strontium aluminate, and potassium aluminum sulfate.
[0006] Furthermore, the particle size range of the recycled coarse aggregate is 10-15 mm, and the particle size range of the recycled fine aggregate is 0.25 mm-4.5 mm.
[0007] Furthermore, the composite zeolite powder is a mixture of zeolite and activated carbon in a mass ratio of 5:1, and the particle size of the zeolite powder ranges from 200 to 250 meshes.
[0008] Furthermore, the ceramic fiber has a length of 4 mm to 10 mm and a diameter of 3 μm to 8 μm.
[0009] Furthermore, the basalt fiber has a length of 2 mm to 12 mm and a diameter of 2 μm to 10 μm.
[0010] Furthermore, the boron fiber has an average diameter of 300-500 nm and an aspect ratio of (12-16):1.
[0011] Furthermore, the butylpropanolamine is liquid butylpropanolamine, and its content is 99%; the water reducer is a polycarboxylic acid high-performance water reducer, and the water reduction rate reaches more than 40%.
[0012] Furthermore, the composition of calcium aluminate, strontium aluminate and potassium aluminum sulfate is all solid, with a mass ratio of 3:1:1; and the cement is ordinary silicate 42.5 cement.
[0013] Furthermore, a method for preparing ceramic fiber-based concrete comprises the following preparation steps:
[0014] (1) preparing materials according to the following components: 1000-1200 parts of recycled coarse aggregate, 500-800 parts of recycled fine aggregate, 200-300 parts of cement, 50-150 parts of composite zeolite powder, 100-150 parts of ceramic fiber, 50-100 parts of basalt fiber, 20-50 parts of boron fiber, 10-20 parts of butylpropanolamine, 10-18 parts of perfluorohexylpropylsilsesquioxane, 1-3 parts of water reducer, 200-240 parts of water, and 30-40 parts of a combination of calcium aluminate, strontium aluminate, and potassium aluminum sulfate per cubic meter;
[0015] (2) mixing perfluorohexylpropylsilsesquioxane with a certain amount of water in a mass ratio of 1:200, immersing the recycled coarse aggregate and the recycled fine aggregate in the silane coupling agent solution until the water is saturated, filtering out, and placing in a ventilated place to dry naturally, thereby obtaining a modified recycled aggregate;
[0016] (3) uniformly mixing the modified recycled aggregate with the weighed cement, composite zeolite powder, butylpropanolamine, calcium aluminate, strontium aluminate and potassium aluminum sulfate for the first time;
[0017] (4) adding the weighed water reducer into water and mixing evenly, the mass ratio is 3.8:170, and the obtained aqueous solution is added into the mixture obtained in step (3) and stirred evenly for a second time;
[0018] (5) Ceramic fiber, basalt fiber and boron fiber are added to the mixture prepared in step (4) and stirred for a third time to obtain ceramic fiber-based concrete.
[0019] Furthermore, the stirring time for the first stirring in step (3) is 60-120 seconds, and the stirring time for the second stirring in step (4) is 120-180 seconds.
[0020] Compared with the prior art, the beneficial effects achieved by the present invention are:
[0021] The present invention uses perfluorohexylpropyl silsesquioxane to soak the recycled aggregate and perform surface modification on the recycled aggregate. A hydrophobic layer is formed on the surface of the soaked aggregate, thereby reducing the water absorption rate of the aggregate, helping to improve the working performance of the recycled concrete, reducing the shrinkage and creep of the recycled concrete, and thus improving the long-term performance of the recycled concrete.
[0022] The present invention adds inorganic ceramic fibers and boron fibers to concrete, and the two can act synergistically. Various hydration products produced by cement hydration can be well attached to the surfaces of various fibers, so that the fibers can better play a role in binding the recycled concrete slurry, thereby improving the defect of poorer mechanical properties in the interface transition zone of the recycled concrete, thereby improving the strength of the recycled concrete, especially the tensile properties of the concrete.
[0023] The invention uses butylpropanolamine to modify ceramic fibers and boron fibers in a solution. The butylpropanolamine significantly enhances the emulsification, wetting, penetration, adsorption, dispersion and other effects of cement particles, is easier to expand and adsorb on the surface and inside of cement particles, increases the hydration degree of cement, thereby improving the dispersion of fibers in concrete and further improving the mechanical properties.
[0024] The present invention uses composite natural zeolite rock and activated carbon to make composite zeolite powder, wherein the natural zeolite rock is ground into a kind of volcanic ash material, which has a huge internal and external specific surface area and contains a large amount of active silicon dioxide and oxide. As a concrete admixture, it can react with Ca(OH)2 released by cement hydration to generate more CSH gel and hydrated aluminate, thereby greatly improving the microstructure of hardened cement paste. At the same time, the introduction of activated carbon strengthens the adsorption effect, thereby increasing the viscosity of concrete, eliminating segregation and bleeding in concrete, and through the filling effect of zeolite powder and volcanic ash reaction, the total void ratio of concrete can be greatly reduced, the interface transition zone between cement paste and recycled aggregate can be improved, and the performance of concrete can be improved. DETAILED DESCRIPTION
[0025] The following will be combined with the embodiments of the present invention to clearly and completely describe the technical solutions in the embodiments of the present invention. Obviously, the described embodiments are only part of the embodiments of the present invention, not all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without making creative work are within the scope of protection of the present invention.
[0026] In order to more clearly illustrate the method provided by the present invention, the following examples are used to describe in detail the various index testing methods of the ceramic fiber-based concrete prepared in the following examples.
[0027] Compressive strength: GB / T 50081-2002
[0028] Concrete slump: GBT50080-2016
[0029] Axial tensile strength: GB / T 50081-2002
[0030] Average water seepage height: GB / T 50082-2009
[0031] Example 1
[0032] (1) Prepare the materials according to the following components: 1000 parts of recycled coarse aggregate, 500 parts of recycled fine aggregate, 300 parts of cement, 80 parts of composite zeolite powder, 100 parts of ceramic fiber, 80 parts of basalt fiber, 50 parts of boron fiber, 10 parts of butylpropanolamine, 10 parts of perfluorohexylpropylsilsesquioxane, 3 parts of water reducer, and 30 parts of a combination of calcium aluminate, strontium aluminate, and potassium aluminum sulfate per cubic meter;
[0033] (2) mixing perfluorohexylpropylsilsesquioxane with a certain amount of water in a mass ratio of 1:200, immersing the recycled coarse aggregate and the recycled fine aggregate in the silane coupling agent solution until the water is saturated, filtering out, and placing in a ventilated place to dry naturally, thereby obtaining a modified recycled aggregate;
[0034] (3) The modified recycled aggregate is mixed with the weighed cement, composite zeolite powder, butyl propanolamine, calcium aluminate, strontium aluminate and potassium aluminum sulfate for the first time and stirred for 120 seconds;
[0035] (4) Add the weighed water reducer into water and mix well, the mass ratio is 3.8:170, and then add the obtained aqueous solution into the mixture obtained in step (3) and stir for a second time, stirring for 180 seconds;
[0036] (5) Ceramic fiber, basalt fiber and boron fiber are added to the mixture prepared in step (4) and stirred for a third time to obtain ceramic fiber-based concrete.
[0037] Example 2
[0038] (1) Prepare the following components: 1200 parts of recycled coarse aggregate, 600 parts of recycled fine aggregate, 320 parts of cement, 80 parts of composite zeolite powder, 100 parts of ceramic fiber, 80 parts of basalt fiber, 50 parts of boron fiber, 10 parts of butylpropanolamine, 10 parts of perfluorohexylpropylsilsesquioxane, 3 parts of water reducer, and 30 parts of a combination of calcium aluminate, strontium aluminate, and potassium aluminum sulfate per cubic meter;
[0039] (2) mixing perfluorohexylpropylsilsesquioxane with a certain amount of water in a mass ratio of 1:200, immersing the recycled coarse aggregate and the recycled fine aggregate in the silane coupling agent solution until the water is saturated, filtering out, and placing in a ventilated place to dry naturally, thereby obtaining a modified recycled aggregate;
[0040] (3) The modified recycled aggregate is mixed with the weighed cement, composite zeolite powder, butyl propanolamine, calcium aluminate, strontium aluminate and potassium aluminum sulfate for the first time, and the mixing time is 100 seconds;
[0041] (4) Add the weighed water reducer into water and mix well, the mass ratio is 3.8:170, and then add the obtained aqueous solution into the mixture obtained in step (3) and stir for a second time, the stirring time is 160s;
[0042] (5) Ceramic fiber, basalt fiber and boron fiber are added to the mixture prepared in step (4) and stirred for a third time to obtain ceramic fiber-based concrete.
[0043] Example 3
[0044] (1) Prepare the materials according to the following components: 900 parts of recycled coarse aggregate, 400 parts of recycled fine aggregate, 250 parts of cement, 150 parts of composite zeolite powder, 120 parts of ceramic fiber, 80 parts of basalt fiber, 35 parts of boron fiber, 15 parts of butylpropanolamine, 14 parts of perfluorohexylpropylsilsesquioxane, 1 part of water reducer, and 30 parts of a combination of calcium aluminate, strontium aluminate, and potassium aluminum sulfate per cubic meter;
[0045] (2) mixing perfluorohexylpropylsilsesquioxane with a certain amount of water in a mass ratio of 1:200, immersing the recycled coarse aggregate and the recycled fine aggregate in the silane coupling agent solution until the water is saturated, filtering out, and placing in a ventilated place to dry naturally, thereby obtaining a modified recycled aggregate;
[0046] (3) The modified recycled aggregate is mixed with the weighed cement, composite zeolite powder, butyl propanolamine, calcium aluminate, strontium aluminate and potassium aluminum sulfate for the first time, and the mixing time is 120 seconds;
[0047] (4) Add the weighed water reducer into water and mix well, the mass ratio is 3.8:170, and the obtained aqueous solution is added into the mixture obtained in step (3) and stirred for a second time, the stirring time is 180s;
[0048] (5) Ceramic fiber, basalt fiber and boron fiber are added to the mixture prepared in step (4) and stirred for a third time to obtain ceramic fiber-based concrete.
[0049] Comparative Example 1
[0050] The difference between Comparative Example 1 and Example 1 is that step (1) is different. Step (1) is changed to prepare materials according to the following components: 1000 parts of recycled coarse aggregate, 500 parts of recycled fine aggregate, 300 parts of cement, 80 parts of composite zeolite powder, 100 parts of ceramic fiber, 80 parts of basalt fiber, 50 parts of boron fiber, 10 parts of butylpropanolamine, 10 parts of perfluorohexylpropylsilsesquioxane, 3 parts of water reducer, and 30 parts of a composition of calcium aluminate, strontium aluminate, and potassium aluminum sulfate per cubic meter;
[0051] Comparative Example 2
[0052] The difference between Comparative Example 3 and Example 1 is that step (1) is different. Step (1) is changed to prepare materials according to the following components: 1000 parts of recycled coarse aggregate, 500 parts of recycled fine aggregate, 300 parts of cement, 80 parts of composite zeolite powder, 100 parts of banana fiber, 80 parts of basalt fiber, 50 parts of boron fiber, 10 parts of butylpropanolamine, 10 parts of perfluorohexylpropylsilsesquioxane, 3 parts of water reducer, and 30 parts of a composition of calcium aluminate, strontium aluminate, and potassium aluminum sulfate per cubic meter;
[0053] Comparative Example 3
[0054] The difference between Comparative Example 3 and Example 1 is that step (1) is different. Step (1) is changed to prepare materials according to the following components: 1000 parts of recycled coarse aggregate, 500 parts of recycled fine aggregate, 300 parts of cement, 80 parts of composite zeolite powder, 100 parts of ceramic fiber, 80 parts of basalt fiber, 50 parts of boron fiber, 10 parts of butylpropanolamine, 10 parts of perfluorohexylpropylsilsesquioxane, 3 parts of water reducer, and 30 parts of a composition of alumina, aluminum sulfate, and potassium aluminum sulfate per cubic meter;
[0055] Effect Example 1
[0056] Table 1 below shows the performance analysis results of the ceramic fiber-based concrete using Examples 1 to 3 of the present invention and Comparative Examples 1 to 3.
[0057] Table 1
[0058] Example 1 Example 2 Example 3 Comparative Example 1 Comparative Example 2 Comparative Example 3 Concrete slump / mm 170 175 175 180 180 175 Compressive strength / MPa 55.9 45.6 52.3 47.8 41.3 48.5 Tensile strength / MPa 4.3 3.9 4.1 4.0 3.6 3.9 Water seepage height / mm 32 40 36 45 50 43
[0059] From the comparison of the experimental data of Examples 1 to 3 and Comparative Examples 1 to 3, it can be found that the present invention uses recycled aggregate to prepare recycled concrete, adds butylpropanolamine solution, composite zeolite powder, ceramic fiber, boron fiber, basalt fiber and other materials, uses perfluorohexylpropyl silsesquioxane to soak the recycled aggregate for modification pretreatment, and adds butylpropanolamine solution when mixing the fibers to improve the impermeability and mechanical properties of the recycled concrete. The present invention uses composite natural zeolite rock and activated carbon as composite zeolite powder, wherein a volcanic ash material formed by grinding natural zeolite rock has a huge internal and external specific surface area and contains a large amount of active silica and oxide. . It is used as a concrete admixture, which can react with Ca(OH)2 released by cement hydration to generate more CSH gel and hydrated aluminate, thereby well improving the microstructure of the hardened cement paste. At the same time, the introduction of activated carbon strengthens the adsorption effect, thereby increasing the viscosity of concrete, eliminating segregation and bleeding in concrete, and through the filling effect of zeolite powder and volcanic ash reaction, it can greatly reduce the total void ratio of concrete, improve the interface transition zone between cement paste and recycled aggregate, and improve the performance of concrete.
[0060] It will be apparent to those skilled in the art that the invention is not limited to the details of the exemplary embodiments described above and that the invention can be implemented in other specific forms without departing from the spirit or essential features of the invention. Therefore, the embodiments should be considered in all respects as exemplary and non-limiting, and the scope of the invention is defined by the appended claims rather than the foregoing description, and it is intended that all variations within the meaning and scope of the equivalent elements of the claims be included in the invention. Any marking in a claim should not be considered as limiting the claim to which it relates.
Claims
1. A ceramic fiber-based concrete, characterized in that: The raw materials of the ceramic fiber-based concrete include, by mass, 1000-1200 parts of recycled coarse aggregate, 500-800 parts of recycled fine aggregate, 200-300 parts of cement, 50-150 parts of composite zeolite powder, 100-150 parts of ceramic fiber, 50-100 parts of basalt fiber, 20-50 parts of boron fiber, 10-20 parts of butylpropanolamine, 10-18 parts of perfluorohexylpropylsilsesquioxane, 1-3 parts of a water reducer, and 30-40 parts of a combination of calcium aluminate, strontium aluminate, and potassium aluminum sulfate.
2. A ceramic fiber-based concrete according to claim 1, characterized in that: The particle size range of the recycled coarse aggregate is 10-15 mm, and the particle size range of the recycled fine aggregate is 0.25 mm-4.5 mm.
3. The ceramic fiber-based concrete according to claim 1, characterized in that: The composite zeolite powder is a mixture of zeolite and activated carbon in a mass ratio of 5:1, and the particle size of the zeolite powder ranges from 200 to 250 meshes.
4. The ceramic fiber-based concrete according to claim 1, characterized in that: The ceramic fibers have a length of 4 mm to 10 mm and a diameter of 3 μm to 8 μm.
5. The ceramic fiber-based concrete according to claim 1, characterized in that: The basalt fiber has a length of 2 mm to 12 mm and a diameter of 2 μm to 10 μm.
6. The ceramic fiber-based concrete according to claim 1, characterized in that: The boron fiber has an average diameter of 300-500 nm and an aspect ratio of (12-16):
1.
7. The ceramic fiber-based concrete according to claim 1, characterized in that: The butylpropanolamine is liquid butylpropanolamine, and its content is 99%; the water reducer is a polycarboxylic acid high-performance water reducer, and the water reduction rate reaches more than 40%.
8. The ceramic fiber-based concrete according to claim 1, characterized in that: The composition of calcium aluminate, strontium aluminate and potassium aluminum sulfate is all solid, with a mass ratio of 3:1:1; the cement is ordinary silicate 42.5 cement.
9. A method for preparing ceramic fiber-based concrete, characterized in that: The method comprises the following preparation steps: (1) Prepare the materials according to the following components: 1000-1200 parts of recycled coarse aggregate, 500-800 parts of recycled fine aggregate, 200-300 parts of cement, 50-150 parts of composite zeolite powder, 100-150 parts of ceramic fiber, 50-100 parts of basalt fiber, 20-50 parts of boron fiber, 10-20 parts of butylpropanolamine, 10-18 parts of perfluorohexylpropylsilsesquioxane, 1-3 parts of water reducer, 200-240 parts of water, and 30-40 parts of a combination of calcium aluminate, strontium aluminate, and potassium aluminum sulfate per cubic meter; (2) mixing perfluorohexylpropylsilsesquioxane with a certain amount of water in a mass ratio of 1:200, immersing the recycled coarse aggregate and the recycled fine aggregate in the silane coupling agent solution until the water is saturated, filtering out, and placing in a ventilated place to dry naturally, thereby obtaining a modified recycled aggregate; (3) uniformly mixing the modified recycled aggregate with the weighed cement, composite zeolite powder, butylpropanolamine, calcium aluminate, strontium aluminate and potassium aluminum sulfate for the first time; (4) adding the weighed water reducer into water and mixing evenly, the mass ratio is 3.8:170, and the obtained aqueous solution is added into the mixture obtained in step (3) and stirred evenly for a second time; (5) Ceramic fiber, basalt fiber and boron fiber are added to the mixture prepared in step (4) and stirred for a third time to obtain ceramic fiber-based concrete.
10. The method for preparing ceramic fiber-based concrete according to claim 9, characterized in that: The stirring time for the first stirring in step (3) is 60-120 seconds, and the stirring time for the second stirring in step (4) is 120-180 seconds.